Method for extracting chromium from chromium-containing material through oxidizing roasting

By using Cr, Fe, Si, C and other additives during chromite oxidation and roasting, the problems of low chromite oxidation conversion rate and waste of resources are solved, efficient extraction of chromite and low-temperature energy-saving roasting are achieved, and production stability is improved. and resource recycling efficiency.

CN118996166AActive Publication Date: 2024-11-22HUBEI ZHENHUA CHEMICAL CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411118939.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The oxidation conversion rate of chromium during the oxidation and roasting of traditional chromite is insufficient, and there are influences of high temperature and low melting point eutectics and impurities, resulting in unstable production and waste of resources. The existing methods have failed to effectively utilize ferrochromium alloy leaching slag.

Method used

Specific additives (Cr, Fe, Si, C) are mixed with chromite and alkali for oxidation and roasting to produce ferrate and aluminosilicate, which reduces the calcination temperature, increases the oxidation rate of chromium and reduces the production of aluminum mud.

Benefits of technology

It realizes efficient extraction and resource utilization of chromium, improves the oxidation rate, reduces the roasting temperature and time, reduces the amount of aluminum mud generated in low-temperature energy-saving roasting treatment of chromite, and improves production stability and resource recovery efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004994453070000131
    Figure BDA0004994453070000131
  • Figure BDA0004994453070000141
    Figure BDA0004994453070000141
Patent Text Reader

Abstract

The invention provides a method for extracting chromium from a chromium-containing material through oxidizing roasting, which comprises the following steps: grinding and mixing the chromium-containing material, alkali and an additive, and then carrying out oxidizing roasting to obtain roasted clinker; the additive comprises the following elements: Cr, Fe, Si and C; and the roasted clinker is leached, and leaching liquid and leaching residues are obtained. According to the method, the specific additive is mixed with the chromium-containing material and the alkali, the oxidizing roasting process of the chromium-containing material is effectively enhanced, efficient extraction of chromium in the chromium-containing material and resource utilization of chromium in the additive are achieved, meanwhile, the oxidizing roasting temperature is reduced, and low-temperature energy-saving roasting treatment of chromite is achieved; and then the roasted clinker is subjected to leaching and solid-liquid separation, and the chromium content in leaching residues is obviously reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inorganic salt production and relates to a method for extracting chromium by oxidative roasting of chromium-containing materials. Background Art

[0002] At present, the main method for industrial production of chromium salts is the calcium-free roasting method. Its main technical route is: under oxidative roasting conditions, chromite is decomposed and oxidized by alkali such as sodium carbonate, so that the insoluble trivalent chromium compounds in the chromite are oxidized and converted into water-soluble sodium chromate, and the chromium in the ore is separated by water leaching. The obtained sodium chromate solution is acidified, evaporated and crystallized to produce sodium dichromate products; among them, sodium dichromate is used to produce chromic anhydride through the sulfuric acid method, or to prepare chromium salt products such as chrome green through reduction.

[0003] However, in the traditional chromite oxidation roasting process, the roasting temperature is as high as 1100-1200℃, and sodium chromate has a low melting point and is easy to form a low-melting eutectic with by-products such as sodium ferrite and sodium aluminate in the charge. There are problems such as reduced oxidation reaction rate and oxidation conversion rate of chromium, and kiln ringing, which greatly affect production. In order to eliminate the adverse effects of liquid phase on the production process, it is necessary to add 2-3 times the amount of ore in the roasting charge. Return slag or limestone / dolomite as filler to reduce the proportion of liquid phase in the charge. Despite this, the oxidation conversion rate of chromium in chromite is still less than 85%. At the same time, the grade of chromium in the return slag is relatively low. The addition of a large amount of return slag is equivalent to reducing the overall grade of the ore, reducing the effective contact area between alkali and chromium, thereby reducing the oxidation rate of chromium and making its leaching rate low.

[0004] CN116590545A discloses a method for strengthening the process of extracting chromium from chromite by roasting without calcium, which method comprises the following steps: adding sulfuric acid solution to chromium slag for leaching reaction to obtain acid leaching slag; using the acid leaching slag as a modified filler, mixing it with chromite and sodium carbonate to obtain a mixed material; roasting the mixed material under air atmosphere to obtain roasted clinker; directly quenching the roasted clinker with water or cooling it with water, separating the solid and liquid, and obtaining a sodium chromate solution and a chromium filter residue. Although this method solves the problem of large chromium slag discharge and large chromium residue in the existing chromium salt production of chromium ore. However, there are still impurities such as aluminum and magnesium leached in the chromium slag during the acid leaching process, and the continuous circulation during the roasting process affects the recovery rate of chromium and reduces the stability of production.

