Production method of high-strength low-temperature-resistant welding wire steel
By controlling the chemical composition and temperature treatment of the welding wire steel, the problems of structural unevenness and fracture of the welding wire steel are solved, and the production of welding wire steel with high strength and low wire breaking rate is achieved, meeting the stable and efficient production requirements of downstream users.
Patent Information
- Application Number
- CN202410933213.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing high-strength and low-temperature resistant wire steel production methods, the low bainite structure transition temperature leads to core segregation, and the surface rough crystals and different deformation areas of the cross-section are mixed, resulting in the welding wire being easily broken and cannot meet the stable and efficient production requirements of downstream users.
Using billet continuous casting, heating furnace heating, rolling, softening and annealing and drawing processes, the chemical composition and temperature treatment of welding wire steel are controlled, including step-by-step heating and cooling, ensuring the structural uniformity and stress reduction of the strips, and avoiding the cooling process. Concentrated stress.
The tensile strength and pulling speed of welding wire steel are significantly improved, the wire breaking rate is reduced, the high strength and low temperature performance of welding wire steel are ensured, and the production needs of downstream users are met.
Smart Images

Figure CN118996083A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of welding wire steel production, and in particular to a production method of high-strength and low-temperature resistant welding wire steel. Background Art
[0002] Welding materials refer to the general term for various materials used in the welding process, such as welding rods, welding wires, metal powders, fluxes, gases, etc. Among them, high-strength and low-temperature resistant welding wire steel is mainly used as welding materials for pressure vessel pipelines, oil storage tanks, gas storage tanks and other low-temperature resistant containers. Hot-rolled wire rod is a kind of high-strength and low-temperature resistant welding wire steel. It is a round steel rolled at high temperature. It has the advantages of high density, high strength, compression resistance and tensile resistance, and is widely used in various industries.
[0003] The matrix structure of hot-rolled wire rod is mainly ferrite + bainite. Since this steel is low-temperature resistant steel, low-temperature impact resistance needs to be guaranteed. The existing production methods of high-strength and low-temperature resistant welding wire steel have the following technical problems: 1) Due to the low transformation temperature of the bainite structure, the core of the wire rod segregates and abnormal structure appears, which leads to pen-shaped fractures when the wire rod is drawn; 2) During the rolling process of low-carbon steel, coarse grains on the surface and mixed grains in different deformation areas of the cross section are prone to occur, which makes it easy to break during drawing; 3) The overlapping and non-overlapping positions of the wire rod are uneven. Since the organizational control and annealing process control of the hot-rolled wire rod affect the mechanical fluctuations of the same circle, it is easy for the hot-rolled wire rod to break when it is drawn to a fine wire of specified specifications. The product cannot meet the requirements of downstream users for stable and efficient production of welding wire.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The invention provides a method for producing high-strength and low-temperature resistant welding wire steel, which is used to solve the problem of how to ensure uniform structure of welding wire steel and reduce wire breakage rate of welding wire.
[0006] On the one hand, the present invention provides a method for producing high-strength and low-temperature resistant welding wire steel, comprising a billet continuous casting process, a heating furnace heating process, a high-pressure water descaling process, a rolling process, a softening annealing process and a drawing process performed in sequence;
[0007] In the steel billet continuous casting process, the chemical composition of the welding wire steel is controlled, and the chemical composition of the welding wire steel includes, by weight percentage: C, 0.07-0.10%; Mn, 0.85-1.10%; Si, 0.45-0.70%; Ni, 3.10-3.70%; Mo, 0.05-0.10%; Cr, 0.02-0.04%; the balance is Fe and unavoidable impurities;
[0008] In the softening annealing process, the wire rod is controlled to be heated stepwise to a softening temperature, and the wire rod is controlled to be cooled stepwise from the softening temperature to an annealing temperature.
[0009] In some embodiments, the stepwise heating of the wire rod to the softening temperature specifically includes:
[0010] Control the wire rod to heat up to the first softening temperature and keep it warm for 1.0 to 1.5 hours. 3 Passing nitrogen into the closed environment where the wire rod is located at a flow rate of / h;
[0011] The wire rod is controlled to be heated from the first softening temperature to the second softening temperature and kept warm for 8.0 to 9.0 hours. 3 Nitrogen is introduced into the closed environment at a flow rate of / h,
[0012] Wherein, the first softening temperature is between 600 and 630°C, and the second softening temperature is between 690 and 710°C.
