Diamond aluminum-based composite material and preparation method thereof
By filling the powder protector inside the aluminum block and using binder to enhance the diamond particles, the performance problems caused by the oxidation of aluminum are solved, the mechanical properties and thermal conductivity of diamond aluminum-based composite materials are improved, and the preparation cost is reduced.
Patent Information
- Application Number
- CN202411092403.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
During the preparation process of existing diamond aluminum-based composite materials, aluminum is prone to oxidation, resulting in low product density, weak bonding strength and poor thermal conductivity, which increases the production difficulty and cost.
By filling the aluminum block with powder protective agent, a dense protective layer is formed, which prevents oxygen contact and improves the fluidity of aluminum liquid. Combined with binders such as paraffin or polyvinyl alcohol to enhance the adhesion of diamond particles, and performs low-cost melting and seepage preparation.
The fluidity and coverage effect of aluminum liquid are improved, the bending strength, thermal expansion coefficient and thermal conductivity of the prepared diamond aluminum-based composite materials are enhanced, and the preparation cost is reduced.
Smart Images

Figure CN118996191A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electronic packaging materials, and in particular to a diamond aluminum-based composite material and a preparation method thereof. Background Art
[0002] Metal diamond composite materials with high thermal conductivity diamond as the reinforcement phase and copper, aluminum and other metals as the matrix have the characteristics of high thermal conductivity and low thermal expansion coefficient. They are often used as heat sink materials and substrates in electronic packaging. Among them, diamond aluminum plays an irreplaceable role in occasions with very high lightweight requirements because the matrix metal aluminum composite material has a very low density.
[0003] Diamond aluminum-based composite materials are currently mainly prepared by melt infiltration. Generally, diamond particles are first made into a blank, and then aluminum is melted. Under the action of capillary action or external pressure, the aluminum liquid enters the pores in the blank, and the diamond aluminum material is obtained after cooling. However, since aluminum is very easy to oxidize and react with a variety of elements, the sintering furnace needs to have a very high cleanliness and vacuum degree to ensure that the aluminum liquid is not oxidized or reacts with other elements in the furnace. This undoubtedly increases the difficulty and cost of preparing diamond aluminum-based composite materials, and the prepared products are prone to low density, weak bonding strength, and poor thermal conductivity, which affects product performance and application. Summary of the invention
[0004] The present invention provides a diamond aluminum-based composite material and a preparation method thereof, the purpose of which is to solve the above-mentioned problems existing in the background technology.
[0005] In order to achieve the above-mentioned purpose, an embodiment of the present invention provides a diamond aluminum-based composite material and a preparation method thereof, which ensures the fluidity of aluminum by adding an aluminum liquid protective agent to achieve low-cost preparation of diamond aluminum.
[0006] An embodiment of the present invention provides a method for preparing a diamond aluminum-based composite material, comprising the following steps:
[0007] S1: Grind and mix the covering agent and the reactant thoroughly to prepare a powder protective agent;
[0008] S2: taking an aluminum block, cleaning it, and hollowing out the inside, and filling the powder protective agent into the hollowed-out part of the aluminum block, compacting it, and then plugging it with an aluminum block to obtain an aluminum block filled with the protective agent;
[0009] S3: loading diamond particles into a mold or making a preform with diamond particles and a binder, placing the aluminum block filled with a protective agent on the mold or the preform, and then placing the mold or the preform into a crucible; the binder is at least one of paraffin wax, polyvinyl alcohol (PVA), and polyacrylate, which increases the adhesion of the diamond particles so that the preform with a certain strength is formed during the cold pressing process;
[0010] S4: placing the crucible in a sintering furnace, evacuating the furnace, heating it, and then maintaining the temperature for infiltration;
[0011] S5: After the infiltration is completed, the material is cooled to room temperature with the furnace, and the slag on the surface of the material is removed after being taken out, and the excess aluminum is cut off.
[0012] According to one aspect of an embodiment of the present invention, in step S1, the reactant is CaF 2 , AlF 3 、Na 3 AlF 6 , LiCl.
[0013] According to one aspect of the embodiment of the present invention, in step S1 , the covering agent includes NaCl crystals and KCl crystals.
[0014] According to one aspect of an embodiment of the present invention, in step S1, the mass fractions of NaCl crystals and KCl crystals are 60% to 85% and 15% to 35% of the powder protective agent respectively; the mass fraction of the reactant is 5% to 10%.
[0015] According to one aspect of an embodiment of the present invention, in step S2, the aluminum block is any one of pure aluminum, Al-Si alloy, Al-Mg alloy, Al-Si-Mg alloy, Al-Mn alloy, and Al-Cu alloy.
