Production method of 20CrMoA round steel for sucker rod
Through converter smelting, LF refining and VD vacuum degassing process flows, combined with specific chemical components and heat treatment, the problem of insufficient mechanical properties of round steel for suction rods is solved, and high-strength and long-life 20CrMoA round steel production is achieved, reducing the production of 20CrMoA round steel The production cost is achieved and the cleanliness and fatigue resistance of the material is improved.
Patent Information
- Application Number
- CN202411063639.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The prior art is difficult to significantly improve the mechanical properties of round steel for suction rods while reducing production costs, resulting in insufficient service life and safety in oil well operations.
Using converter smelting, LF refining, VD vacuum degassing, continuous casting and round steel rolling, combined with specific chemical composition and heat treatment systems, including the addition of deoxidant and high-purity alloys to the converter for pre-deoxygenation, in the LF furnace Perform full-process stirring and strengthened desalination of high alkaline slag, VD vacuum degassing to remove debris, full-protect casting of continuous casting machine, control temperature uniformity during billet heating and rolling, and the heat treatment system is 880℃ quenching and 500℃ temptation .
The longitudinal mechanical properties and impact work of 20CrMoA round steel for suction rods are significantly improved, which extends the service life, reduces production costs, and improves the cleanliness and fatigue resistance of the material.
Smart Images

Figure SMS_1 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of smelting and rolling, and in particular relates to a production method of 20CrMoA round steel for pumping rods. Background Art
[0002] As global oil demand continues to grow, the demand for high-performance pumping equipment is also increasing. In particular, as oilfield exploitation expands to deep wells and the ocean, the performance requirements for materials are more stringent. Sucker rods need to withstand huge tension and pressure in oil well operations, so there are extremely high requirements for the strength and durability of round steel. By optimizing the alloy composition and heat treatment process, steel mills can produce high-strength, wear-resistant, and corrosion-resistant round steel for pump rods to meet the needs of harsh working environments. Pump rods are subject to frequent cyclic loads during use, and good fatigue resistance is the key to ensuring their long-term reliable operation. Steel mills can use advanced metallurgical technology and precision processing technology to produce round steel with excellent fatigue resistance, extend the service life of pump rods, and reduce the frequency of maintenance and replacement. High-performance round steel for pump rods will become an important material in the field of oilfield equipment manufacturing and has broad market prospects. By improving the performance and service life of round steel for pump rods, the maintenance and replacement costs of oilfield equipment can be significantly reduced, and mining efficiency can be improved. The high-performance round steel produced by steel mills can not only bring economic benefits to oilfield enterprises, but also enhance the market competitiveness and economic benefits of steel mills themselves. Summary of the invention
[0003] The purpose of the present invention is to provide a production method of 20CrMoA round steel for pumping rods, which utilizes the principle of composite alloying of a small amount of Cr and Mo to significantly improve the mechanical properties of hot-rolled round steel while reducing production costs, thereby producing 20CrMoA round steel for pumping rods, thereby significantly improving the overall life and safety of the pumping rods.
[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0005] The present invention discloses a production method of 20CrMoA round steel for pumping rods, which comprises: converter smelting, LF refining, VD vacuum degassing, continuous casting, heating in a casting furnace, and round steel rolling; wherein:
[0006] Combined blowing converter smelting ensures that the smelting materials are dry to prevent water vapor from entering the steel to produce white spots; [P] < 0.012%, [S] < 0.030%; 4.0 kg of AlMnFe deoxidizer and various high-purity alloys are added per ton for pre-deoxidation and initial adjustment of Si, Mn, Cr, Mo and other components during steel tapping, and slag retention during steel tapping is used to prevent P from returning; 2.5-4 kg of binary synthetic slag is added per ton during steel tapping; slag is blocked during steel tapping, and argon is blown throughout the steel tapping process;
[0007] In the LF furnace, the molten steel is deeply stripped and alloyed, and high basicity slag (R≥3.0) is made to strengthen the removal of sulfur and inclusions. The refining process adopts stirring throughout the whole process;
[0008] After LF refining, use VD circulating degassing equipment to perform vacuum degassing and remove impurities. Maintain it under high vacuum for more than 25 minutes to ensure that [H] ≤ 0.0002%, [O] ≤ 0.0020%, and all components are within the required range;
[0009] Adopt continuous casting machine, use mold protection slag, work casting speed is 1.5-1.8m / min, implement full protection casting to produce continuous casting billet, the billet enters the slow cooling pit, the slow cooling time is ≥24 hours;
[0010] The billet heating temperature is 1080~1120℃, the allowable temperature difference is ≤50℃, the total heating time is controlled to be 2h, the rolling temperature is 1030~1050℃, prevent overheating, overburning and decarburization, and heat up slowly to ensure uniform billet heating temperature and reduce temperature difference;
[0011] The heat treatment system is quenching at 880℃ and tempering at 500℃;
[0012] The mass percentage of the chemical composition of the 20CrMoA round steel includes: C 0.17%-0.24%, Si 0.17%-0.37%, Mn 0.40%-0.70%, P≤0.025%, S≤0.020%, Cr 0.80-1.10%, Mo 0.15-0.25%, Ni≤0.30%, Cu≤0.20%, and the rest is Fe and inevitable trace impurities, with a total mass fraction of 100%.