[0013] In some embodiments, the wire rod is controlled to be heated to the first softening temperature at a rate of 2.5-3.5°C / min, and at the same time, the wire rod is heated to the first softening temperature at a rate of 60-70m 3 Nitrogen is introduced into the closed environment at a flow rate of / h.
[0014] In some embodiments, the wire rod is controlled to be heated from the first softening temperature to the second softening temperature at a rate of 1.5 to 2.5°C / min, and at the same time, the wire rod is heated at a rate of 150 to 180 min. 3 Nitrogen is introduced into the closed environment where the wire rod is located at a flow rate of / h.
[0015] In some embodiments, controlling the wire rod to be cooled stepwise from the softening temperature to the annealing temperature comprises:
[0016] The wire rod is controlled to be cooled from the second softening temperature to the first annealing temperature at a rate of 0.7 to 1.0°C / min, and at the same time, the wire rod is cooled at a rate of 30 to 40 min. 3 Passing nitrogen into the closed environment where the wire rod is located at a flow rate of / h;
[0017] The wire rod is controlled to be cooled from the first annealing temperature to below the second annealing temperature at a rate of 0.5 to 2.0°C / min, and at the same time, the wire rod is cooled at a rate of 15 to 25 min. 3 Passing nitrogen into the closed environment at a flow rate of / h;
[0018] Wherein, the first annealing temperature is between 500 and 520°C, and the second annealing temperature is ≤200°C.
[0019] In some embodiments, in the softening annealing process, the wire rod is placed in a bell-type annealing furnace, and the furnace pressure of the bell-type annealing furnace is controlled to be between 75.0 and 79.0 mbar, and the combustion-supporting air volume is controlled to be between 800 and 1300 m 3 / h, and the combustion-supporting air valve opening is between 25% and 35%.
[0020] In some embodiments, during the rolling process, the wire rod is controlled to complete phase change between 450 and 550°C in the hood, and the temperature of the overlapping position of the wire rod is between 440 and 450°C when it comes out of the hood, and the temperature of the non-overlapping position is between 380 and 400°C.
[0021] In some of the embodiments, the heating process in the heating furnace controls the core temperature and the surface temperature of the steel billet to be between 1050 and 1080°C, the core of the steel billet is kept warm for 30 to 50 minutes, and the surface of the steel billet is kept warm for 40 to 70 minutes, so that the core temperature and the surface temperature of the steel billet are controlled between 970 and 990°C after the steel billet is taken out of the furnace and before it enters the rolling mill.
[0022] In some of the embodiments, after the softening annealing procedure, the tensile strength of the wire rod is ≤700MPa, the wire breakage rate of 1.2mm drawn welding wire is ≤1.0 times / ton, the tensile strength deviation of the same turn is ≤30Mpa, and there is no mixed crystal and martensitic structure in the metallographic structure.
[0023] After adopting the above technical scheme, the present invention has the following beneficial effects compared with the prior art.
[0024] 1. In the billet continuous casting process, the chemical composition of the welding wire steel, especially the Ni content, is controlled so that the welding wire steel has good strength, toughness and thermal cracking resistance, thereby making the welding wire steel have good temperature resistance.
[0025] 2. In the softening annealing process, the wire rod is controlled to be heated up step by step to the softening temperature, the internal wire rod stress is reduced and the organizational state is adjusted, the uniformity of the core organization, the entire cross-sectional organization, the overlap point and the non-overlap point organization of the wire rod is improved, and the wire rod is controlled to be cooled down step by step from the softening temperature to the annealing temperature to avoid stress concentration during the cooling process, which is conducive to the shedding of the oxide scale.
[0026] 3. The wire rod is obtained by controlling the chemical composition and softening annealing treatment. Its tensile strength is ≤700Mpa, and the tensile strength deviation of the same circle is ≤30Mpa. The iron oxide scale is in large blocks and easy to peel off. The wire rod can be drawn into fine wires at high speed without annealing treatment in the middle. The wire breakage rate of 1.2mm welding wire is ≤1.0 times / ton, which significantly improves the drawing speed. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1is a comparison diagram of the metallographic structures of Example 1 and Example 2 of the present invention;
[0028] Figure 1 (a) shows the metallographic structure diagram of Example 1; Figure 1 (b) shows the metallographic structure diagram of Example 2.