[0005] At present, liquid flow batteries are considered to be one of the preferred technologies for large-scale energy storage due to their high safety, long cycle life, recyclable electrolyte, and environmental friendliness. Iron-chromium liquid flow batteries are the earliest proposed and applicable liquid flow batteries. They have significant advantages such as independent system energy and power, low material cost, easy expansion, high safety, fast response speed, long cycle life, and high energy efficiency. They are a promising large-scale energy storage technology that has developed rapidly in recent years.

[0006] CN116826127A discloses a method for preparing an electrolyte for an iron-chromium flow battery, the method comprising the following steps: mixing a ferrochrome raw material with hydrochloric acid to obtain a leachate; concentrating and cooling the obtained leachate to obtain mixed crystals and a mother liquor; dissolving the obtained mixed crystals and mixing them with hydrochloric acid and chloride salts to obtain an electrolyte for an iron-chromium flow battery. However, the method does not disclose a comprehensive utilization scheme and method for the ferrochrome alloy leaching residue.

[0007] Therefore, a method for extracting chromium by calcium-free roasting of chromite using ferrochrome leaching slag as an additive is provided, so that the chromium in the ferrochrome leaching slag can be fully extracted, the conversion rate of chromium in the chromite roasting process can be improved, the amount of aluminum mud generated can be reduced, and low-temperature energy-saving roasting treatment of chromite can be achieved, which is of great value for promoting the development of the chromium salt production industry and the iron-chromium liquid flow battery industry. Summary of the invention

[0008] The object of the present invention is to provide a method for extracting chromium by oxidative roasting of chromium-containing materials, which adopts a specific additive to mix with the chromium-containing material and alkali to effectively strengthen the oxidative roasting process of the chromium-containing material, realize the efficient extraction of chromium in the chromium-containing material and the resource utilization of chromium in the additive, and at the same time reduce the temperature of oxidative roasting to realize low-temperature energy-saving roasting treatment of chromite.

[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0010] The present invention provides a method for extracting chromium by oxidative roasting of chromium-containing materials, the method comprising the following steps:

[0011] (1) grinding and mixing the chromium-containing material, alkali and additives, and then oxidizing and roasting to obtain roasted clinker;

[0012] The additives include the following elements: Cr, Fe, Si, C;

[0013] (2) Leaching the roasted clinker in step (1) to obtain a leachate and leach residue.

[0014] The method for extracting chromium by oxidative roasting of chromium-containing materials provided by the present invention uses a specific additive to mix with the chromium-containing material and an alkali for extracting the chromium element from the chromium-containing material, effectively strengthens the oxidative roasting process of the chromium-containing material, realizes efficient extraction of chromium from the chromium-containing material and resource utilization of chromium in the additive, significantly accelerates the oxidation reaction of chromium in the material, significantly improves the oxidation rate, reduces the temperature of oxidative roasting, shortens the time of oxidative roasting, and realizes low-temperature energy-saving roasting treatment of chromite; and subsequently, after leaching the roasted clinker, the chromium content in the leached residue is significantly reduced.

[0015] It is worth noting that the additives used in the present invention have the following effects: first, when the additives are added during the oxidative roasting process, the iron element therein generates ferrate to enhance the roasting and extraction of chromium, which helps to increase the oxidation rate of chromium; second, during the oxidative roasting process, silicon combines with aluminum in the chromium-containing material to generate aluminosilicates that are fixed in the slag phase, thereby reducing the generation of aluminum mud in the subsequent neutralization process; third, during the roasting process, carbon increases the calorific value, reduces the roasting temperature and time, and has the advantages of energy saving and emission reduction.

[0016] As a preferred technical solution of the present invention, the chromium-containing material in step (1) includes chromite and / or chromium slag.

[0017] In the present invention, the chromite ore and chromium slag both contain a certain content of Cr2O3.

