Thermal barrier coating integrated repairing method for improving coating interface bonding
Through laser diffraction beam splitter and atmospheric plasma spraying technology, laser cleaning, remelting and textured repair of thermal barrier coatings is achieved, solving the problem of coating bonding layer failure, and improving the binding force and resistance of the coating Thermal performance reduces maintenance costs.
Patent Information
- Application Number
- CN202411083806.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
After laser cleaning of the thermal barrier coating, the bonding layer fails, resulting in difficult deposition and easy falling off of the coating, affecting the performance and maintenance cost of the turbine blades.
The laser diffraction beam splitter is used to divide the laser into two beams, and the ceramic layer is removed by scanning layer by layer multiple times. Then the two laser beam splitting synchronously perform remelting and texture processing of the bonding layer, optimize the interface structure, and atmospheric plasma Spray the ceramic layer for repair under spraying technology.
The bonding force between the ceramic layer and the bonding layer is improved, the residual stress inside the coating is optimized, the interface toughness and thermal shock resistance are enhanced, the service life of the coating is extended, and the production cost is reduced.
Smart Images

Figure HDA0004984582520000011 
Figure HDA0004984582520000012 
Figure HDA0004984582520000013
Abstract
Description
Technical Field
[0001] The invention belongs to the field of coating surface processing, and in particular relates to a thermal barrier coating integrated repair method for improving coating interface bonding. Background Art
[0002] Thermal barrier coating is a surface protection technology mainly used in hot-end components such as aerospace, energy and power. It is composed of preparing a metal bonding layer on the surface of a high-temperature alloy substrate, and then coating a ceramic layer that can play a heat-insulating role. It has the characteristics of corrosion resistance, high temperature resistance and thermal shock resistance, thereby protecting the substrate from high temperature and oxidation damage and extending the service life of the parts. The widely used ceramic coating is YSZ (7-8wt% Y 2 O 3 Partially stabilized ZrO 2 ), usually produced by atmospheric plasma spraying (APS), electron beam physical vapor deposition (EB-PVD) and plasma spray physical vapor deposition (PS-PVD). The metal bonding layer generally uses MCrAlY (M is Ni, Co or Ni+Co) as the material to improve the bonding force between the ceramic coating and the substrate, and has excellent anti-oxidation and corrosion properties.
[0003] Atmospheric plasma spraying is widely used in the preparation of ceramic insulation layers and bonding layers in thermal barrier coatings due to its flexible process, convenient operation and low preparation cost. In addition, the plasma spraying process also has many advantages such as small substrate size effect, wide range of coating material selection and high coating preparation efficiency. As a core technical means for preparing wear-resistant, corrosion-resistant and thermal protective coatings, the plasma spraying process is widely used in oil and gas storage and transportation, aviation flight, aerospace engineering and military industry, especially high heat load parts in the aviation field.
[0004] However, due to the long-term service of the engine's turbine blades in harsh environments such as high temperature and high pressure, the thermal barrier coating will gradually fail due to erosion and foreign object damage, sintering reaction and oxidation reaction, as well as molten salt corrosion and CMAS corrosion, which seriously affect the performance of the turbine blades. As a key component of an aircraft engine, the turbine blades have a complex structure, high precision, complex and difficult processes, and a low part qualification rate. Repairing the engine by replacing new parts will result in problems such as high cost, long production cycle, and high production pressure. If the coating of the failed blade is removed and re-coated so that it can be used again, the production cycle can be greatly shortened and manufacturing costs can be reduced.
[0005] Among them, laser cleaning is an emerging technology that is precisely controllable. Compared with traditional cleaning technologies, laser cleaning can achieve substrate-free and efficient cleaning of failed thermal barrier coatings by adjusting parameters such as laser power, scanning speed, and pulse frequency. Then, a new coating is applied through plasma spraying technology to complete the repair of the coating. However, laser cleaning is difficult to completely remove ceramic materials from the surface of the bonding layer, and particles will splash during the cleaning process, causing some residual ceramic materials to adhere to the surface of the bonding layer. If a ceramic layer is sprayed directly on the surface for repair, it is easy to cause problems such as the coating failing to effectively bond or even falling off.
[0006] Laser remelting uses a laser beam to melt the surface without adding any metal elements to achieve the purpose of improving the surface structure. Its main features are as follows:
[0007] (1) Generally, no alloying elements are added during surface melting, and the molten layer and the material matrix form a natural metallurgical bond.
[0008] (2) During the laser melting process, impurities and gases can be removed, and the structure obtained by rapid cooling and recrystallization has higher hardness, wear resistance and corrosion resistance.