[0029] Figure 2 is a comparison diagram of the metallographic structures of Example 1 of the present invention and Comparative Example 1;
[0030] Figure 2 (a) shows the metallographic structure diagram of Example 1; Figure 2 (b) shows the metallographic structure diagram of Comparative Example 1.
[0031] Figure 3 is a comparison diagram of the metallographic structures of Example 1 of the present invention and Comparative Example 2;
[0032] Figure 3 (a) shows the metallographic structure diagram of Example 1; Figure 3 (b) shows the metallographic structure diagram of Comparative Example 2.
[0033] Figure 4 is a comparison diagram of the metallographic structures of Example 1 of the present invention and Comparative Example 3;
[0034] Figure 4 (a) shows the metallographic structure diagram of Example 1; Figure 4 (b) shows the metallographic structure diagram of Comparative Example 3.
[0035] Figure 5 is a comparison diagram of the metallographic structures of Example 1 of the present invention and Comparative Example 4;
[0036] Figure 5 (a) shows the metallographic structure diagram of Example 1; Figure 5 (b) shows the metallographic structure diagram of Comparative Example 4.
[0037] Figure 6 1 is a comparison diagram of the appearance of Example 1 and Example 2 of the present invention and Comparative Example 1 and Comparative Example 2;
[0038] Figure 6 (a) and (b) respectively represent the appearance of Example 1; Figure 6 (c) and (d) show the appearance of Comparative Example 1 and Comparative Example 2, respectively.
[0039] Figure 7 It is a schematic diagram of step-by-step heating and cooling in the softening annealing process of the present invention. DETAILED DESCRIPTION
[0040] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] Example 1
[0042] A preferred embodiment of a method for producing high-strength and low-temperature resistant welding wire steel disclosed in the present invention comprises: continuous casting of steel billet → heating in a heating furnace → descaling with high-pressure water → rolling → softening annealing → drawing to control composition, heating, descaling, water tank, rolling deformation, cooling, softening annealing and drawing, specifically:
[0043] 1) Composition control: The welding wire steel billet is obtained by smelting, and the chemical composition of the welding wire steel includes by weight percentage:
[0044] C, 0.08%; Mn, 1.02%; Si, 0.57%; Ni, 3.5%; Mo, 0.06%; Cr, 0.04%; the balance is Fe and unavoidable impurities;
[0045] 2) Heating control: The temperature of the high temperature section of the heating furnace is controlled at 1080°C, and the holding time is 90 minutes to heat the steel billet;
[0046] 3) Water descaling control: high-pressure water descaling is carried out after the furnace is taken out, wherein the descaling pressure is 20MPa, the descaling roller speed is 0.8m / s, and the nozzle impact force is 1.0N / mm 2 , the billet is accurately centered;
[0047] 4) Water tank control: control the temperature of the finishing mill to 900℃, the temperature of the sizing machine to 880℃, and the spinning temperature to 840℃. The first and second water tanks before finishing, the first, second, and third water tanks between finishing and sizing, and the first and second water tanks before sizing and spinning are opened. The first five nozzles of all water tanks are opened, the cooling water temperature is 30℃, the nozzle pressure is 0.6MPa, all the back-blowing nozzles are opened, and the gas pressure of the back-blowing nozzles is 0.6Mpa.
[0048] 5) Rolling deformation control: the height of the incoming material of the finishing mill is controlled to be 17.3mm, the height of the material shape of the outlet of the finishing mill is controlled to be 7.01mm, the R factors of the 8 passes of the finishing mill are controlled to be 1.24, 1.23, 1.25, 1.23, 1.29, 1.23, 1.29, 1.22 respectively, the torque parameter of the pinch roll is set to 30%, and the pinch roll adopts an elliptical hole type;
[0049] 6) Cooling control: set the advance amount of the laying machine to 8%, the initial roller speed to 0.12m / s, the subsequent roller speed to increase by 0.02m / s, open the first two insulation covers, open the last insulation cover, the wire rod inlet temperature is 720℃, the wire rod outlet temperature at the overlap position is 440℃, the non-overlap position temperature is 380℃, and a 5.5mm diameter welding wire steel wire rod is obtained;
[0050] 7) Softening annealing control: Feed the 5.5mm diameter welding wire steel wire rod into the annealing furnace, where the annealing furnace pressure is set to 78.0mbar and the combustion air volume is 1000m 3 / h, the combustion-supporting air valve opening is 30%, and the annealing temperature and nitrogen flow rate are controlled according to the annealing temperature and nitrogen flow rate shown in Table 1.