[0013] Furthermore, pay attention to the condition of the rollers, steel turning machines, guide plates, roller tables and cover plates, and ensure that they are smooth and have no sharp edges to avoid scratches and bumps on the surface of the rolled product.
[0014] Furthermore, the specification of the rolled product is φ120mm.
[0015] Furthermore, the produced 20CrMoA round steel for sucker rods meets the following requirements: longitudinal mechanical properties Rm≥735MPa, ReL≥930MPa, A≥12.0%, Z≥50%, impact energy KU2≥78J, austenite grain size≥8 levels, and no cracks, scars, folds or inclusions on the steel surface.
[0016] Furthermore, the mass percentage of the chemical composition of the 20CrMoA round steel includes: C 0.19%, Si 0.26%, Mn 0.58%, P: 0.012%, S: 0.0058%, Cr 0.92%, Mo 0.20%, Ni: 0.03%, Cu: 0.04%, and the rest is Fe and inevitable trace impurities, with a total mass fraction of 100%.
[0017] Furthermore, the mass percentage of the chemical composition of the 20CrMoA round steel includes: C 0.23%, Si 0.28%, Mn 0.62%, P: 0.014%, S: 0.0075%, Cr 0.95%, Mo 0.23%, Ni: 0.05%, Cu: 0.03%, and the rest is Fe and inevitable trace impurities, with a total mass fraction of 100%.
[0018] Furthermore, the mass percentage of the chemical composition of the 20CrMoA round steel includes: C 0.20%, Si 0.27%, Mn 0.60%, P: 0.013%, S: 0.0055%, Cr 0.93%, Mo 0.21%, Ni: 0.04%, Cu: 0.05%, and the rest is Fe and inevitable trace impurities, with a total mass fraction of 100%.
[0019] Compared with the prior art, the beneficial technical effects of the present invention are:
[0020] (1) The steel of the present invention has the advantage of high strength; (2) The present invention reduces the preparation cost by optimizing the preparation process, replacing the electric furnace with a converter, and improving the cleanliness of the material by degassing and removing inclusions, thereby significantly improving the strength and toughness of the steel and the life of the material. The preparation method is simple in process, low in energy consumption, and is suitable for the preparation technology of the existing industrial equipment level.
[0021] The longitudinal mechanical properties of the 20CrMoA round steel for pumping rod produced by the chemical composition and process of the present invention can reach R m ≥735MPa, R eL ≥930MPa, A≥12.0%, Z≥50%, impact energy KU2≥78J, austenite grain size of steel ≥8 levels, no cracks, scars, folds or inclusions on the steel surface. DETAILED DESCRIPTION
[0022] The 20CrMoA round steel for sucker rod and the production method thereof of the present invention are further described in detail below.
[0023] Example:
[0024] The 20CrMoA round steel for sucker rods of the present embodiment and the production method thereof have the following chemical components in percentage by weight: C 0.17% to 0.24%, Si 0.17% to 0.37%, Mn 0.40% to 0.70%, P≤0.025%, S≤0.020%, Cr 0.80 to 1.10%, Mo 0.15 to 0.25%, Ni≤0.30%, Cu≤0.20%, and the rest are Fe and inevitable trace impurities, with a total mass fraction of 100%.