[0018] As a preferred technical solution of the present invention, the alkali in step (1) comprises any one of sodium carbonate, potassium carbonate, sodium hydroxide or potassium hydroxide, or a combination of at least two of them, wherein the combination is typically but not limited to: a combination of sodium carbonate and potassium carbonate, a combination of potassium carbonate and sodium hydroxide, or a combination of sodium hydroxide and potassium hydroxide, etc.

[0019] Preferably, the mass ratio of the alkali to the chromium-containing material in step (1) is (0.5-2):1, for example, it can be 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1 or 1.9:1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0020] As a preferred technical solution of the present invention, the additive in step (1) includes the following elements in terms of mass content: Cr: 30wt.%~60wt.%, Fe: 10wt.%~30wt.%, Si: 1wt.%~20wt.%, C: 5wt.%~30wt.%, and the remainder is O and unavoidable impurities.

[0021] In the present invention, the Cr element in the additive mainly exists in the form of Cr single substance, the Fe element mainly exists in the form of Fe single substance, and the Si and C elements exist in the form of carbides and silicides.

[0022] In the present invention, the additive contains 30wt.% to 60wt.% of Cr element, for example, 32wt.%, 35wt.%, 38wt.%, 40wt.%, 42wt.%, 45wt.%, 48wt.%, 50wt.%, 52wt.%, 55wt.% or 58wt.%, etc., and the additive contains 10wt.% to 30wt.% of Fe element, for example, 12wt.%, 15wt.%, 18wt.%, 20wt.%, 22wt.%, 25wt.% or 28wt.%, etc. The additive contains 1wt.% to 20wt.% of Si element, for example, 2wt.%, 5wt.%, 8wt.%, 10wt.%, 12wt.%, 15wt.% or 18wt.%, etc. The additive contains 5wt.% to 30wt.% of C element, for example, 8wt.%, 10wt.%, 12wt.%, 15wt.%, 18wt.%, 20wt.%, 22wt.%, 25wt.% or 28wt.%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0023] Preferably, the mass ratio of Fe to Cr in the additive in step (1) is (0.4-0.8):1, for example, it can be 0.45:1, 0.5:1, 0.55:1, 0.6:1, 0.65:1, 0.7:1 or 0.75:1, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] In the present invention, the mass ratio of Fe to Cr in the additive is controlled within a narrow range, thereby further improving the chromium oxidation rate and the purity of the subsequent leached chromium.

[0025] Preferably, the additive in step (1) comprises any one of ferrochrome, ferrochrome acid leaching residue or ferrochrome chlorination decomposition residue, or a combination of at least two of them, wherein the combinations are typically but not limitatively: a combination of ferrochrome and ferrochrome acid leaching residue, a combination of ferrochrome acid leaching residue and ferrochrome chlorination decomposition residue, or a combination of ferrochrome, ferrochrome acid leaching residue and ferrochrome chlorination decomposition residue, etc.

[0026] In the present invention, ferrochrome, ferrochrome acid leaching residue or ferrochrome chlorination decomposition residue is selected as an additive, so that chromium in the ferrochrome or its leaching residue can be fully extracted, and the conversion rate of chromium in the chromite / chromium slag roasting process is improved, the amount of aluminum mud generated is reduced, and low-temperature energy-saving roasting treatment of chromite is achieved.

[0027] As a preferred technical solution of the present invention, the mass ratio of the additive to the chromium-containing material in step (1) is (0.1-2):1, for example, it can be 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1 or 1.9:1, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably (0.2-1.5):1.

[0028] Preferably, after grinding and mixing in step (1), the average particle size of the mixed material is ≤74 μm, for example, it can be 72 μm, 70 μm, 68 μm, 65 μm, 60 μm, 55 μm, 50 μm or 40 μm, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] As a preferred technical solution of the present invention, the temperature of the oxidative roasting in step (1) is 300-1200°C, for example, it can be 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C or 1150°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 600-1000°C.

[0030] Preferably, the time of the oxidative roasting in step (1) is 10 to 400 min, for example, it can be 30 min, 50 min, 80 min, 100 min, 120 min, 150 min, 180 min, 200 min, 220 min, 250 min, 280 min, 300 min, 320 min, 350 min or 380 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] In the present invention, the equipment used for the oxidation roasting includes any one of a muffle furnace, a microwave heating furnace or an atmosphere furnace, or a combination of at least two of them.