[0051] Table 1
[0052]
[0053] Example 2
[0054] The difference between this embodiment and embodiment 1 is that:
[0055] 2) Heating control: The temperature of the high temperature section of the heating furnace is controlled at 1070°C, and the holding time is 90 minutes to heat the steel billet;
[0056] 4) Water tank control: control the temperature of entering the finishing mill at 870℃, entering the sizing machine at 870℃, and the spinning machine at 840℃. Among them, open the 1st and 2nd water tanks before finishing, the 1st, 2nd, and 3rd water tanks between finishing and sizing, and the 1st and 2nd water tanks before sizing and spinning. All water tanks open the first 5 nozzles, the cooling water temperature is 30℃, the nozzle pressure is 0.6MPa, all the back-blowing nozzles are open, and the back-blowing nozzle gas pressure is 0.6Mpa;
[0057] 5) Rolling deformation control: the height of the incoming material of the finishing mill is controlled to be 17.2mm, the height of the material shape of the outlet of the finishing mill is controlled to be 7.01mm, the R factors of the 8 passes of the finishing mill are controlled to be 1.24, 1.23, 1.25, 1.23, 1.29, 1.23, 1.29, 1.22 respectively, the torque parameter of the pinch roll is set to 30%, and the pinch roll adopts an elliptical hole type;
[0058] 6) Cooling control: set the advance amount of the laying machine to 8%, the initial roller speed to 0.12m / s, the subsequent roller speed increases by 0.02m / s, open the first three insulation covers, open the last insulation cover, the wire rod inlet temperature is 670°C, the wire rod outlet temperature at the overlap position is 440°C, the non-overlap position temperature is 380°C, and a 5.5mm diameter welding wire steel wire rod is obtained;
[0059] 7) Softening annealing control: Feed the 5.5mm diameter welding wire steel wire rod into the annealing furnace, where the annealing furnace pressure is set to 78.0mbar and the combustion air volume is 1020m 3 / h, the combustion-supporting air valve opening is 30%, and the annealing temperature and nitrogen flow rate are controlled according to the annealing temperature and nitrogen flow rate shown in Table 1.
[0060] Example 3
[0061] The difference between this embodiment and embodiment 1 is that:
[0062] 1) Composition control: The welding wire steel billet is obtained by smelting, and the chemical composition of the welding wire steel includes by weight percentage:
[0063] C, 0.09%; Mn, 0.96%; Si, 0.62%; Ni, 3.52%; Mo, 0.07%; Cr, 0.03%; the balance is Fe and unavoidable impurities;
[0064] 2) Heating control: The temperature of the high temperature section of the heating furnace is controlled at 1070°C, and the holding time is 96 minutes to heat the steel billet;
[0065] 4) Water tank control: control the temperature of entering the finishing mill at 880℃, entering the sizing machine at 880℃, and the spinning machine at 840℃. Among them, open the 1st and 2nd water tanks before finishing, the 1st, 2nd and 3rd water tanks between finishing and sizing, and the 1st and 2nd water tanks before sizing and spinning. All water tanks open the first 5 nozzles, the cooling water temperature is 30℃, the nozzle pressure is 0.6MPa, all the back-blowing nozzles are open, and the back-blowing nozzle gas pressure is 0.6Mpa;
[0066] 6) Cooling control: set the advance amount of the laying machine to 10%, the initial roller speed to 0.12m / s, the subsequent roller speed increases by 0.02m / s, open the first two insulation covers, open the last insulation cover, the wire rod inlet temperature is 714°C, the wire rod outlet temperature at the overlap position is 450°C, the non-overlap position temperature is 390°C, and a 5.5mm diameter welding wire steel wire rod is obtained;
[0067] Example 4
[0068] The difference between this embodiment and embodiment 1 is that:
[0069] 1) Composition control: The welding wire steel billet is obtained by smelting, and the chemical composition of the welding wire steel includes by weight percentage:
[0070] C, 0.09%; Mn, 0.96%; Si, 0.62%; Ni, 3.52%; Mo, 0.07%; Cr, 0.03%; the balance is Fe and unavoidable impurities;
[0071] 2) Heating control: The temperature of the high temperature section of the heating furnace is controlled at 1070°C, and the holding time is 96 minutes to heat the steel billet;