[0025] The production method of 20CrMoA round steel for pumping rod in this embodiment is: converter smelting, LF refining, VD vacuum degassing, continuous casting, heating in a casting furnace, and round steel rolling.
[0026] Combined blowing converter smelting ensures that the smelting materials are dry to prevent water vapor from entering the steel to produce white spots; [P] < 0.012%, [S] < 0.030%; 4.0 kg of AlMnFe deoxidizer and various high-purity alloys are added per ton for pre-deoxidation and initial adjustment of Si, Mn, Cr, Mo and other components during steel tapping, and slag retention during steel tapping is used to prevent P from returning; 2.5-4 kg of binary synthetic slag is added per ton during steel tapping; slag is blocked during steel tapping, and argon is blown throughout the steel tapping process;
[0027] In the LF furnace, the molten steel is deeply stripped and alloyed, and high basicity slag (R≥3.0) is made to strengthen the removal of sulfur and inclusions. The refining process adopts stirring throughout the whole process;
[0028] After LF refining, use VD circulating degassing equipment to perform vacuum degassing and remove impurities. Maintain it under high vacuum for more than 25 minutes to ensure that [H] ≤ 0.0002%, [O] ≤ 0.0020%, and all components are within the required range;
[0029] Adopt continuous casting machine, use mold protection slag, work casting speed is 1.5-1.8m / min, implement full protection casting to produce continuous casting billet, the billet enters the slow cooling pit, the slow cooling time is ≥24 hours;
[0030] The billet heating temperature is 1080~1120℃, the allowable temperature difference is ≤50℃, the total heating time is controlled to be 2h, the rolling temperature is 1030~1050℃, prevent overheating, overburning and decarburization, and heat up slowly to ensure uniform billet heating temperature and reduce temperature difference;
[0031] Pay attention to the condition of the rolls, steel turning machine, guide plate, roller table and cover plate, and ensure that they are smooth without sharp edges and corners to avoid scratches and dents on the surface of the rolled piece. The specification of the rolled product is φ120mm. The heat treatment system is quenching at 880℃ and tempering at 500℃.
[0032] The 20CrMoA round steel for sucker rods produced by the chemical composition and process flow of the present invention can achieve longitudinal mechanical properties of Rm≥735MPa, ReL≥930MPa, A≥12.0%, Z≥50%, impact energy KU2≥78J, austenite grain size of the steel ≥8 levels, and no cracks, scars, folds or inclusions on the steel surface.
[0033] Table 1 shows the chemical compositions of three embodiments of the present invention, and Tables 2 and 3 further illustrate the present invention.
[0034] Table 1 Chemical composition of various examples of 20CrMoA round steel for sucker rods (mass percentage / %)
[0035] Example C Si Mn P S Cu Cr Ni Mo Example 1 0.19 0.26 0.58 0.012 0.0058 0.04 0.92 0.03 0.20 Example 2 0.23 0.28 0.62 0.014 0.0075 0.03 0.95 0.05 0.23 Example 3 0.20 0.27 0.60 0.013 0.0055 0.05 0.93 0.04 0.21
[0036] Table 2 Mechanical properties of 20CrMoA round steel for sucker rod
[0037]
[0038]
[0039] Table 3 Non-metallic inclusions and austenite grain size of various examples of 20CrMoA round steel for sucker rods
[0040]
[0041] It can be seen from Tables 1-3 that the 20CrMoA round steel for the sucker rod of the present invention has excellent mechanical properties.