[0009] (3) Its molten layer is thin and the heat action zone is small, which has little effect on the surface roughness and workpiece size and can even be used directly.
[0010] In order to improve the mechanical bonding between coatings, sandblasting technology is often used in industry. However, sandblasting technology has disadvantages such as residual particles, easy crack formation, and poor uniformity, which need to be improved urgently. Surface texture can produce a strong mechanical anchoring effect between coatings and improve the adhesion of surface coatings. Summary of the invention
[0011] In view of the current problems that after laser cleaning of thermal barrier coatings, the bonding layer fails, resulting in the coating being difficult to deposit and easy to fall off during repair, the present invention provides an integrated repair method for thermal barrier coatings that improves the coating interface bonding.
[0012] The method realizes laser cleaning, surface remelting, and integrated microtexture repair of the thermal barrier coating, can enhance the bonding force between the ceramic layer and the bonding layer, optimize the residual stress inside the coating, and improve the interface toughness. The present invention optimizes the performance of the bonding layer and prolongs the service life of the coating.
[0013] The technical solution of the present invention is as follows:
[0014] A method for integrated repair of thermal barrier coatings for improving coating interface bonding comprises the following steps:
[0015] Step 1: Clean and dry the surface of the thermal barrier coating workpiece to be repaired;
[0016] Specifically, the thermal barrier coating workpiece to be repaired is placed in 95-99.9% ethanol, ultrasonically cleaned for 10-15 minutes to remove impurities on the coating surface, and then dried in an environment of 60-70° C. to complete the pretreatment;
[0017] Step 2: Place the workpiece to be processed on the workbench, and use a laser diffraction beam splitter to split the laser into two beams. First, use one laser beam splitter to scan layer by layer multiple times for laser cleaning to remove the ceramic layer of the original thermal barrier coating. Then, the two laser beam splitters act synchronously on the surface of the bonding layer of the original thermal barrier coating to achieve laser texturing after laser remelting of the bonding layer.
[0018] The parameters of laser cleaning are set as follows: laser power 120-200W, repetition frequency 30-50kHz, laser scanning speed 400-800mm / s, spot overlap rate 80-99%, laser spot size 115μm, so that the light beam is incident vertically on the coating surface, and the laser scans the coating surface layer by layer for multiple times until the ceramic layer is removed;
[0019] When two laser split beams act synchronously on the bonding layer surface of the original thermal barrier coating, in the scanning direction, the laser split beam used for remelting is in front, and the laser split beam used for texturing is in the back, and the center distance between the two laser split beam focuses is preferably 5 mm;
[0020] The laser beam splitting parameters used for remelting were set as follows: laser power 80-120 W, repetition frequency 30-50 kHz, laser scanning speed 400-800 mm / s, spot overlap rate 80-99%, and laser spot size 85 μm;
[0021] The laser beam splitting parameters used for texturing were set as follows: laser power 30-80 W, repetition frequency 30-50 kHz, laser scanning speed 400-800 mm / s, spot overlap rate 80-99%, and laser spot size 60 μm;
[0022] The laser beam splitting for remelting first acts on the surface of the bonding layer to achieve remelting of the surface of the bonding layer, and then the laser beam splitting for texturing quickly processes a texture array on the surface of the remelting layer. The preferred texture array is: a circular hole array with a diameter of 115 to 230 μm, a center distance between adjacent circular holes of 115 to 230 μm, and a depth of 1 to 50 μm;
[0023] Step 3: spraying a ceramic layer on the surface of the bonding layer textured in step 2 by atmospheric plasma spraying to complete the repair of the thermal barrier coating;
[0024] The process parameters of atmospheric plasma spraying are: power 15-35kW, spraying distance 80-200mm, scanning speed 50-200mm / s, plasma spray gun powder feeding rate 10-50g / min, main gas argon flow rate 20-60L / min, secondary gas hydrogen flow rate 1-10L / min.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention provides an integrated repair method for thermal barrier coatings that improves the interface bonding of coatings. A laser diffraction beam splitter is used to split the laser on a device into two beams. By controlling the relative position of the focus and the action time of the two laser beams, multiple processing processes can be carried out simultaneously. First, a laser beam splitter is used to scan layer by layer multiple times to achieve the removal of the ceramic layer; then the two laser beam splitters act synchronously to achieve rapid texturing after remelting the bonding layer; finally, the atmospheric plasma spraying technology is used to spray the ceramic layer on the surface of the bonding layer to achieve high-performance repair of the coating.