[0072] 4) Water tank control: control the temperature of entering the finishing mill at 880℃, entering the sizing machine at 880℃, and the spinning machine at 840℃. Among them, open the 1st and 2nd water tanks before finishing, the 1st, 2nd and 3rd water tanks between finishing and sizing, and the 1st and 2nd water tanks before sizing and spinning. All water tanks open the first 5 nozzles, the cooling water temperature is 30℃, the nozzle pressure is 0.6MPa, all the back-blowing nozzles are open, and the back-blowing nozzle gas pressure is 0.6Mpa;
[0073] 6) Cooling control: set the advance amount of the laying machine to 10%, the initial roller speed to 0.12m / s, the subsequent roller speed increases by 0.02m / s, open the first two insulation covers, open the last insulation cover, the wire rod inlet temperature is 714°C, the wire rod outlet temperature at the overlap position is 450°C, the non-overlap position temperature is 390°C, and a 5.5mm diameter welding wire steel wire rod is obtained;
[0074] 7) Softening annealing control: Feed the 5.5mm diameter welding wire steel wire rod into the annealing furnace, where the annealing furnace pressure is set to 78.0mbar and the combustion air volume is 1000m 3 / h, the combustion air valve opening is 30%, and the annealing temperature and nitrogen flow rate are controlled according to the annealing temperature and nitrogen flow rate shown in Table 2.
[0075] Table 2
[0076]
[0077] Comparative Example 1
[0078] The difference between this comparative example and Example 1 is:
[0079] 4) Water tank control: control the temperature of entering the finishing mill at 930℃, entering the sizing machine at 930℃, and the spinning machine at 900℃. Among them, open the first water tank before finishing, the first water tank between finishing and sizing, and the first water tank before sizing and spinning. All water tanks open the first three nozzles, the cooling water temperature is 30℃, the nozzle pressure is 0.6MPa, all the back-blowing nozzles are open, and the back-blowing nozzle gas pressure is 0.6Mpa;
[0080] 6) Cooling control: set the advance amount of the laying machine to 8%, the initial roller speed to 0.12m / s, the subsequent roller speed increases by 0.02m / s, close all insulation covers, the temperature of the wire rod entering the cover is 860℃, the temperature of the overlapping position of the wire rod when it leaves the cover is 680℃, and the temperature of the non-overlapping position is 560℃;
[0081] Comparative Example 2
[0082] The difference between this comparative example and Example 1 is:
[0083] 7) Softening annealing control: Feed the 5.5mm diameter welding wire steel wire rod into the annealing furnace, where the annealing furnace pressure is set to 78.0mbar and the combustion air volume is 1000m 3 / h, the combustion air valve opening is 30%, and the annealing temperature and nitrogen flow rate are controlled according to the annealing temperature and nitrogen flow rate shown in Table 3:
[0084] Table 3
[0085]
[0086] Comparative Example 3
[0087] The difference between this comparative example and Example 1 is:
[0088] 7) Softening annealing control: Feed the 5.5mm diameter welding wire steel wire rod into the annealing furnace, where the annealing furnace pressure is set to 78.0mbar and the combustion air volume is 1000m 3 / h, the combustion air valve opening is 30%, and the annealing temperature and nitrogen flow rate are controlled according to the annealing temperature and nitrogen flow rate shown in Table 4:
[0089] Table 4
[0090]
[0091] Comparative Example 4
[0092] The difference between this comparative example and Example 1 is:
[0093] No step 7) softening annealing control.
[0094] Performance Testing
[0095] A full circle of wire rods prepared in Examples 1 to 4 and Comparative Examples 1 to 4 was cut into 12 specimens and the following mechanical property tests were performed:
[0096] Maximum tensile strength, minimum tensile strength and extreme difference of tensile strength in the same circle: tested in accordance with GB228;
[0097] Metallographic structure: Tested in accordance with GB / T 6394;
[0098] The test results of the extreme difference in tensile strength of the same circle, maximum tensile strength, minimum tensile strength, wire breakage rate of 1.2 mm welding wire, metallographic structure and iron oxide scale state of the wire rods prepared in Examples 1 to 4 and Comparative Examples 1 to 4 are filled in Table 5.