[0042] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for producing 20CrMoA round steel for sucker rods, characterized in that: The production method includes: converter smelting, LF refining, VD vacuum degassing, continuous casting, heating in a casting furnace, and round steel rolling; wherein: Combined blowing converter smelting ensures that the smelting materials are dry to prevent water vapor from entering the steel to produce white spots; [P] < 0.012%, [S] < 0.030%; 4.0 kg of AlMnFe deoxidizer and various high-purity alloys are added per ton for pre-deoxidation and initial adjustment of Si, Mn, Cr, and Mo components during steel tapping, and slag retention during steel tapping is used to prevent P from returning; 2.5-4 kg of binary synthetic slag is added per ton during steel tapping; slag is blocked during steel tapping, and argon is blown throughout the steel tapping process; In the LF furnace, the molten steel is deeply stripped and alloyed, and high-basicity slag is made to strengthen the removal of sulfur and inclusions. The refining process adopts stirring throughout the whole process. After LF refining, use VD circulating degassing equipment to perform vacuum degassing and remove impurities. Maintain it under high vacuum for more than 25 minutes to ensure that [H] ≤ 0.0002%, [O] ≤ 0.0020%, and all components are within the required range; Adopt continuous casting machine, use mold protection slag, work casting speed is 1.5-1.8m / min, implement full protection casting to produce continuous casting billet, the billet enters the slow cooling pit, the slow cooling time is ≥24 hours; The billet heating temperature is 1080~1120℃, the allowable temperature difference is ≤50℃, the total heating time is controlled to be 2h, the rolling temperature is 1030~1050℃, prevent overheating, overburning and decarburization, and heat up slowly to ensure uniform billet heating temperature and reduce temperature difference; The heat treatment system is quenching at 880℃ and tempering at 500℃; The mass percentage of the chemical composition of the 20CrMoA round steel includes: C 0.17%-0.24%, Si 0.17%-0.37%, Mn 0.40%-0.70%, P≤0.025%, S≤0.020%, Cr 0.80-1.10%, Mo 0.15-0.25%, Ni≤0.30%, Cu≤0.20%, and the rest is Fe and inevitable trace impurities, with a total mass fraction of 100%.
2. The method for producing 20CrMoA round steel for sucker rod according to claim 1, characterized in that: Pay attention to the condition of the rollers, steel turning machines, guide plates, roller tables and cover plates, and ensure that they are smooth and have no sharp edges to avoid scratches and bumps on the surface of the rolled product.
3. The method for producing 20CrMoA round steel for sucker rod according to claim 1, characterized in that: The specification of the rolled product is φ120mm.
4. The method for producing 20CrMoA round steel for sucker rod according to claim 1, characterized in that: The 20CrMoA round steel for sucker rods produced meets the following requirements: longitudinal mechanical properties Rm≥735MPa, ReL≥930MPa, A≥12.0%, Z≥50%, impact energy KU2≥78J, austenite grain size≥8 levels, and no cracks, scars, folds or inclusions on the steel surface.
5. The method for producing 20CrMoA round steel for sucker rod according to claim 1, characterized in that: The mass percentage of the chemical composition of the 20CrMoA round steel includes: C 0.19%, Si 0.26%, Mn 0.58%, P: 0.012%, S: 0.0058%, Cr 0.92%, Mo 0.20%, Ni: 0.03%, Cu: 0.04%, and the rest is Fe and inevitable trace impurities, with a total mass fraction of 100%.
6. The method for producing 20CrMoA round steel for sucker rod according to claim 1, characterized in that: The mass percentage of the chemical composition of the 20CrMoA round steel includes: C 0.23%, Si 0.28%, Mn 0.62%, P: 0.014%, S: 0.0075%, Cr 0.95%, Mo 0.23%, Ni: 0.05%, Cu: 0.03%, and the rest is Fe and inevitable trace impurities, with a total mass fraction of 100%.
7. The method for producing 20CrMoA round steel for sucker rod according to claim 1, characterized in that: The mass percentage of the chemical composition of the 20CrMoA round steel includes: C 0.20%, Si 0.27%, Mn 0.60%, P: 0.013%, S: 0.0055%, Cr 0.93%, Mo 0.21%, Ni: 0.04%, Cu: 0.05%, and the rest is Fe and inevitable trace impurities, with a total mass fraction of 100%.
Citation Information
Patent Citations
Ultrahigh-strength and high-toughness steel for pumping rod and production process thereof
CN103233172A
High-strength high-toughness steel for valves of oil drilling platforms and technology for manufacturing high-strength high-toughness steel
CN104894487A
Steel for sucker rod, and making method of sucker rod
CN105441816A
20CrMo round steel and production process method
CN114892103A
Production method of high-strength heavy-load H-level sucker rod
CN115044822A