Process for heating medium-carbon annealing-free cold forging steel and reducing depth of decarburized layer

Through the three-stage heating process and combustion atmosphere control, combined with rapid cooling and surface treatment, the problem of decarbonization layer depth of medium-carbon annealing-free cold heading steel is solved, and the mechanical properties and surface quality of the material are improved.

CN118996077APending Publication Date: 2024-11-22XINJI AOSEN STEEL GRP CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410025088.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-01-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to effectively reduce the depth of the decarbonized layer of medium-carbon annealed cold heading steel, affecting the surface hardness and hardenability of the fastener.

Method used

Adopt three-stage heating process and combustion atmosphere control. The specific steps include pickling, cutting, heating, cold heading processing, cooling, surface treatment and inspection. By controlling the heating temperature range and air gas ratio, combining rapid cooling and surface treatment, it reduces the Decarbonization layer depth.

Benefits of technology

The surface quality of medium-carbon annealed-free cold heading steel is improved and the depth of the decarbonized layer is reduced, the plasticity, toughness and wear resistance of the material are improved, and the service life is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004654138270000011
    Figure HDA0004654138270000011
  • Figure HDA0004654138270000012
    Figure HDA0004654138270000012
  • Figure HDA0004654138270000021
    Figure HDA0004654138270000021
Patent Text Reader

Abstract

The invention relates to the technical field of steel and iron material production, and discloses a process for heating medium-carbon annealing-free cold forging steel and reducing the depth of a decarburized layer, which comprises the following steps: step 1, acid pickling: carrying out acid pickling cleaning on the cold forging steel; 2, cutting, wherein the cold forging steel of the raw material is cut into the required size meeting the specification; 3, three-section type heating is conducted, specifically, the cold forging steel subjected to length calibration is put into a special heating furnace, and the heating temperature and the combustion atmosphere are controlled; the temperature of the first adding section is controlled to be 790-900 DEG C, specifically, a workpiece is put into a heating furnace, and the temperature of the furnace is controlled to reach the first adding section temperature interval of 790-900 DEG C; and the temperature of the second adding section is controlled to be 900-1010 DEG C, and after heating is conducted for a certain time in the first adding section temperature interval, the temperature of the workpiece continues to be increased to be 900-1010 DEG C in the second adding section temperature interval. According to the process for heating the medium-carbon annealing-free cold forging steel and reducing the depth of the decarburized layer, the decarburized layer on the surface of the wire rod for the medium-carbon annealing-free cold forging steel is reduced by adopting reasonable three-section type heating parameters and controlling the combustion atmosphere in the heating furnace.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel material production, in particular to a process for heating medium-carbon annealing-free cold heading steel and reducing the depth of a decarburized layer. Background Art

[0002] Medium-carbon, anneal-free, cold-heading steel wire rod grades include SWRCH35K and SWRCH40K, primarily used to produce 8.8-grade strength fasteners. These products offer high strength, stable composition, low levels of harmful elements, high surface quality, and precise geometric dimensions.

[0003] To ensure the surface hardness and hardenability of fasteners, extremely strict requirements are placed on the decarburization layer of the raw materials. Therefore, it is of great significance to develop a method for reducing the depth of the decarburization layer by controlling the heating process and combustion atmosphere for medium-carbon annealing-free cold heading steel. Summary of the Invention

[0004] The object of the present invention is to provide a process for heating medium carbon annealing-free cold heading steel and reducing the depth of the decarburized layer, so as to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: a process for heating medium carbon annealing-free cold heading steel and reducing the depth of the decarburized layer, the process steps being:

[0006] Step 1, pickling: cold heading steel is pickled and cleaned;

[0007] Step 2: Cutting: The raw material cold heading steel is cut into the required size that meets the specifications;

[0008] Step 3, three-stage heating: Place the length-calibrated cold-headed steel into a dedicated heating furnace, and control the heating temperature and combustion atmosphere;

[0009] Add a temperature range of 790-900℃: Place the workpiece in a heating furnace and control the furnace temperature to reach a temperature range of 790-900℃. In this temperature range, the workpiece begins to be gradually heated, but the temperature is not high enough to cause annealing.

[0010] The second stage temperature is controlled at 900-1010℃: After heating in the first temperature range for a certain period of time, the workpiece is further heated to the second temperature range of 900-1010℃. In this temperature range, the workpiece continues to absorb heat and reaches a higher temperature, allowing its grains to grow and increasing the plasticity and toughness of the material;

[0011] The temperature of the third stage is controlled at 1010-1130℃: After heating in the second stage temperature range for a certain period of time, the workpiece is heated to the third stage temperature range of 1010-1130℃. In this temperature range, the temperature of the workpiece is further increased. When it reaches a certain temperature, the grains grow more, further improving the plasticity and toughness of the material.