[0099] Table 5
[0100]
[0101] From Table 5 and Appendix Figures 1 to 5It can be seen that in Comparative Example 1, the temperature of the wire rod is improperly controlled during the water tank control and cooling control, especially the temperature of the wire rod entering the hood is 860°C, the temperature of the overlapping position when the wire rod exits the hood is 680°C, and the temperature of the non-overlapping position is 560°C. The phase change temperature of the wire rod is improperly controlled, resulting in abnormal structure in the core of the wire rod, i.e., martensite exists in the core of the welding wire steel, and the extreme difference in tensile strength in the same turn is high. However, Example 1 controls the phase change temperature of the wire rod in the hood to complete the phase change between 450 and 550°C, reduces segregation, and thus avoids abnormal structure of the wire rod during the phase change process, ensures that the core structure of the wire rod, the entire cross-section of the wire rod, and the overlapping and non-overlapping positions of the wire rod are uniform, and reduces the deviation in tensile strength in the same turn.
[0102] From Table 5, Appendix Figures 1 to 4 and Figure 7 It can be seen that the first softening temperature and the second softening temperature of Comparative Example 2 are relatively low, and the holding time is relatively short; Comparative Example 3 only involves the second softening temperature, and does not involve the step-wise heating and step-wise cooling of the wire rod, resulting in the wire rod heating and cooling speed being too fast; Comparative Example 4 does not involve softening annealing, and cannot eliminate the stress of the inner wire rod and the inhomogeneity of the composition and organization. Due to improper temperature control, Comparative Examples 2 to Comparative Examples 4 are prone to the phenomenon of coarse crystals on the surface of the wire rod and mixed crystals in different deformation areas of the entire cross section of the wire rod, resulting in a high extreme difference in tensile strength of the same circle, while Example 1 controls the softening and heating process of the wire rod in the bell-type annealing furnace, the first softening temperature reaches 620°C, the second softening temperature reaches 700°C and is kept warm for 8h, reducing segregation, thereby avoiding abnormal organization of the wire rod during the phase change process, reducing the internal stress of the wire rod and adjusting the organizational state, preventing the coarse crystals on the surface of the wire rod and the mixed crystals of the entire cross section of the wire rod, so that the maximum tensile strength and minimum tensile strength of the wire rod meet the process requirements of downstream customers.
[0103] From Table 5, Appendix Figure 6 and Figure 7 It can be seen that in Comparative Example 2, the temperature control of the wire rod during softening annealing is improper, the first softening temperature and the second softening temperature are low, and the time for cooling from the second softening temperature to the first annealing temperature is long, which affects the oxidation decarburization effect, and the iron oxide scale on the surface of the wire rod is not easy to peel off; Comparative Example 4 does not involve softening annealing, that is, it does not involve uniform cooling from the second softening temperature to the first annealing temperature, and the state of the iron oxide scale cannot be improved, and the iron oxide scale on the surface of the wire rod is not easy to peel off.
[0104] From Table 5, Appendix Figures 1 to 5 and Figure 7It can be seen that in Example 1, the temperature control of the wire rod is improper during the water tank control and cooling control, resulting in abnormal structure in the core of the wire rod, resulting in pen-shaped fracture during drawing, while in Examples 2 and 3, the temperature control of the wire rod is improper during the softening annealing control, and Example 4 does not involve softening annealing, and there are coarse crystals on the surface of the wire rod and mixed crystals in different deformation areas of the entire cross-section of the wire rod, which makes it easy to break during drawing, resulting in a high wire breakage rate for the 1.2mm welding wire drawn in Examples 1 to 4, while in the process of softening annealing in Examples 1 to 4, the first softening temperature is controlled to reach 620-630℃ and the second softening temperature is controlled to reach 700-710℃, so that the stress in the wire rod is reduced and the structure is uniform, the wire can be drawn at high speed to the finished filament without the need for annealing treatment in the middle, and the wire breakage rate of drawing 1.2mm welding wire is ≤1.0 times / ton.
[0105] In the description of the present invention, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0106] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0107] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for producing high-strength and low-temperature resistant welding wire steel, characterized in that: It includes a continuous casting process of steel billet, a heating process of heating in a heating furnace, a high-pressure water descaling process, a rolling process, a softening annealing process and a drawing process which are carried out in sequence; In the steel billet continuous casting process, the chemical composition of the welding wire steel is controlled, and the chemical composition of the welding wire steel includes, by weight percentage: C, 0.07-0.10%; Mn, 0.85-1.10%; Si, 0.45-0.70%; Ni, 3.10-3.70%; Mo, 0.05-0.10%; Cr, 0.02-0.04%; the balance is Fe and unavoidable impurities; In the softening annealing process, the wire rod is controlled to be heated stepwise to a softening temperature, and the wire rod is controlled to be cooled stepwise from the softening temperature to an annealing temperature.