[0027] Laser remelting technology can improve the density of the bonding layer and effectively heal the cracks, while the impact brought by laser microtexturing technology can optimize the residual stress inside the coating, improve the interface toughness, and inhibit the generation and expansion of coating cracks. At the same time, it also increases the contact area between the bonding layer and the ceramic layer, effectively improving the deposition quality and interface bonding strength of the YSZ ceramic surface layer repaired by the atmospheric plasma spraying method, and making the coating have higher thermal shock resistance. In addition, the laser remelting technology has a small thermal action zone on the coating, and has little effect on the surface roughness and workpiece size. The laser remelting process makes the coating structure dense, reduces or eliminates defects such as pores in the original sprayed coating, and improves the coating microstructure.
[0028] The present invention creatively realizes the simultaneous laser cleaning, laser remelting, and ultrafast laser texturing on the same device, which greatly improves the processing efficiency, reduces the production cost, provides certain technical support for the field of coating repair, and helps to improve the high-temperature service life of gas turbine blades. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 : Cross-sectional microstructure of the ceramic layer after laser cleaning.
[0030] Figure 2 : Cross-sectional microstructure of failed coating repair.
[0031] Figure 3 : Schematic diagram of micro-woven circular hole array on the coating surface.
[0032] Figure 4 : Cross-sectional microstructure after coating repair. DETAILED DESCRIPTION
[0033] The implementation scheme of the present invention will be described in detail below in conjunction with embodiments, and the following embodiments are only used to illustrate the present invention.
[0034] Example 1
[0035] (1) The YSZ thermal barrier coating workpiece to be repaired was placed in 95% pure anhydrous ethanol, and ultrasonic cleaning was performed for 15 min to remove impurities on the coating surface. The workpiece was then dried at 60-70°C until the anhydrous ethanol was completely evaporated.
[0036] (2) Place the workpiece to be processed on the workbench and set the laser parameters: laser power of 180W, repetition frequency of 50kHz, laser scanning speed of 600mm / s, spot overlap rate of 90%, laser spot size of 115μm, make the light beam incident vertically on the surface of the coating material, and let the laser scan the coating surface layer by layer many times until the ceramic layer is removed. The microstructure morphology of the cross section of the cleaned coating is as follows: Figure 1 As shown in the figure, it can be found that some ceramic material still remains on the surface of the bonding layer. If the ceramic layer is sprayed directly on the surface, it may cause problems such as coating shedding or bonding failure. Figure 2 shown.
[0037] (3) Setting laser parameters: the laser beam splitting parameters for remelting are: laser power 80 W, repetition frequency 50 kHz, laser scanning speed 600 mm / s, spot overlap rate 90%, laser spot size 85 μm; the laser beam splitting parameters for texturing are: laser power 35 W, repetition frequency 50 kHz, laser scanning speed 500 mm / s, spot overlap rate 80%, laser spot size 60 μm. The center distance between the two laser beam splitting focal points is 5 mm.
[0038] (4) The laser beam splitting used for remelting first acts on the surface of the bonding layer material to achieve remelting of the bonding layer surface, and then the laser beam splitting used for texturing quickly processes a circular hole-shaped texture array on the surface of the remelting layer, such as Figure 3 As shown, the obtained texture is: a circular hole array with a diameter of 115 μm, a center distance between adjacent circular holes of 230 μm, and a depth of 20 μm.
[0039] (5) Using atmospheric plasma spraying to spray a ceramic layer on the surface of the bonding layer, finally obtaining a repaired thermal barrier coating, such as Figure 4 As shown, the atmospheric plasma spraying process parameters are: power of 35kW, spraying distance of 110mm, scanning speed of 50mm / s, plasma spray gun powder feeding rate of 35g / min, main gas argon flow rate of 50L / min, and secondary gas hydrogen flow rate of 5L / min.
[0040] In this embodiment, the original ceramic layer is 300 μm thick, which can be basically removed by laser cleaning, but a small amount of ceramic material still remains on the surface of the bonding layer. After laser remelting, it can be observed that the ceramic material remaining on the surface of the bonding layer has disappeared. During the laser melting process, some impurities and gases are removed, and the pores and unmelted particles in the coating are reduced. The hardness and corrosion resistance of the obtained bonding layer are improved to a certain extent. After micro-texturing the surface of the remelted layer, atmospheric plasma spraying is used to repair the ceramic layer. Through a metallographic microscope, it can be observed that the coating is tightly bonded and the size has not changed significantly compared to before. By tensile testing the coating, it can be found that the tensile mechanical properties of the coating obtained by this repair process are 25% higher than those of the coating obtained by direct spray repair.