[0032] Preferably, the oxidative roasting in step (1) is carried out in air and / or oxygen-rich gas.

[0033] In the present invention, the oxygen-rich gas is an atmosphere in which the volume percentage of oxygen is greater than 20%.

[0034] As a preferred technical solution of the present invention, step (1) further includes a second grinding after the oxidative roasting.

[0035] Preferably, after the second grinding, the average particle size of the calcined material is ≤74 μm, for example, it can be 72 μm, 70 μm, 68 μm, 65 μm, 60 μm, 55 μm, 50 μm or 40 μm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] As a preferred technical solution of the present invention, the leaching method in step (2) includes water immersion.

[0037] Preferably, the liquid-to-solid ratio of the leached liquid to the roasted clinker in step (2) is (2-10):1 mL / g, for example, it can be 3:1 mL / g, 4:1 mL / g, 5:1 mL / g, 6:1 mL / g, 7:1 mL / g, 8:1 mL / g or 9:1 mL / g, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0038] Preferably, the leaching temperature in step (2) is 50-100°C, for example, it can be 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C or 95°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0039] Preferably, the leaching time in step (2) is 1 to 5 hours, for example, it can be 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours or 4.5 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0040] Preferably, step (2) further includes solid-liquid separation after the leaching.

[0041] As a preferred technical solution of the present invention, the chromium content (in terms of Cr2O3) in the leached residue in step (2) is less than 2wt.%, for example, it can be 1.9wt.%, 1.8wt.%, 1.5wt.%, 1.4wt.%, 1.2wt.%, 1wt.%, 0.8wt.% or 0.5wt.%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0042] As a preferred technical solution of the present invention, the method comprises the following steps:

[0043] (1) grinding and mixing the chromium-containing material, alkali and additives, wherein the average particle size of the mixed material is ≤74 μm, then oxidizing and roasting the mixed material at a temperature of 300 to 1200° C. for 10 to 400 min, and then performing a second grinding to obtain a roasted clinker having an average particle size of ≤74 μm;

[0044] The chromium-containing material includes chromite and / or chromium slag; the alkali includes any one of sodium carbonate, potassium carbonate, sodium hydroxide or potassium hydroxide or a combination of at least two of them; the mass ratio of the alkali to the chromium-containing material is (0.5-2):1; the additive includes the following elements according to mass content: Cr: 30wt.%-60wt.%, Fe: 10wt.%-30wt.%, Si: 1wt.%-20wt.%, C: 5wt.%-30wt.%, the remainder is O and unavoidable impurities; the mass ratio of Fe to Cr in the additive is (0.4-0.8):1; the additive includes any one of ferrochrome, ferrochrome acid leaching residue or ferrochrome chlorination decomposition residue or a combination of at least two of them; the mass ratio of the additive to the chromium-containing material is (0.1-2):1;

[0045] (2) leaching the roasted clinker in step (1) at a temperature of 50 to 100° C. for 1 to 5 hours, and obtaining a leachate and a leach residue after solid-liquid separation;

[0046] The liquid-to-solid ratio of the leached liquid to the roasted clinker is (2-10): 1 mL / g;

[0047] The chromium content in the leached residue is less than 2 wt.%.

[0048] Compared with the prior art, the present invention has the following beneficial effects:

[0049] (1) The method for extracting chromium by oxidative roasting of chromium-containing materials provided by the present invention adopts a specific additive to mix with the chromium-containing material and alkali to achieve enhanced calcium-free roasting and effectively enhance the oxidative roasting process of the chromium-containing material, thereby achieving efficient extraction of chromium from the chromium-containing material and resource utilization of chromium in the additive, and significantly accelerating the oxidation reaction of chromium in the material, significantly improving the oxidation rate, and at the same time reducing the temperature of oxidative roasting, shortening the time of oxidative roasting, and achieving low-temperature energy-saving roasting treatment of chromite; subsequently, after leaching the roasted clinker, the chromium content (in terms of Cr2O3) in the leached residue is less than 2wt.%;

[0050] (2) The present invention adopts a specific additive, and the chromium resources in the additive are recycled; the iron element in the additive generates ferrate to enhance the roasting and chromium extraction, which helps to increase the oxidation rate of chromium; the silicon in the additive can combine with the aluminum in the chromium-containing material to form aluminosilicate and precipitate in the slag phase, reducing the amount of aluminum mud generated in the subsequent chromium salt production process; the carbon in the additive increases the calorific value during the roasting process, reduces the roasting temperature and time, and has the advantages of energy saving and emission reduction. DETAILED DESCRIPTION

[0051] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0052] In the following examples and comparative examples, the oxygen-rich gas is a gas having an oxygen content greater than 20% by volume.