[0012] Control the air-gas ratio to be 0.70-0.95. During the entire heating process, control the air-gas ratio in the heating furnace to be 0.70-0.95 to control the oxidizing and reducing properties of the atmosphere in the furnace. A suitable atmosphere can protect the workpiece surface from oxidation and prevent defects such as oxide scale from appearing on the material surface.

[0013] When steel with a carbon content of 0.30% or more is heated in a heating furnace, carbon atoms easily diffuse to the surface, reacting with the decarburizing atmosphere in the furnace to produce carbon dioxide. The carbon on the surface of the billet diffuses into the furnace atmosphere, eventually forming a decarburized layer on the billet surface. After multiple rolling processes, the surface decarburized layer does not disappear after being rolled into wire rods, and is inherited as the surface decarburized layer of the hot-rolled wire rods. It is generally believed that the higher the billet heating temperature and the higher the oxygen content in the heating furnace atmosphere, the deeper the decarburized layer on the wire rod surface. The present invention has conducted multiple actual production tests with different heating temperatures and combustion atmospheres, and finally developed a process control method that can ensure qualified wire rod surface quality while reducing the depth of the decarburized layer.

[0014] Step 4: Cold heading: The heated cold heading steel is processed through a cold heading machine;

[0015] Step 5: Cooling: After the cold heading process is completed, the steel is quickly cooled;

[0016] Step 6: Surface treatment: The steel can be surface treated as needed;

[0017] Step 7, Inspection: Conduct quality inspection on the processed steel;

[0018] Step 8: Packaging and storage: Pack and store qualified steel products.

[0019] Preferably, the detailed operation of step 1 is as follows: prepare a hydrochloric acid solution with a concentration of 15% as a pickling liquid, clean the cold-headed steel parts to be pickled, and ensure that there is no grease, oxide, rust or other contaminants on the surface. If there is grease or lubricant remaining on the surface, it can be cleaned with an appropriate solvent or alkaline detergent. Place the cleaned cold-headed steel parts in a hydrochloric acid pickling tank, ensure that the cold-headed steel parts are completely immersed in the hydrochloric acid solution, and let the cold-headed steel soak in the hydrochloric acid solution. The specific time depends on the degree of contamination of the steel and the required cleaning effect. Remove the cold-headed steel from the hydrochloric acid pickling tank and rinse it thoroughly with clean water to completely remove the hydrochloric acid residue. , use alkaline neutralizer to neutralize the cold heading steel, clean and dry the cold heading steel to prevent moisture from remaining on the surface, pickling can effectively remove grease, rust, oxides and other impurities on the surface of the steel to ensure that the surface of the material is clean, pickling can improve the surface quality of the steel, making it smoother and more uniform, which helps the subsequent processing technology, and also removes the oxide scale on the surface of the steel, which is very important for the heating process of medium carbon annealing-free cold heading steel, because the oxide scale will affect the uniformity and efficiency of heating. The steel is pretreated before heating to ensure that the material has appropriate surface conditions to obtain the required performance and quality in subsequent processes.

[0020] Preferably, the detailed operation of the step 2 is: placing the cold heading steel on the cutting machine, adjusting the tool and clamping device of the cutting machine according to the required standard size to ensure the accuracy of the cutting process, starting the cutting equipment, and making the tool drop quickly to cut the cold heading steel into the required size. During the cutting process, the cold heading steel will be clamped and the tool will shear along the predetermined cutting line. The cutting is achieved by placing the cold heading steel on the cutting equipment and using the tool on the cutting equipment to shear the cold heading steel. The rapid descent and rotation of the tool causes it to contact the cold heading steel, generating a shearing force. This shearing force will cause the cold heading steel to break and be cut into the required size. At the same time, the function of the clamping device is to fix the cold heading steel to ensure the accuracy and stability of the cutting.

[0021] Preferably, the detailed operation of cutting in step 2 is: marking the cold heading steel to determine the required length or size, using the selected cutting tool to cut on the raw material according to the marked size or length, ensuring that the cutting line is accurate to avoid waste of material or difficulties in subsequent processing steps, during the cutting process, pay attention to controlling the temperature of the cutting area to avoid overheating or overcooling affecting the performance and quality of the material, the cutting operation can ensure that the size and length of the raw material meet the specification requirements, thereby meeting the design requirements of the final product, and converting the raw material from a roll or rod form into the required plane or strip form for subsequent processing steps. Through precise cutting, the waste of raw materials can be minimized, and production efficiency and cost-effectiveness can be improved.