2. The method for producing high-strength and low-temperature resistant welding wire steel according to claim 1, characterized in that: The stepwise heating of the wire rod to the softening temperature specifically includes: Control the wire rod to heat up to the first softening temperature and keep it warm for 1.0 to 1.5 hours. 3 Passing nitrogen into the closed environment where the wire rod is located at a flow rate of / h; The wire rod is controlled to be heated from the first softening temperature to the second softening temperature and kept warm for 8.0 to 9.0 hours. 3 Nitrogen is introduced into the closed environment at a flow rate of / h, Wherein, the first softening temperature is between 600 and 630°C, and the second softening temperature is between 690 and 710°C.
3. The method for producing high-strength and low-temperature resistant welding wire steel according to claim 2, characterized in that: The wire rod is controlled to be heated to the first softening temperature at a rate of 2.5 to 3.5°C / min, and at the same time, the wire rod is heated to the first softening temperature at a rate of 60 to 70 min. 3 Nitrogen is introduced into the closed environment at a flow rate of / h.
4. The method for producing high-strength and low-temperature resistant welding wire steel according to claim 3, characterized in that: The wire rod is controlled to be heated from the first softening temperature to the second softening temperature at a rate of 1.5 to 2.5°C / min, and at the same time, the wire rod is heated at a rate of 150 to 180 min. 3 Nitrogen is introduced into the closed environment at a flow rate of / h.
5. The method for producing high-strength and low-temperature resistant welding wire steel according to claim 2, characterized in that: The step of controlling the wire rod to cool down from the softening temperature to the annealing temperature in a stepwise manner comprises: The wire rod is controlled to be cooled from the second softening temperature to the first annealing temperature at a rate of 0.7 to 1.0°C / min, and at the same time, the wire rod is cooled at a rate of 30 to 40 min. 3 Passing nitrogen into the closed environment where the wire rod is located at a flow rate of / h; The wire rod is controlled to be cooled from the first annealing temperature to below the second annealing temperature at a rate of 0.5 to 2.0°C / min, and at the same time, the wire rod is cooled at a rate of 15 to 25 min. 3 Passing nitrogen into the closed environment at a flow rate of / h; Wherein, the first annealing temperature is between 500 and 520°C, and the second annealing temperature is ≤200°C.
6. The method for producing high-strength and low-temperature resistant welding wire steel according to claim 1, characterized in that: In the softening annealing process, the wire rod is placed in a bell-type annealing furnace, and the furnace pressure of the bell-type annealing furnace is controlled to be between 75.0 and 79.0 mbar, and the combustion air volume is controlled to be between 800 and 1300 m 3 / h, and the combustion-supporting air valve opening is between 25% and 35%.
7. The method for producing high-strength and low-temperature resistant welding wire steel according to claim 1, characterized in that: During the rolling process, the wire rod is controlled to complete phase change between 450 and 550° C. in the hood, and the temperature of the overlapping position of the wire rod is between 440 and 450° C. when it leaves the hood, and the temperature of the non-overlapping position is between 380 and 400° C.
8. The method for producing high-strength and low-temperature resistant welding wire steel according to claim 1, characterized in that: The heating process in the heating furnace controls the core temperature and the surface temperature of the steel billet to be between 1050 and 1080°C, the core of the steel billet is kept warm for 30 to 50 minutes, and the surface of the steel billet is kept warm for 40 to 70 minutes, so that the core temperature and the surface temperature of the steel billet are controlled between 970 and 990°C after the steel billet is taken out of the furnace and before it enters the rolling mill.
9. The method for producing high-strength and low-temperature resistant welding wire steel according to any one of claims 1 to 8, characterized in that: After the softening annealing procedure, the tensile strength of the wire rod is ≤700MPa, the wire breakage rate of 1.2mm drawn welding wire is ≤1.0 times / ton, the tensile strength deviation of the same circle is ≤30Mpa, and there is no mixed crystal and martensite structure in the metallographic structure.