[0053] Example 1

[0054] This embodiment provides a method for extracting chromium by oxidative roasting of a chromium-containing material, the method comprising the following steps:

[0055] (1) grinding and mixing chromite ore, sodium hydroxide and ferrochrome acid leaching residue in a mass ratio of 1:0.6:1.5, wherein the average particle size of the mixed material is ≤50 μm, and then oxidizing roasting is performed at a temperature of 800° C. for 120 min, and then a second grinding is performed to obtain a roasted clinker with an average particle size of ≤50 μm;

[0056] The content of Cr2O3 in the chromite is 43wt.%; the ferrochrome acid leaching residue includes the following elements by mass content: Cr: 45wt.%, Fe: 20wt.%, Si: 10wt.%, C: 10wt.%, and the balance is O and unavoidable impurities;

[0057] The oxidative roasting is carried out in air;

[0058] (2) soaking the roasted clinker in step (1) in water at a temperature of 100° C. for 1 hour, and obtaining a leachate and a leach residue after solid-liquid separation;

[0059] The liquid-to-solid ratio of the water in the water immersion to the roasted clinker is 6:1 mL / g.

[0060] Example 2

[0061] This embodiment provides a method for extracting chromium by oxidative roasting of a chromium-containing material, the method comprising the following steps:

[0062] (1) grinding and mixing chromite, sodium hydroxide and ferrochrome in a mass ratio of 1:0.9:0.2, wherein the average particle size of the mixed material is ≤70 μm, and then oxidizing roasting is performed at a temperature of 850° C. for 100 min, and then a second grinding is performed to obtain a roasted clinker with an average particle size of ≤70 μm;

[0063] The content of Cr2O3 in the chromite is 43wt.%; the ferrochrome includes the following elements by mass content: Cr: 52wt.%, Fe: 30wt.%, Si: 8wt.%, C: 5wt.%, and the balance is O and unavoidable impurities;

[0064] The oxidative roasting is carried out in air;

[0065] (2) soaking the roasted clinker in step (1) in water at a temperature of 80° C. for 0.5 h, and obtaining a leachate and a leach residue after solid-liquid separation;

[0066] The liquid-to-solid ratio of the water in the water immersion to the roasted clinker is 8:1 mL / g.

[0067] Example 3

[0068] This embodiment provides a method for extracting chromium by oxidative roasting of a chromium-containing material, the method comprising the following steps:

[0069] (1) grinding and mixing chromite ore, sodium carbonate and ferrochrome acid leaching residue in a mass ratio of 1:1.1:0.7, wherein the average particle size of the mixed material is ≤40 μm, and then oxidizing roasting is performed at a temperature of 950° C. for 150 min, and then a second grinding is performed to obtain a roasted clinker with an average particle size of ≤40 μm;

[0070] The content of Cr2O3 in the chromite is 43wt.%; the ferrochrome acid leaching residue includes the following elements by mass content: Cr: 43wt.%, Fe: 25wt.%, Si: 10wt.%, C: 15wt.%, and the balance is O and unavoidable impurities;

[0071] The oxidative roasting is carried out in air;

[0072] (2) soaking the roasted clinker in step (1) in water at 90° C. for 1.5 h, and obtaining a leachate and leach residue after solid-liquid separation;

[0073] The liquid-to-solid ratio of the water in the water immersion to the roasted clinker is 10:1 mL / g.