[0022] Preferably, the detailed operation of step 4 is as follows: according to the processing requirements, adjust the clamping device, cold heading rod and cold heading die of the cold heading machine, clamp and fix the cold heading steel, select a suitable cold heading steel die, start the cold heading machine, and make the cold heading rod quickly apply cold heading force to the heated cold heading steel to process it into the required shape and size. The cold heading die will plastically deform the cold heading steel through the cold heading rod, press or stretch it into the required shape, and use the cold heading rod and cold heading die to apply cold heading force to the heated cold heading steel to cause it to undergo plastic deformation to be processed into the required shape and size. The cold heading rod presses the cold heading steel through the cold heading force. During the cold heading process, the contact between the cold heading rod and the cold heading steel will generate friction, and the cold heading force will cause the cold heading steel to undergo plastic deformation, gradually forming the processed shape. The heated cold heading steel can be processed into the shape and size according to the specification requirements. During the cold heading process, the action of the cold heading rod and the cold heading die causes the cold heading steel to undergo plastic deformation, which can also improve the surface quality of the cold heading steel and enhance its mechanical properties. The cold heading steel after cold heading has precise size and good surface finish, which can meet the requirements of the product and provide a good processing foundation for subsequent processes.

[0023] Preferably, the detailed operation of step five is: selecting cooling media including water, wind, liquid nitrogen, etc., using spray cooling to control within 1-5 seconds, and controlling the cooling rate by adjusting the flow rate, speed or parameters of the cooling equipment of the cooling medium. The rapid cooling in the heating process of medium-carbon annealing-free cold heading steel is to control and change the organizational structure of the steel so as to obtain good mechanical properties. Rapid cooling can change the organizational structure of the steel by generating a rapid cooling effect with a rapid cooling rate, thereby achieving a hardening effect of the steel. The cooling medium absorbs the heat inside the steel and cools it down rapidly, so that the austenite in the steel organization is transformed into martensite or bainite, thereby improving the hardness and strength of the steel. In addition, the stress in the cooling process will also be adjusted to a certain extent, further increasing the strength and toughness of the steel.

[0024] Preferably, the detailed operation of step six is: using mechanical descaling, pickling descaling or sandblasting descaling to remove scales, rust and other substances on the surface, and using spraying rust inhibitors, galvanizing, hot dipping and other methods to perform rust prevention treatment on the surface of cold heading steel. The surface treatment in the heating process of medium carbon annealing-free cold heading steel is mainly to improve the surface quality and performance of the steel. Cleaning and descaling can remove impurities on the surface, making the steel surface cleaner and smoother. Surface tempering can improve the wear resistance of the steel by increasing the surface hardness and strength. Rust prevention treatment can prevent the steel from being oxidized or rusted again, thereby extending the service life of the steel. The overall quality and appearance of the steel can be improved through surface treatment to meet the use requirements.

[0025] Preferably, the detailed operations of step seven are: using visual inspection, touch and microscope to check whether there are obvious cracks, scars, pitting and other defects on the surface of the steel; using tools such as rulers and calipers to measure the size of the steel, such as diameter and length, and compare them with the design requirements; using chemical analysis instruments to analyze the composition of the steel, including the content of major elements such as carbon, silicon, manganese, phosphorus, sulfur, etc.; after cutting the steel into samples, metallographic structure observation is carried out; using a microscope to observe the crystal structure, grain size, phase content, etc. of the steel to determine whether the steel has defects such as grain boundary segregation and non-uniform structure; using a hardness testing instrument to calculate the hardness value of the steel by applying a certain pressure on the steel surface and measuring the size of the indentation generated; using an impact testing machine to perform an impact test on the steel, measuring the impact energy and absorbed energy, and evaluating the toughness and impact resistance of the steel. , expose the steel to corrosive media such as acid and alkali, observe the corrosion of the steel, and evaluate the corrosion resistance of the steel through inspection. Surface inspection can determine whether there are obvious defects on the surface of the steel to ensure the appearance quality of the steel. Dimensional inspection can ensure that the steel meets the design dimensions and meets the precision requirements of the product. Chemical composition analysis can detect the component content of the steel to ensure that the chemical composition of the steel meets the requirements. Metallographic structure inspection can observe the crystal structure and organization of the steel to judge the quality and performance of the steel. Hardness test can evaluate the hardness of the steel and indicate the strength and wear resistance of the steel. Impact test can evaluate the toughness and impact resistance of the steel to determine the performance of the steel under stress. Corrosion resistance test can evaluate the corrosion resistance of the steel in corrosive media to ensure the service life and safety of the steel in a specific environment.