[0041] Example 2
[0042] (1) The YSZ thermal barrier coating workpiece to be repaired was placed in 95% pure anhydrous ethanol, and ultrasonic cleaning was performed for 15 min to remove impurities on the coating surface. The workpiece was then dried at 60-70°C until the anhydrous ethanol was completely evaporated.
[0043] (2) Place the workpiece to be processed on the workbench and set the laser parameters: laser power of 180W, repetition frequency of 50kHz, laser scanning speed of 600mm / s, spot overlap rate of 90%, laser spot size of 115μm, make the light beam incident vertically on the surface of the coating material, and let the laser scan the coating surface layer by layer many times until the ceramic layer is removed. The microstructure morphology of the cross section of the cleaned coating is as follows: Figure 1 As shown in the figure, it can be found that some ceramic material still remains on the surface of the bonding layer. If the ceramic layer is sprayed directly on the surface, it may cause problems such as coating shedding or bonding failure. Figure 2 shown.
[0044] (3) Setting laser parameters: the laser beam splitting parameters for remelting are: laser power 120 W, repetition frequency 50 kHz, laser scanning speed 500 mm / s, spot overlap rate 90%, laser spot size 85 μm; the laser beam splitting parameters for texturing are: laser power 35 W, repetition frequency 50 kHz, laser scanning speed 500 mm / s, spot overlap rate 80%, laser spot size 60 μm. The center distance between the two laser beam splitting foci is 5 mm.
[0045] (4) The laser beam splitting used for remelting first acts on the surface of the bonding layer material to achieve remelting of the bonding layer surface, and then the laser beam splitting used for texturing quickly processes a circular hole-shaped texture array on the surface of the remelting layer, such as Figure 3 As shown, the obtained texture is: a circular hole array with a diameter of 115 μm, a center distance between adjacent circular holes of 230 μm, and a depth of 20 μm.
[0046] (5) A ceramic layer was sprayed on the surface of the bonding layer by atmospheric plasma spraying to finally obtain a repaired thermal barrier coating. The atmospheric plasma spraying process parameters were as follows: power of 35 kW, spraying distance of 110 mm, scanning speed of 50 mm / s, powder feeding rate of the plasma spray gun of 35 g / min, main gas argon flow rate of 50 L / min, and secondary gas hydrogen flow rate of 5 L / min.
[0047] The process parameters and methods of laser cleaning, remelting layer texturing, and atmospheric plasma spraying in this embodiment are the same as those in Example 1. The difference is that the process parameters of laser remelting are adjusted. By performing a tensile test on the coating, it can be found that the mechanical resistance of the coating obtained by this repair process is improved by 33% compared with the coating obtained by direct spray repair.
[0048] Example 3
[0049] (1) The YSZ thermal barrier coating workpiece to be repaired was placed in 95% pure anhydrous ethanol, and ultrasonic cleaning was performed for 15 min to remove impurities on the coating surface. The workpiece was then dried at 60-70°C until the anhydrous ethanol was completely evaporated.
[0050] (2) Place the workpiece to be processed on the workbench and set the laser parameters: laser power of 180W, repetition frequency of 50kHz, laser scanning speed of 600mm / s, spot overlap rate of 90%, laser spot size of 115μm, make the light beam incident vertically on the surface of the coating material, and let the laser scan the coating surface layer by layer many times until the ceramic layer is removed. The microstructure morphology of the cross section of the cleaned coating is as follows: Figure 1 As shown in the figure, it can be found that some ceramic material still remains on the surface of the bonding layer. If the ceramic layer is sprayed directly on the surface, it may cause problems such as coating shedding or bonding failure. Figure 2 shown.
[0051] (3) Setting laser parameters: the laser beam splitting parameters for remelting are: laser power 80 W, repetition frequency 50 kHz, laser scanning speed 600 mm / s, spot overlap rate 90%, laser spot size 85 μm; the laser beam splitting parameters for texturing are: laser power 55 W, repetition frequency 50 kHz, laser scanning speed 400 mm / s, spot overlap rate 80%, laser spot size 60 μm. The center distance between the two laser beam splitting foci is 5 mm.
[0052] (4) The laser beam splitting used for remelting first acts on the surface of the bonding layer material to achieve remelting of the bonding layer surface, and then the laser beam splitting used for texturing quickly processes a circular hole-shaped texture array on the surface of the remelting layer, such as Figure 3As shown, the obtained texture is: a circular hole array with a diameter of 115 μm, a center distance between adjacent circular holes of 230 μm, and a depth of 30 μm.