[0016] According to one aspect of the embodiment of the present invention, in step S2, the volume of the protective agent accounts for 10% to 20% of the entire aluminum block.
[0017] According to one aspect of an embodiment of the present invention, in step S4, the vacuum is evacuated to below 20 Pa; the infiltration temperature is 20 to 50° C. above the melting point of the aluminum block, and the insulation time is 20 to 120 min.
[0018] According to one aspect of an embodiment of the present invention, in step S4, the top and the bottom of the sintering furnace each include at least one heating element and / or a cooling device to independently control the heating or heat dissipation power.
[0019] Based on a general concept of the invention, an embodiment of the present invention provides a diamond aluminum-based composite material prepared by the above-mentioned preparation method.
[0020] The above scheme of the present invention has the following beneficial effects:
[0021] (1) During the infiltration process of the preparation method of a diamond aluminum-based composite material of the present invention, the protective agent forms a dense protective layer on the surface of the aluminum liquid, preventing oxygen from contacting the aluminum liquid and reacting with the generated oxides, thereby improving the fluidity of the aluminum liquid and being more conducive to the infiltration of the aluminum liquid between the diamond particles; the method of using aluminum-coated protective agents not only reduces the reaction between the protective agent and other impurities in the furnace during the early heating and melting stage, but also ensures that the protective agent flows out again after the aluminum base is melted, thereby forming a better covering effect on the aluminum liquid.
[0022] (2) The present invention arranges a protective agent inside the aluminum block, so that the prepared diamond aluminum-based composite material has better bending strength mechanical properties, thermal expansion coefficient and thermal conductivity than when the protective agent is arranged on the surface of the aluminum block. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 It is a schematic flow chart of a method for preparing a diamond aluminum-based composite material of the present invention. DETAILED DESCRIPTION
[0025] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.
[0026] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0027] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0028] In view of the existing problems, the present invention provides a diamond aluminum-based composite material and a preparation method thereof. The flow diagram of the preparation method is as follows: Figure 1 As shown, the following steps are included:
[0029] S1: Grind and mix the covering agent and the reactant thoroughly to prepare a powder protective agent;
[0030] S2: taking an aluminum block, cleaning it, and hollowing out the inside, and filling the powder protective agent into the hollowed-out part of the aluminum block, compacting it, and then plugging it with an aluminum block to obtain an aluminum block filled with the protective agent;
[0031] S3: loading diamond particles into a mold or making a preform with diamond particles and a binder, placing the aluminum block filled with a protective agent on the mold or the preform, and then placing the mold or the preform into a crucible; the binder is at least one of paraffin wax, polyvinyl alcohol (PVA), and polyacrylate, which increases the adhesion of the diamond particles so that the preform with a certain strength is formed during the cold pressing process;
[0032] S4: placing the crucible in a sintering furnace, evacuating the furnace, heating it, and then maintaining the temperature for infiltration;
[0033] S5: After the infiltration is completed, the material is cooled to room temperature with the furnace, and the slag on the surface of the material is removed after being taken out, and the excess aluminum is cut off.
[0034] According to one aspect of an embodiment of the present invention, in step S1, the reactant is CaF 2 , AlF 3 、Na 3 AlF 6 , LiCl.
[0035] According to one aspect of the embodiment of the present invention, in step S1 , the covering agent includes NaCl crystals and KCl crystals.
[0036] According to one aspect of an embodiment of the present invention, in step S1, the mass fractions of NaCl crystals and KCl crystals are 60% to 85% and 15% to 35% of the powder protective agent respectively; the mass fraction of the reactant is 5% to 10%.
[0037] According to one aspect of an embodiment of the present invention, in step S2, the aluminum block is any one of pure aluminum, Al-Si alloy, Al-Mg alloy, Al-Si-Mg alloy, Al-Mn alloy, and Al-Cu alloy.
[0038] According to one aspect of the embodiment of the present invention, in step S2, the volume of the protective agent accounts for 10% to 20% of the entire aluminum block.
[0039] According to one aspect of an embodiment of the present invention, in step S4, the vacuum is evacuated to below 20 Pa; the infiltration temperature is 20 to 50° C. above the melting point of the aluminum block, and the insulation time is 20 to 120 min.
[0040] According to one aspect of an embodiment of the present invention, in step S4, the top and the bottom of the sintering furnace each include at least one heating element and / or a cooling device to independently control the heating or heat dissipation power.
[0041] Based on a general concept of the invention, an embodiment of the present invention provides a diamond aluminum-based composite material prepared by the above-mentioned preparation method.
[0042] The following will be described through specific examples and comparative examples.
[0043] The following will describe the invention through specific embodiments.