[0026] Preferably, the detailed operations of step eight are: cleaning the surface of the steel, removing dust and impurities, selecting appropriate packaging materials such as plastic film and cartons according to the size and shape of the steel, and clearly marking the specifications, batch number, weight and other information of the steel on the packaging. The packaging can effectively protect the surface of the steel from external mechanical damage, oxidation and pollution, ensuring that the quality and appearance of the steel are not affected. The selection and sealing of packaging materials can prevent the steel from being invaded by moisture, water and dust, and prevent the steel from corrosion and deformation during storage. The selection and management of the storage environment can keep the steel dry, ventilated and moisture-proof, and extend the service life of the steel. Classified storage and regular inspections can ensure the convenience of management and retrieval of the steel, and avoid expiration and waste of the steel due to long-term non-use. The protective measures during steel storage can be based on the special requirements of the steel, such as the requirements for corrosion resistance, and corresponding measures can be taken to extend the service life of the steel.

[0027] Preferably, after the heating in step 3 is completed, samples of the 10 mm hot-rolled wire rod are taken and decarburization inspection is performed according to the inspection standards.

[0028] Compared with the prior art, the present invention provides a process for heating medium-carbon annealing-free cold heading steel and reducing the depth of the decarburized layer, which has the following beneficial effects:

[0029] 1. The process of heating medium carbon annealing-free cold heading steel and reducing the depth of decarburization layer achieves the goal of reducing the surface decarburization layer of medium carbon annealing-free cold heading steel wire rod by adopting reasonable three-stage heating parameters and controlling the combustion atmosphere in the heating furnace.

[0030] 2. The process of heating the medium carbon annealing-free cold heading steel and reducing the depth of the decarburized layer. The rapid cooling in the heating process of the medium carbon annealing-free cold heading steel is to control and change the organizational structure of the steel to obtain good mechanical properties. The stress in the cooling process will also be adjusted to a certain extent, further increasing the strength and toughness of the steel.

[0031] 3. The process of heating the medium carbon annealing-free cold heading steel and reducing the depth of the decarburized layer, cleaning and descaling can remove surface impurities, making the steel surface cleaner and smoother. Surface tempering can improve the surface hardness and strength, improve the wear resistance of the steel, and anti-rust treatment can prevent the steel from re-oxidation or rusting, thereby extending the service life of the steel. Through surface treatment, the overall quality and appearance of the steel can be improved to meet the use requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a metallographic photograph of wire rod decarburization in Experiment 1 of the present invention;

[0033] Figure 2 This is a metallographic photograph of wire rod decarburization in Experiment 2 of the present invention;

[0034] Figure 3 This is a metallographic photograph of wire rod decarburization in Experiment 3 of the present invention;

[0035] Figure 4 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION

[0036] like Figure 1-4 As shown, the present invention provides a technical solution: a process for heating medium carbon annealing-free cold heading steel and reducing the depth of the decarburized layer, the process steps are:

[0037] Step 1, pickling: cold heading steel is pickled and cleaned;

[0038] Step 2: Cutting: The raw material cold heading steel is cut into the required size that meets the specifications;

[0039] Step 3, three-stage heating: Place the length-calibrated cold-headed steel into a dedicated heating furnace, and control the heating temperature and combustion atmosphere;

[0040] Add a temperature range of 790-900℃: Place the workpiece in a heating furnace and control the furnace temperature to reach a temperature range of 790-900℃. In this temperature range, the workpiece begins to be gradually heated, but the temperature is not high enough to cause annealing.

[0041] The second stage temperature is controlled at 900-1010℃: After heating in the first temperature range for a certain period of time, the workpiece is further heated to the second temperature range of 900-1010℃. In this temperature range, the workpiece continues to absorb heat and reaches a higher temperature, allowing its grains to grow and increasing the plasticity and toughness of the material;

[0042] The temperature of the third stage is controlled at 1010-1130℃: After heating in the second stage temperature range for a certain period of time, the workpiece is heated to the third stage temperature range of 1010-1130℃. In this temperature range, the temperature of the workpiece is further increased. When it reaches a certain temperature, the grains grow more, further improving the plasticity and toughness of the material.