[0074] Example 4

[0075] This embodiment provides a method for extracting chromium by oxidative roasting of a chromium-containing material, the method comprising the following steps:

[0076] (1) grinding and mixing chromium slag, potassium hydroxide and chromium iron chlorination decomposition slag in a mass ratio of 1:0.5:1, wherein the average particle size of the mixed material is ≤38 μm, and then oxidizing roasting is performed at a temperature of 700° C. for 60 min, and then a second grinding is performed to obtain a roasted clinker with an average particle size of ≤38 μm;

[0077] The content of Cr2O3 in the chromium slag is 9wt.%; the ferrochrome chlorination decomposition slag includes the following elements by mass content: Cr: 31wt.%, Fe: 15wt.%, Si: 20wt.%, C: 19wt.%, and the balance is O and unavoidable impurities;

[0078] The oxidative roasting is carried out in an oxygen-rich gas;

[0079] (2) soaking the roasted clinker in step (1) in water at a temperature of 85° C. for 2 h, and obtaining a leachate and a leach residue after solid-liquid separation;

[0080] The liquid-to-solid ratio of the water in the water immersion to the roasted clinker is 4:1 mL / g.

[0081] Example 5

[0082] This embodiment provides a method for extracting chromium by oxidative roasting of a chromium-containing material, the method comprising the following steps:

[0083] (1) grinding and mixing chromium slag, potassium carbonate and chromium ferrochlorination decomposition slag in a mass ratio of 1:2:1.4, wherein the average particle size of the mixed material is ≤45 μm, and then oxidizing roasting is performed at a temperature of 1000° C. for 30 minutes, and then a second grinding is performed to obtain a roasted clinker with an average particle size of ≤45 μm;

[0084] The content of Cr2O3 in the chromium slag is 9wt.%; the ferrochrome chlorination decomposition slag includes the following elements by mass content: Cr: 32wt.%, Fe: 19wt.%, Si: 18wt.%, C: 15wt.%, and the remainder is O and unavoidable impurities;

[0085] The oxidative roasting is carried out in air;

[0086] (2) soaking the roasted clinker in step (1) in water at a temperature of 65° C. for 2 h, and obtaining a leachate and a leach residue after solid-liquid separation;

[0087] The liquid-to-solid ratio of the water in the water immersion to the roasted clinker is 5:1 mL / g.

[0088] Example 6

[0089] This embodiment provides a method for extracting chromium by oxidative roasting of a chromium-containing material, the method comprising the following steps:

[0090] (1) grinding and mixing chromite ore, potassium carbonate and chromium ferrochlorination decomposition slag in a mass ratio of 1:1.5:0.9, wherein the average particle size of the mixed material is ≤45 μm, and then oxidizing roasting is performed at a temperature of 700° C. for 60 min, and then a second grinding is performed to obtain a roasted clinker with an average particle size of ≤45 μm;

[0091] The content of Cr2O3 in the chromite is 43wt.%; the chromium-iron chlorination decomposition slag includes the following elements by mass content: Cr: 35wt.%, Fe: 17wt.%, Si: 15wt.%, C: 13wt.%, and the remainder is O and unavoidable impurities;

[0092] The oxidative roasting is carried out in an oxygen-rich gas;

[0093] (2) soaking the roasted clinker in step (1) in water at a temperature of 85° C. for 2 h, and obtaining a leachate and a leach residue after solid-liquid separation;

[0094] The liquid-to-solid ratio of the water in the water immersion to the roasted clinker is 4:1 mL / g.

[0095] Example 7

[0096] The present embodiment provides a method for extracting chromium by oxidative roasting of a chromium-containing material, except that the ferrochrome acid leaching residue in step (1) is adjusted to include the following elements by mass content: Cr: 30wt.%, Fe: 30wt.%, Si: 2wt.%, C: 10wt.%, and the remainder is O and unavoidable impurities; other conditions are the same as those in Example 1.

[0097] Example 8

[0098] The present embodiment provides a method for extracting chromium by oxidative roasting of a chromium-containing material, except that the ferrochrome acid leaching residue in step (1) is adjusted to include the following elements by mass content: Cr: 45wt.%, Fe: 8wt.%, Si: 10wt.%, C: 10wt.%, and the remainder is O and unavoidable impurities; other conditions are the same as those in Example 1.

[0099] Example 9

[0100] The present embodiment provides a method for extracting chromium by oxidative roasting of a chromium-containing material, except that the ferrochromium in step (1) is adjusted to include the following elements by mass content: Cr: 55wt.%, Fe: 30wt.%, Si: 17wt.%, C: 1wt.%, and the remainder is O and unavoidable impurities; other conditions are the same as those in Example 1.

[0101] Example 10

[0102] This embodiment provides a method for extracting chromium by oxidative roasting of a chromium-containing material, except that the mass ratio of chromite ore to ferrochrome acid leaching residue in step (1) is 1:3; other conditions are the same as those in Example 1.