[0044] Example 1
[0045] This embodiment provides a method for preparing a diamond aluminum-based composite material.
[0046] The method of this embodiment includes the following steps:
[0047] Step 1: Prepare protective agent: According to the mass percentage, 72% NaCl crystals and 22% KCl crystals are used as the covering agent, and 6% Na 3 AlF 6 The reactants are fully ground and mixed to prepare a powder protective agent;
[0048] Step 2: Aluminum coating protective agent: clean the pure aluminum block to be infiltrated, hollow out the middle to hold the protective agent. Put the above protective agent into the hollowed part, compact it, and then plug it with aluminum block. The volume fraction of the protective agent accounts for 15% of the aluminum block, and obtain an aluminum block filled with protective agent;
[0049] Step 3: Infiltration preparation: diamond particles are loaded into the mold to be formed or diamond particles and a binder are made into a preform, and then the mold or preform is placed in a crucible, and an aluminum block coated with a protective agent is placed on the mold or preform;
[0050] Step 4: Infiltration sintering: Place the crucible in a sintering furnace, evacuate to below 20 Pa, heat to 700°C, and keep warm for 60 minutes to melt the aluminum and fully infiltrate into the diamond particles under capillary action;
[0051] Step 5: Forming and post-processing: After the infiltration is completed, wait for the material to cool to room temperature with the furnace, remove the slag on the surface of the material, cut off the excess aluminum, and obtain diamond aluminum material.
[0052] Example 2
[0053] This embodiment provides a method for preparing a diamond aluminum-based composite material.
[0054] The method of this embodiment includes the following steps:
[0055] Step 1: Prepare protective agent: According to the mass percentage, 65% NaCl crystals, 30% KCl crystals and 5% CaF 2 and AlF3 The reactants are fully ground and mixed to prepare a powder protective agent;
[0056] Step 2: Aluminum coating protective agent: Clean the Al9Si1Mg aluminum block to be infiltrated, hollow out the middle to hold the protective agent. Put the above protective agent into the hollowed part, compact it, and then plug it with aluminum block. The volume fraction of the protective agent accounts for 20% of the aluminum block, and obtain an aluminum block filled with protective agent;
[0057] Step 3: Infiltration preparation: diamond particles are loaded into the mold to be formed or diamond particles and a binder are made into a preform, and then the mold or preform is placed in a crucible, and an aluminum block coated with a protective agent is placed on the mold or preform;
[0058] Step 4: Infiltration sintering: Place the crucible in a sintering furnace, evacuate to below 20 Pa, heat to 660°C, and keep warm for 90 minutes to melt the aluminum and fully infiltrate into the diamond particles under capillary action;
[0059] Step 5: Forming and post-processing: After the infiltration is completed, wait for the material to cool to room temperature with the furnace, remove the slag on the surface of the material, cut off the excess aluminum, and obtain diamond aluminum material.
[0060] Comparative Example 1
[0061] The difference between this embodiment and Example 1 is that the protective agent is not placed inside the aluminum block, but on the upper surface of the aluminum block, and the remaining steps are the same.
[0062] Comparative Example 2
[0063] The present embodiment is different from Example 1 in that no protective agent is used, and the remaining steps are the same.
[0064] Comparative Example 3
[0065] The difference between this embodiment and Example 1 is that the volume of the protective agent accounts for 5% of the entire aluminum block, and the remaining steps are the same.
[0066] Comparative Example 4
[0067] The difference between this embodiment and Example 1 is that the volume of the protective agent accounts for 30% of the entire aluminum block, and the remaining steps are the same.
[0068] Comparative Example 5
[0069] The present embodiment is different from Example 1 in that the composition of the protective agent is different, the NaCl crystals are replaced with MgCl crystals, and the remaining steps are the same.
[0070] Comparative Example 6
[0071] The difference between this embodiment and Example 1 is that the composition of the protective agent is different, and the NaCl crystals are replaced by NaNO 3 Crystal, the rest of the steps are the same.
[0072] Comparative Example 7
[0073] The difference between this embodiment and Example 1 is that the mass fraction of the reactant is 3%, and the other steps are the same.
[0074] Comparative Example 8
[0075] The difference between this embodiment and Example 1 is that the mass fraction of the reactant is 15%, and the remaining steps are the same.
[0076] Comparative Example 9
[0077] The difference between this embodiment and Example 1 is that the mass fraction of NaCl is 50%, and the other steps are the same.
[0078] Comparative Example 10
[0079] The difference between this embodiment and Example 1 is that the mass fraction of NaCl is 90%, and the other steps are the same.