[0043] Control the air-gas ratio to be 0.70-0.95: During the entire heating process, the air-gas ratio in the heating furnace is controlled to be 0.70-0.95 to control the oxidizing and reducing properties of the atmosphere in the furnace. A suitable atmosphere can protect the workpiece surface from oxidation and prevent defects such as oxide scale from appearing on the material surface.

[0044] Experiment 1:

[0045] Process parameter control: first heating section temperature 850-970℃, second heating section temperature 970-1080℃, third heating section temperature 1080-1200℃, air-gas ratio 1.00-1.20, decarburization layer depth 170um, metallographic photos of wire rod decarburization are shown in Figure 1 .

[0046] Experiment 2:

[0047] Process parameter control: first heating section temperature 820-940℃, second heating section temperature 940-1050℃, third heating section temperature 1050-1170℃, air-gas ratio 0.90-1.10, decarburization layer depth 120um, metallographic photos of wire rod decarburization are shown in Figure 2 .

[0048] Experiment 3:

[0049] Process parameter control: first heating section temperature 790-900℃, second heating section temperature 900-1010℃, third heating section temperature 1010-1130℃, air-gas ratio 0.70-0.95, decarburization layer depth 80um, wire rod decarburization metallographic photos see Figure 3 .

[0050] During the heating process in a heating furnace, carbon atoms in steel with a carbon content of 0.30% or more easily diffuse to the surface, where they undergo an oxidation reaction with the decarburizing atmosphere within the furnace, producing carbon dioxide. The carbon on the surface of the steel billet diffuses into the furnace atmosphere, ultimately forming a decarburized layer on the billet surface. This surface decarburization persists after being rolled into wire rod through multiple rolling processes, becoming a inherited decarburized layer on the surface of the hot-rolled wire rod. It is generally believed that the higher the billet heating temperature and the higher the oxygen content in the heating furnace atmosphere, the deeper the decarburization layer on the wire rod surface. The present invention, through multiple actual production tests at different heating temperatures and combustion atmospheres, ultimately developed a process control method that ensures acceptable wire rod surface quality while simultaneously reducing the depth of the decarburized layer.

[0051] Step 4: Cold heading: The heated cold heading steel is processed through a cold heading machine;

[0052] Step 5: Cooling: After the cold heading process is completed, the steel is quickly cooled;

[0053] Step 6: Surface treatment: The steel can be surface treated as needed;

[0054] Step 7, Inspection: Conduct quality inspection on the processed steel;

[0055] Step 8: Packaging and storage: Pack and store qualified steel products.

[0056] The detailed operation of step one is: prepare a hydrochloric acid solution with a concentration of 15% as the pickling liquid, clean the cold heading steel parts that need to be pickled, and ensure that there is no grease, oxide, rust or other contaminants on the surface. If there is grease or lubricant remaining on the surface, you can use an appropriate solvent or alkaline detergent to clean it. Place the clean cold heading steel parts in the hydrochloric acid pickling tank, and ensure that the cold heading steel parts are completely immersed in the hydrochloric acid solution. Let the cold heading steel soak in the hydrochloric acid solution. The specific time depends on the degree of contamination of the steel and the required cleaning effect. Take the cold heading steel out of the hydrochloric acid pickling tank and rinse it with clean water to completely remove the hydrochloric acid residue. Use Alkaline neutralizer is used to neutralize the cold heading steel, clean and dry the cold heading steel to prevent moisture from remaining on the surface. Pickling can effectively remove grease, rust, oxides and other impurities on the surface of the steel to ensure that the surface of the material is clean. Pickling can improve the surface quality of the steel, making it smoother and more uniform, which is helpful for subsequent processing. It also removes the oxide scale on the surface of the steel, which is very important for the heating process of medium carbon annealing-free cold heading steel, because the oxide scale will affect the uniformity and efficiency of heating. The steel is pretreated before heating to ensure that the material has appropriate surface conditions to obtain the required performance and quality in subsequent processes.

[0057] The detailed operation of step two is: place the cold heading steel on the cutting machine, adjust the tool and clamping device of the cutting machine according to the required specification size to ensure the accuracy of the cutting process, start the cutting equipment, make the tool drop quickly, and cut the cold heading steel into the required size. During the cutting process, the cold heading steel will be clamped and the tool will shear along the predetermined cutting line. The cutting is achieved by placing the cold heading steel on the cutting equipment and using the tool on the cutting equipment to shear the cold heading steel. The rapid descent and rotation of the tool causes it to contact the cold heading steel, generating a shearing force. This shearing force will cause the cold heading steel to break and cut it into the required size. At the same time, the function of the clamping device is to fix the cold heading steel to ensure the accuracy and stability of the cutting.

