Preparation method and application of AlN film for cavity surface of semiconductor laser
The preparation of AlN films under low temperature conditions through electron cyclonic resonance ion coating technology has solved the problem of AlN film preparation in the prior art, and achieved laser cavity surface coating with high chemical stability and high working current, which has improved the performance stability of semiconductor lasers .
Patent Information
- Application Number
- CN202410919544.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-22
AI Technical Summary
It is difficult to prepare high-quality AlN films under low temperature conditions for use in the cavity surface of semiconductor lasers, and common deposition methods such as MOCVD and magnetron reactive sputtering have the problem of low nitrogen content, which affects the performance stability of the laser.
Electron cyclonic resonance ion coating (ECR) technology is used to coat AlN films at low temperature, low pressure and low damage, and combine microwave sources and plasma gas for cleaning and deposition to form excellent AlN film.
The prepared AlN film has high chemical stability, can effectively prevent cavity surface oxidation, improve the stability and reliability of the laser, and does not fall off in high temperature and high humidity environments, significantly increasing the working current.
Smart Images

Figure CN118996329A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of an AlN film for a semiconductor laser cavity surface, belonging to the technical field of semiconductor laser cavity surface coating. Background Art
[0002] High-quality optical films on the cavity surface can prevent cavity surface oxidation, protect cavity surface, and increase the reliability of lasers. Therefore, laser cavity surface coating is crucial to improving the performance of semiconductor lasers, especially aluminum-containing GaAs / AlGaAs lasers. The aluminum element absorbs water vapor and oxygen, which can easily cause end face oxidation to form local defects, affecting the surface's absorption of light, leading to local heat generation, and causing laser performance degradation or even failure.
[0003] Conventional laser cavity films are mostly Al2O3. The oxygen in the film can migrate to the laser light output area and oxidize the semiconductor laser cavity surface without direct contact with the atmosphere. Therefore, in order to avoid cavity surface oxidation, an oxygen-free optical film material should be selected. AlN materials can be used in high-temperature and high-power optoelectronic devices due to their high melting point and thermal conductivity. At present, AlN is mostly used for epitaxial material buffer layers, so the common AlN film is grown by metal organic chemical vapor deposition (MOCVD). The formed film has high purity and good density, but due to the high substrate temperature, it is not suitable for semiconductor laser cavity surface coating. In addition to chemical vapor deposition (MOCVD) growth, magnetron reactive sputtering is also the most widely used deposition method, but the nitrogen content of the prepared AlN film is low. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a method for preparing AlN thin films on the cavity surface of semiconductor lasers, which uses electron cyclotron resonance ion plating equipment (ECR) to generate high-activity, high-density, low-energy auxiliary plating ion beams under low temperature, low pressure and low damage conditions, and has the characteristics of non-polar discharge and concentrated discharge area. The prepared insulating AlN thin film is particularly suitable for the cavity surface coating of semiconductor lasers of GaAs, AlGaAs, and AlGaInP systems, which require low film growth temperature and good density.
[0005] The technical solution of the present invention is as follows:
[0006] A method for preparing an AlN film on a semiconductor laser cavity surface comprises the following steps:
[0007] 1) Use a scriber to cleave the 808nm GaAs / AlGaAs semiconductor laser chip into bars of the required cavity length, and place the cleaved bars into a special fixture to expose the resonant cavity surface;
[0008] 2) Clean the coating chamber of the ECR coating equipment in advance to ensure that the chamber is clean and tidy, and put in the GaAs material of the coating laser and epitaxial material system as a companion piece;
[0009] 3) Place the specific bar fixture into the ECR transfer chamber, start the coating process, and immediately evacuate the chamber. When the vacuum reaches 3.0 to 10×10-5 Torr, the robotic arm moves the bar fixture in the transfer chamber into the coating chamber, and the robotic arm is retracted;
[0010] 4) After the fixture carrying the bar enters the coating chamber, the front cavity surface is first cleaned at room temperature using ions. During cleaning, the RF source on the target is turned off, the 2.45GHz microwave source is turned on, the microwave source power is set, and plasma gas is introduced. This process condition is used to remove unstable oxides on the laser cavity surface, increase the activity of the front cavity surface of the coating, and provide an excellent attachment for the attachment of the anti-reflection film, and then clean it;
[0011] 5) After the ion source cleans the cavity surface, the heating is not turned on and the AlN film is evaporated. Before coating, pre-coating is first performed. During pre-coating, the coating shield is closed, the RF source on the Al target is turned on, and N2 gas is introduced for pre-reaction; the coating shield is turned on and the AlN film is coated;
[0012] 6) After the front cavity surface is coated, the cavity surface is turned over to deposit on the back cavity surface. Like the front cavity surface, the light-emitting cavity surface is first cleaned with ions. During cleaning, the RF source on the target is turned off, the 2.45 GHz microwave source is turned on, the microwave source power is set, and plasma gas is introduced. This process condition is used to remove unstable oxides on the laser cavity surface, increase the activity of the cavity surface before coating, and provide an excellent attachment for the attachment of the anti-reflection film, and then clean it;
[0013] 7) Performing ion source assisted high reflective film evaporation, the high reflective film layer is AlN+(SiO2 / Si)^6, or AlN+(Al2O3 / TiO2)^6, or AlN+(Al2O3 / Si)^6, or AlN+(SiO2 / Ta2O5)^6;
[0014] 8) After the high-reflective film is evaporated, the coated bars are taken out and the laser bars are divided into individual laser chips using a fully automatic dicing machine and a chip splitting machine;
[0015] 9) Use a fully automatic die bonding machine to mount the cleaved laser chip on a gold-tin heat sink to form a COS assembly, mount the COS assembly on a TO tube, use an automatic wire bonding machine to complete the electrical connection of the laser, use a fully automatic capping machine to cap, and finally package the laser into a TO5.6 sample.