[0053] (5) A ceramic layer was sprayed on the surface of the bonding layer by atmospheric plasma spraying to finally obtain a repaired thermal barrier coating. The atmospheric plasma spraying process parameters were as follows: power of 35 kW, spraying distance of 110 mm, scanning speed of 50 mm / s, powder feeding rate of the plasma spray gun of 35 g / min, main gas argon flow rate of 50 L / min, and secondary gas hydrogen flow rate of 5 L / min.
[0054] The process parameters and methods of laser cleaning, laser remelting, and atmospheric plasma spraying in this embodiment are the same as those in Example 1. The difference is that the process parameters of laser texturing are adjusted and the depth of the circular hole groove is changed. By performing a tensile test on the coating, it can be found that the tensile mechanical properties of the coating obtained by this repair process are improved by 42% compared with the coating obtained by direct spray repair.
[0055] Matters not covered in the present invention are known technologies. The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for integrated repair of thermal barrier coatings to improve coating interface bonding, characterized in that: The steps include: Step 1: Clean and dry the surface of the thermal barrier coating workpiece to be repaired; Step 2: Place the workpiece to be processed on the workbench, and use a laser diffraction beam splitter to split the laser into two beams. First, use one laser beam splitter to scan layer by layer for multiple times for laser cleaning to remove the ceramic layer of the original thermal barrier coating. Then, the two laser beam splitters act synchronously on the surface of the bonding layer of the original thermal barrier coating. In the scanning direction, the laser beam splitter used for remelting is in front, and the laser beam splitter used for texturing is in the back, so as to realize the laser texturing treatment after laser remelting of the bonding layer. Step 3: Use atmospheric plasma spraying to spray a ceramic layer on the surface of the bonding layer textured in step 2 to complete the repair of the thermal barrier coating.
2. The integrated repair method for thermal barrier coatings for improving coating interface bonding according to claim 1, characterized in that: In step 1, the thermal barrier coating workpiece to be repaired is placed in 95-99.9% ethanol, ultrasonically cleaned for 10-15 minutes to remove impurities on the coating surface, and then dried in an environment of 60-70° C. to complete the pretreatment.
3. The integrated repair method for thermal barrier coatings for improving coating interface bonding according to claim 1, characterized in that: In step 2, the laser cleaning parameters are set as follows: laser power 120-200W, repetition frequency 30-50kHz, laser scanning speed 400-800mm / s, spot overlap rate 80-99%, laser spot size 115μm, so that the light beam is incident vertically on the coating surface, and the laser scans the coating surface layer by layer multiple times until the ceramic layer is removed.
4. The integrated repair method for thermal barrier coatings for improving coating interface bonding according to claim 1, characterized in that: In step 2, when the two laser split beams act synchronously on the bonding layer surface of the original thermal barrier coating, the center distance between the two laser split beam focuses is 5 mm.
5. The integrated repair method for thermal barrier coatings for improving coating interface bonding according to claim 1, characterized in that: In step 2, the laser beam splitting parameters for remelting are set as follows: laser power 80-120 W, repetition frequency 30-50 kHz, laser scanning speed 400-800 mm / s, spot overlap rate 80-99%, and laser spot size 85 μm.
6. The integrated repair method for thermal barrier coatings for improving coating interface bonding according to claim 1, characterized in that: In step 2, the laser beam splitting parameters used for texturing are set as follows: laser power 30-80 W, repetition frequency 30-50 kHz, laser scanning speed 400-800 mm / s, spot overlap rate 80-99%, and laser spot size 60 μm.
7. The integrated repair method for thermal barrier coatings for improving coating interface bonding according to claim 1, characterized in that: In step 2, laser texturing is performed to obtain a texture array, wherein the texture array is a circular hole array with a diameter of 115 to 230 μm, a center distance between adjacent circular holes of 115 to 230 μm, and a depth of 1 to 50 μm.
8. The integrated repair method for thermal barrier coatings for improving coating interface bonding according to claim 1, characterized in that: In step three, the atmospheric plasma spraying process parameters are: power 15-35kW, spraying distance 80-200mm, scanning speed 50-200mm / s, plasma spray gun powder feeding rate 10-50g / min, main gas argon flow rate 20-60L / min, secondary gas hydrogen flow rate 1-10L / min.
Citation Information
Cited By
Method for multi-system laser cleaning and texturing of magnesium alloy matrix surface
CN119456576A