[0058] The detailed cutting operations in step two are: mark the cold heading steel to determine the required length or size, use the selected cutting tool to cut on the raw material according to the marked size or length, ensure that the cutting line is accurate to avoid waste of material or difficulties in subsequent processing steps, during the cutting process, pay attention to controlling the temperature of the cutting area to avoid overheating or overcooling affecting the performance and quality of the material, the cutting operation can ensure that the size and length of the raw material meet the specification requirements, thereby meeting the design requirements of the final product, and converting the raw material from coil or rod form to the required flat or strip form for subsequent processing steps. Through precise cutting, the waste of raw materials can be minimized, and production efficiency and cost-effectiveness can be improved.

[0059] The detailed operation of step four is as follows: according to the processing requirements, adjust the clamping device, cold heading rod and cold heading die of the cold heading machine, clamp and fix the cold heading steel, select the appropriate cold heading steel die, start the cold heading machine, and make the cold heading rod quickly apply cold heading force to the heated cold heading steel to process it into the required shape and size. The cold heading die will plastically deform the cold heading steel through the cold heading rod, press or stretch it into the required shape, and use the cold heading rod and cold heading die to apply cold heading force to the heated cold heading steel to plastically deform it to process it into the required shape and size. The cold heading rod presses or stretches the cold heading steel through the cold heading force. During the cold heading process, the contact between the cold heading rod and the cold heading steel will generate friction, and the cold heading force will cause the cold heading steel to undergo plastic deformation, gradually forming the processed shape. The heated cold heading steel can be processed into the shape and size according to the specification requirements. During the cold heading process, the action of the cold heading rod and the cold heading die causes the cold heading steel to undergo plastic deformation, and at the same time, it can also improve the surface quality of the cold heading steel and enhance its mechanical properties. The cold heading steel after cold heading has precise size and good surface finish, which can meet the requirements of the product and provide a good processing foundation for subsequent processes.

[0060] The detailed operation of step five is: select cooling media including water, wind, liquid nitrogen, etc., use spray cooling to control within 1-5 seconds, and control the cooling speed by adjusting the flow rate, speed or parameters of the cooling equipment of the cooling medium. The rapid cooling in the heating process of medium carbon annealing-free cold heading steel is to control and change the organizational structure of the steel to obtain good mechanical properties. Rapid cooling can change the organizational structure of the steel by generating a rapid cooling effect with a rapid cooling rate, thereby achieving the hardening effect of the steel. The cooling medium absorbs the heat inside the steel and cools it down rapidly, so that the austenite in the steel organization is transformed into martensite or bainite, thereby improving the hardness and strength of the steel. In addition, the stress in the cooling process will also be adjusted to a certain extent, further increasing the strength and toughness of the steel.

[0061] The detailed operation of step six is: use mechanical descaling, pickling descaling or sandblasting descaling to remove scales, rust and other substances on the surface, use spraying rust inhibitor, galvanizing, hot dip plating and other methods to treat the surface of cold heading steel for rust prevention. The surface treatment in the heating process of medium carbon annealing-free cold heading steel is mainly to improve the surface quality and performance of steel. Cleaning and descaling can remove impurities on the surface, making the steel surface cleaner and smoother. Surface tempering can improve the wear resistance of steel by increasing surface hardness and strength. Rust prevention can prevent steel from re-oxidation or rusting, and extend the service life of steel. Surface treatment can improve the overall quality and appearance of steel to meet the use requirements.