[0080] The composite materials prepared in Examples 1 to 2 and Comparative Examples 1 to 10 were tested for flexural strength, mechanical properties, thermal expansion coefficient and thermal conductivity. The test results are shown in Table 1 below.
[0081] The test methods are as follows: the flexural strength test refers to GBT6569-2006-Fine Ceramics Flexural Strength Test Method; the thermal expansion coefficient test refers to QBT 1321-1991 Ceramic Material Average Linear Thermal Expansion Coefficient Determination Method; the thermal conductivity test method first refers to GB / T 22588-2008 Flash Method for Measurement of Thermal Diffusivity or Thermal Conductivity to measure the thermal conductivity, then the drainage method is used to measure the material density and the corresponding theoretical specific heat capacity, and finally the thermal conductivity of the material is calculated by the formula.
[0082] Table 1 Mechanical and thermal properties test results
[0083] Flexural strength(MPa) Thermal expansion coefficient (ppm / K) Thermal conductivity (W / (m·K)) Example 1 327 8.2 577 Example 2 296 8.6 593 Comparative Example 1 105 11.2 248 Comparative Example 2 Sintering failure Sintering failure Sintering failure Comparative Example 3 125 10.6 128 Comparative Example 4 225 9.2 431 Comparative Example 5 169 10.1 268 Comparative Example 6 168 10.6 235 Comparative Example 7 233 9.5 379 Comparative Example 8 240 9.6 365 Comparative Example 9 216 10.3 332 Comparative Example 10 246 9.5 347
[0084] As can be seen from Table 1, since the protective agent in Comparative Example 1 is not placed inside the aluminum block, the covering effect is poor, the aluminum liquid is oxidized to a certain extent, and the fluidity of aluminum is weak, so the performance of the prepared material is poor; in Comparative Example 2, due to the lack of a protective agent, the aluminum liquid is severely oxidized, a layer of aluminum oxide skin is formed on the surface, and the fluidity is poor, and it cannot enter the diamond particles during the melting stage.
[0085] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a diamond aluminum-based composite material, characterized in that: The steps include: S1: Grind and mix the covering agent and the reactant thoroughly to prepare a powder protective agent; S2: taking an aluminum block, cleaning it, and hollowing out the inside, and filling the powder protective agent into the hollowed-out part of the aluminum block, compacting it, and then plugging it with an aluminum block to obtain an aluminum block filled with the protective agent; S3: loading diamond particles into a mold or making a preform with diamond particles and a binder, placing the aluminum block filled with a protective agent on the mold or the preform, and then placing the mold or the preform into a crucible; S4: placing the crucible in a sintering furnace, evacuating the furnace, heating it, and then maintaining the temperature for infiltration; S5: After the infiltration is completed, the material is cooled to room temperature with the furnace, and the slag on the surface of the material is removed after being taken out, and the excess aluminum is cut off.
2. The method for preparing a diamond aluminum-based composite material according to claim 1, characterized in that: In step S1, the reactant is at least one of CaF2, AlF3, Na3AlF6, and LiCl.
3. The method for preparing a diamond aluminum-based composite material according to claim 1, characterized in that: In step S1, the covering agent includes NaCl crystals and KCl crystals.
4. The method for preparing a diamond aluminum-based composite material according to claim 3, characterized in that: In step S1, the mass fractions of NaCl crystals and KCl crystals are 60% to 85% and 15% to 35% of the powder protective agent respectively; the mass fraction of the reactant is 5% to 10%.
5. The method for preparing a diamond aluminum-based composite material according to claim 1, characterized in that: In step S2, the aluminum block is any one of pure aluminum, Al-Si alloy, Al-Mg alloy, Al-Si-Mg alloy, Al-Mn alloy, and Al-Cu alloy.
6. The method for preparing a diamond aluminum-based composite material according to claim 1, characterized in that: In step S2, the volume of the protective agent accounts for 10% to 20% of the entire aluminum block.
7. The method for preparing a diamond aluminum-based composite material according to claim 1, characterized in that: In step S3, the binder is at least one of paraffin, polyvinyl alcohol (PVA), and polyacrylate.
8. The method for preparing a diamond aluminum-based composite material according to claim 1, characterized in that: In step S4, the vacuum is evacuated to below 20 Pa; the infiltration temperature is 20 to 50° C. above the melting point of the aluminum block, and the insulation time is 20 to 120 min.
9. The method for preparing a diamond aluminum-based composite material according to claim 1, characterized in that: In step S4, the top and bottom of the sintering furnace each include at least one heating element and / or cooling device to independently control the heating or heat dissipation power.
10. A diamond aluminum-based composite material prepared by the preparation method according to any one of claims 1 to 9.