[0103] Embodiment 11

[0104] This embodiment provides a method for extracting chromium by oxidative roasting of a chromium-containing material. Except that the oxidative roasting temperature in step (1) is 300° C., other conditions are the same as those in Example 1.

[0105] Example 12

[0106] This embodiment provides a method for extracting chromium by oxidative roasting of a chromium-containing material. Except that the oxidative roasting temperature in step (1) is 1200° C., other conditions are the same as those in Example 1.

[0107] Comparative Example 1

[0108] This comparative example provides a method for extracting chromium by oxidative roasting of a chromium-containing material, except that no ferrochromium acid leaching residue is added in step (1); other conditions are the same as those in Example 1.

[0109] Comparative Example 2

[0110] This comparative example provides a method for extracting chromium by oxidative roasting of a chromium-containing material, except that no ferrochromium acid leaching residue is added in step (1); other conditions are the same as those in Example 3.

[0111] Comparative Example 3

[0112] This comparative example provides a method for extracting chromium by oxidative roasting of a chromium-containing material, except that no ferrochromium chlorination decomposition slag is added in step (1); other conditions are the same as those in Example 4.

[0113] After the clinker, leachate and leached residue obtained in the above examples and comparative examples were tested, the oxidation rate of chromium after roasting in step (1), the leaching rate of chromium after step (2) and the chromium content (in terms of Cr2O3) of the leached residue were calculated. The results are shown in Table 1.

[0114] Table 1 Chromium oxidation rate, leaching rate and chromium content of leached residue in each embodiment and comparative example

[0115]

[0116]

[0117] From Table 1, we can see that:

[0118] (1) The method for extracting chromium by oxidative roasting of chromium-containing materials provided in Examples 1-6 of the present invention uses a specific additive mixed with the chromium-containing material and an alkali to achieve efficient extraction and recovery of chromium from the chromium-containing material and the additive, with an oxidation rate of chromium greater than 93%, a leaching rate of chromium greater than 99%, and a chromium content (in terms of Cr2O3) of the leached residue less than 2 wt.%;

[0119] (2) From the comparison between Example 1 and Example 7, it can be seen that when the mass ratio of Fe to Cr in the additive is too large, although it will not affect the oxidation rate of chromium and the subsequent chromium leaching rate, excessive ferrate is generated, resulting in residual ferrate in the roasted clinker, and the iron content in the solution after leaching is high, which affects the purity of chromium in the leachate; from the comparison between Example 1 and Examples 8-9, it can be seen that when the content of Fe in the additive is too low, it is not conducive to strengthening the roasting and chromium extraction, resulting in a decrease in the oxidation rate of chromium in the roasted clinker; when the content of C in the additive is too low, it is not conducive to increasing the calorific value of the roasting process, and at the same roasting temperature, it leads to the disadvantages of incomplete roasting of the material and high energy consumption;

[0120] (3) It can be seen from the comparison between Example 1 and Example 10 that when the amount of additive is too much, due to the addition of a large amount of additive, part of the additive does not participate in the reaction, so the oxidation rate of chromium is not further improved and the chromium content of the slag is increased;

[0121] (4) By comparing Example 1 with Examples 11-12, it can be seen that when the temperature of the oxidative roasting is too low, the chromium extraction rate is low due to incomplete roasting; when the temperature of the oxidative roasting is too high, the material will become hardened during the roasting process due to the high temperature, which is not conducive to the leaching of chromium and increases energy consumption;

[0122] (5) By comparing the embodiment with comparative examples 1-3, it can be seen that when no additive is added, it is not conducive to the efficient extraction and recovery of chromium in the chromium-containing material, the oxidation rate of chromium in the roasted clinker is greatly reduced, and the chromium content (in terms of Cr2O3) in the leached slag is increased.

[0123] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for extracting chromium by oxidative roasting of chromium-containing materials, characterized in that: The method comprises the following steps: (1) grinding and mixing the chromium-containing material, alkali and additives, and then oxidizing and roasting to obtain roasted clinker; The additives include the following elements: Cr, Fe, Si, C; (2) Leaching the roasted clinker in step (1) to obtain a leachate and leach residue.