[0062] The detailed operation of step seven is as follows: use visual inspection, touch and microscope to check whether there are obvious cracks, scars, pitting and other defects on the surface of the steel; use rulers, calipers and other tools to measure the size of the steel, such as diameter, length, etc., and compare with the design requirements; use chemical analysis instruments to analyze the composition of the steel, including the content of major elements such as carbon, silicon, manganese, phosphorus, sulfur, etc.; after cutting the steel into samples, conduct metallographic organization observation; use a microscope to observe the crystal structure, grain size, phase content, etc. of the steel to determine whether the steel has defects such as grain boundary segregation and non-uniform organization; use a hardness testing instrument to calculate the hardness value of the steel by applying a certain pressure on the steel surface and measuring the size of the indentation produced; use an impact testing machine to perform an impact test on the steel, measure the impact energy and absorbed energy, evaluate the toughness and impact resistance of the steel, and The steel is exposed to corrosive media such as acids and alkalis, and the corrosion of the steel is observed. Through inspection, the corrosion resistance of the steel is evaluated. Surface inspection can determine whether there are obvious defects on the surface of the steel to ensure the appearance quality of the steel. Dimensional inspection can ensure that the steel meets the design dimensions and meets the precision requirements of the product. Chemical composition analysis can detect the component content of the steel to ensure that the chemical composition of the steel meets the requirements. Metallographic structure inspection can observe the crystal structure and organization of the steel to judge the quality and performance of the steel. Hardness test can evaluate the hardness of the steel and indicate the strength and wear resistance of the steel. Impact test can evaluate the toughness and impact resistance of the steel to determine the performance of the steel under stress. Corrosion resistance test can evaluate the corrosion resistance of the steel in corrosive media to ensure the service life and safety of the steel in a specific environment.

[0063] The detailed operations of step eight are: clean the surface of the steel, remove dust and impurities, select appropriate packaging materials according to the size and shape of the steel, such as plastic film and cartons, and clearly mark the specifications, batch number, weight and other information of the steel on the packaging. Packaging can effectively protect the surface of the steel from external mechanical damage, oxidation and pollution, and ensure that the quality and appearance of the steel are not affected. The selection and sealing of packaging materials can prevent the steel from being invaded by moisture, water and dust, and prevent the steel from corrosion and deformation during storage. The selection and management of the storage environment can keep the steel dry, ventilated and moisture-proof, and extend the service life of the steel. Classified storage and regular inspections can ensure the convenience of management and retrieval of steel, and avoid expiration and waste of steel due to long-term non-use. The protective measures during steel storage can be based on the special requirements of steel, such as the requirements for corrosion resistance, and take corresponding measures to extend the service life of steel.

[0064] After the heating in step 3 is completed, samples of 10 mm hot-rolled wire rod are taken and decarburization test is carried out according to the test standards.

[0065] The above generally describes the present invention in detail. However, it is obvious to those skilled in the art that modifications or improvements may be made based on the present invention. Therefore, modifications or improvements that do not depart from the spirit of the present invention are within the scope of protection of the present invention.

Claims

1. A process for heating medium carbon annealing-free cold heading steel and reducing the depth of decarburized layer, characterized in that: The process steps are: Step 1, pickling: cold heading steel is pickled and cleaned; Step 2, cutting: the raw material cold heading steel is cut into the required size that meets the specifications; Step 3, three-stage heating: put the length-calibrated cold heading steel into a dedicated heating furnace, and control the heating temperature and combustion atmosphere; Add a section of temperature control at 790-900℃: put the workpiece into the heating furnace and control the furnace temperature to reach a temperature range of 790-900℃; The second stage temperature is controlled at 900-1010℃: After heating in the first temperature range for a certain period of time, the workpiece is further heated to the second stage temperature range of 900-1010℃; The temperature of the third stage is controlled at 1010-1130℃: after heating in the second stage temperature interval for a certain period of time, the workpiece is heated to the third stage temperature interval of 1010-1130℃; Control the air-gas ratio to 0.70-0.95: During the entire heating process, control the air-gas ratio in the heating furnace to 0.70-0.95; Step 4: cold heading: the heated cold heading steel is processed by a cold heading machine; Step 5, cooling: After the cold heading process is completed, the steel is quickly cooled; Step 6: Surface treatment: The steel can be surface treated as needed; Step 7, Inspection: Conduct quality inspection on the processed steel; Step 8: Packaging and storage: Packaging and storage of qualified steel.

2. The process for heating medium carbon annealing-free cold heading steel and reducing the depth of decarburized layer according to claim 1, characterized in that: The detailed operation of step one is as follows: prepare a hydrochloric acid solution with a concentration of 15% as a pickling liquid, clean the cold heading steel parts that need to be pickled, ensure that there is no grease, oxide, rust or other contaminants on the surface, if there is grease or lubricant remaining on the surface, use an appropriate solvent or alkaline detergent to clean it, put the cleaned cold heading steel parts into a hydrochloric acid pickling tank, ensure that the cold heading steel parts are completely immersed in the hydrochloric acid solution, let the cold heading steel soak in the hydrochloric acid solution, the specific time depends on the degree of contamination of the steel and the required cleaning effect, take the cold heading steel out of the hydrochloric acid pickling tank, and rinse it with clean water to completely remove the hydrochloric acid residue, use an alkaline neutralizer to neutralize the cold heading steel, and clean and dry the cold heading steel.

3. The process for heating and reducing the depth of decarburized layer of medium carbon annealing-free cold heading steel according to claim 1 is characterized in that: The detailed operation of step 2 is as follows: placing the cold heading steel on the cutting machine, adjusting the tool and clamping device of the cutting machine according to the required specification size to ensure the accuracy during the cutting process, starting the cutting equipment, and making the tool descend quickly to cut the cold heading steel into the required size. During the cutting process, the cold heading steel will be clamped and the tool will shear along the predetermined cutting line.

4. The process for heating medium carbon annealing-free cold heading steel and reducing the depth of decarburized layer according to claim 3 is characterized in that: The detailed operation of cutting in step 2 is: mark the cold heading steel to determine the required length or size, use the selected cutting tool to cut on the raw material according to the marked size or length, ensure that the cutting line is accurate to avoid wasting materials or difficulties in subsequent processing steps, and during the cutting process, pay attention to controlling the temperature of the cutting area to avoid overheating or overcooling affecting the performance and quality of the material.

5. The process for heating medium carbon annealing-free cold heading steel and reducing the depth of decarburized layer according to claim 1, characterized in that: The detailed operation of step four is as follows: according to the processing requirements, adjust the clamping device, cold heading rod and cold heading die of the cold heading machine, clamp and fix the cold heading steel, select a suitable cold heading steel die, start the cold heading machine, and make the cold heading rod quickly apply cold heading force to the heated cold heading steel to process it into the required shape and size. The cold heading die will plastically deform the cold heading steel through the cold heading rod to press or stretch it into the required shape.

6. The process for heating medium carbon annealing-free cold heading steel and reducing the depth of decarburized layer according to claim 1, characterized in that: The detailed operation of step five is: select cooling media including water, wind, liquid nitrogen, etc., use spray cooling to control within 1-5 seconds, and control the cooling speed by adjusting the flow rate, speed of the cooling medium or the parameters of the cooling equipment.

7. The process for heating and reducing the depth of decarburized layer of medium carbon annealing-free cold heading steel according to claim 1 is characterized in that: The detailed operation of step six is: remove the scales, rust and other substances on the surface by mechanical descaling, pickling descaling or sandblasting descaling, and perform anti-rust treatment on the surface of the cold heading steel by spraying rust inhibitor, galvanizing, hot dip plating and other methods.

8. The process for heating medium carbon annealing-free cold heading steel and reducing the depth of decarburized layer according to claim 1, characterized in that: The detailed operation of the step seven is as follows: using visual inspection, touch and microscope to check whether there are obvious cracks, scars, pitting and other defects on the surface of the steel; using tools such as rulers and calipers to measure the size of the steel, such as diameter, length, etc., and compare them with the design requirements; using chemical analysis instruments to analyze the composition of the steel, including the content of major elements such as carbon, silicon, manganese, phosphorus, sulfur, etc.; after cutting the steel into samples, metallographic structure observation is carried out; using a microscope to observe the crystal structure, grain size, phase content, etc. of the steel, and determine whether the steel has defects such as grain boundary segregation and non-uniform structure; using a hardness testing instrument, by applying a certain pressure on the steel surface and measuring the size of the indentation generated, the hardness value of the steel is calculated; using an impact testing machine to perform an impact test on the steel, measuring the impact energy and absorbed energy, and evaluating the toughness and impact resistance of the steel; exposing the steel to corrosive media such as acids and alkalis, observing the corrosion of the steel, and evaluating the corrosion resistance of the steel through inspection.

9. The process for heating medium carbon annealing-free cold heading steel and reducing the depth of decarburized layer according to claim 1, characterized in that: The detailed operation of step eight is: clean the surface of the steel, remove dust and impurities, select suitable packaging materials such as plastic film and cartons according to the size and shape of the steel, and clearly mark the specifications, batch number, weight and other information of the steel on the packaging.

10. The process for heating medium carbon annealing-free cold heading steel and reducing the depth of decarburized layer according to claim 1, characterized in that: After the heating in step 3 is completed, samples of the 10 mm hot-rolled wire rod are taken and decarburization inspection is carried out according to the inspection standards.

Citation Information

Cited By

  • Low-carbon steel hot-rolled wire rod and decarburized layer depth measuring method thereof

    CN122038916A