2. The method according to claim 1, characterized in that The chromium-containing material in step (1) includes chromite and / or chromium slag.

3. The method according to claim 1 or 2, characterized in that: The base in step (1) comprises any one of sodium carbonate, potassium carbonate, sodium hydroxide or potassium hydroxide, or a combination of at least two thereof; Preferably, in step (1), the mass ratio of the alkali to the chromium-containing material is (0.5-2):

1.

4. The method according to any one of claims 1 to 3, characterized in that: The additive in step (1) comprises the following elements by mass content: Cr: 30wt.% to 60wt.%, Fe: 10wt.% to 30wt.%, Si: 1wt.% to 20wt.%, C: 5wt.% to 30wt.%, and the remainder is O and unavoidable impurities; Preferably, the mass ratio of Fe to Cr in the additive in step (1) is (0.4-0.8):1; Preferably, the additive in step (1) comprises any one of ferrochrome, ferrochrome acid leaching residue or ferrochrome chlorination decomposition residue, or a combination of at least two thereof.

5. The method according to any one of claims 1 to 4, characterized in that: The mass ratio of the additive to the chromium-containing material in step (1) is (0.1-2):1, preferably (0.2-1.5):1; Preferably, after grinding and mixing in step (1), the average particle size of the mixed material is ≤74 μm.

6. The method according to any one of claims 1 to 5, characterized in that: The temperature of the oxidation roasting in step (1) is 300-1200° C., preferably 600-1000° C.; Preferably, the oxidative roasting time in step (1) is 10 to 400 minutes; Preferably, the oxidative roasting in step (1) is carried out in air and / or oxygen-rich gas.

7. The method according to any one of claims 1 to 6, characterized in that: Step (1) further comprises a second grinding after the oxidative roasting; Preferably, after the second grinding, the average particle size of the roasted clinker is ≤74 μm.

8. The method according to any one of claims 1 to 7, characterized in that: The leaching method in step (2) includes water immersion; Preferably, the liquid-to-solid ratio of the leached liquid to the roasted clinker in step (2) is (2-10): 1 mL / g; Preferably, the leaching temperature in step (2) is 50-100°C; Preferably, the leaching time in step (2) is 1 to 5 hours; Preferably, step (2) further includes solid-liquid separation after the leaching.

9. The method according to any one of claims 1 to 8, characterized in that: The chromium content in the leached residue in step (2) is less than 2wt.%.

10. The method according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: (1) grinding and mixing the chromium-containing material, alkali and additives, wherein the average particle size of the mixed material is ≤74 μm, then oxidizing and roasting the mixed material at a temperature of 300 to 1200° C. for 10 to 400 min, and then performing a second grinding to obtain a roasted clinker having an average particle size of ≤74 μm; The chromium-containing material includes chromite and / or chromium slag; the alkali includes any one of sodium carbonate, potassium carbonate, sodium hydroxide or potassium hydroxide or a combination of at least two of them; the mass ratio of the alkali to the chromium-containing material is (0.5-2):1; the additive includes the following elements by mass content: Cr: 30wt.%-60wt.%, Fe: 10wt.%-30wt.%, Si: 1wt.%-20wt.%, C: 5wt.%-30wt.%, the remainder is O and unavoidable impurities; the mass ratio of Fe to Cr in the additive is (0.4-0.8):1; the additive includes any one of ferrochrome, ferrochrome acid leaching residue or ferrochrome chlorination decomposition residue or a combination of at least two of them; the mass ratio of the additive to the chromium-containing material is (0.1-2):1; (2) leaching the roasted clinker in step (1) at a temperature of 50 to 100° C. for 1 to 5 hours, and obtaining a leachate and a leach residue after solid-liquid separation; The liquid-to-solid ratio of the leached liquid to the roasted clinker is (2-10): 1 mL / g; The chromium content in the leached residue is less than 2 wt.%.

Citation Information

Patent Citations

  • Method for extracting Cr from Cr-containing material by liquid-phase oxidation

    CN109399715A

  • Method for extracting chromium by controlling oxidizing roasting of return slag composition

    CN109402377A

  • Method for extracting Cr from Cr-containing material by oxidizing roasting

    CN109402378A

  • Method for extracting Cr from Cr-containing material by liquid-phase oxidation

    CN109402416A

  • Method for extracting chromium from chromium-containing material

    CN112063860A