[0016] The AlN film plated by the present invention has a smooth surface and uniform film thickness. When the packaged laser is placed in an environment of 85° C. high temperature and 85% high humidity for 200 hours, the film layer does not fall off, which greatly improves the working current.
[0017] Preferably, in step 1), the semiconductor laser is GaAs or AlGaAs or GaN or other III-V compounds containing Ga.
[0018] Preferably, in step 4), the microwave source power is set to 200-400 W, 8-20 sccm of plasma gas is introduced, and cleaning is performed for 5-10 minutes.
[0019] Preferably, in step 6), the microwave source power is set to 200-400 W, 8-20 sccm of plasma gas is introduced, and cleaning is performed for 5-10 minutes.
[0020] Further preferably, in step 4) and step 6), the microwave source power is set to 300 W, 10 sccm of plasma gas is introduced, and cleaning is performed for 10 minutes.
[0021] Further preferably, in step 4) and step 6), the plasma gas is a non-oxide, selected from N2, Ar, H2, NH3, and methane.
[0022] Preferably, in step 5), the RF power of the RF source is 300-500W, the microwave power is 400-600W, 20-40sccmAr and 3-5sccmN2 gas are introduced, and the pre-reaction is 2-4min; the thickness of the AlN film is 181nm, and the coating rate is about 3nm / min.
[0023] Further preferably, in step 5), the RF power of the RF source is 400 W, the microwave power is 500 W, 30 sccm Ar and 4 sccm N2 gases are introduced, and the pre-reaction is carried out for 3 minutes.
[0024] Preferably, in step 7), when the high reflective film layer is AlN+(SiO2 / Si)^6, the thickness is 20nm+(138nm / 59nm)^6; when the high reflective film layer is AlN+(Al2O3 / TiO2)^6, the thickness is 20nm+(124nm / 93nm)^6; when the high reflective film layer is AlN+(Al2O3 / Si)^6, the thickness is 20nm+(124nm / 59nm)^6; when the high reflective film layer is AlN+(SiO2 / Ta2O5)^6), the thickness is 20nm+(138nm / 99nm)^6.
[0025] Preferably, in step 7), a layer of AlN coating method is the same as described above, as follows: firstly, pre-coating is performed, during which the coating shield is closed, the RF source on the Al target is turned on, the RF power is 400W, the microwave power is 500W, and 30sccmAr and 4sccmN2 gases are introduced, pre-react for 3min, the coating shield is turned on, and AlN thin film is coated at a coating rate of about 3nm / min. After AlN coating, the Al target shield is closed;
[0026] Turn on the RF source on the Si target with an RF power of 600W, and introduce 30sccm of Ar gas and 6.8sccm of O2, set the microwave power to 500W, and the coating rate to 7.5nm / min; after SiO2 coating, coat the Si thin film according to the film system design structure, using 600W of RF power, 30sccm of Ar, and 500W of microwave power for coating, with a Si film deposition rate of 4nm / min; then evaporate SiO2 and Si in turn according to the film system design, and a total of 6 pairs of SiO2 / Si thin films with high and low refractive index materials are evaporated.
[0027] The heating power source is not turned on during the film coating process, and the film coating is carried out at a low temperature throughout the process.
[0028] The laser prepared by the above preparation method has a cavity surface coated with an AlN film.
[0029] The beneficial effects of the present invention are:
[0030] 1) The present invention provides a method for preparing an AlN film as a laser cavity mask. The prepared AlN film has excellent chemical stability and can effectively prevent the active area material in contact with it from undergoing oxidation reaction in an oxidizing environment, which is of great significance for improving the stability and reliability of the device.
[0031] 2) This method has the advantages of flexible preparation process, excellent film performance and broad application prospects, and is expected to provide strong support for the development of microelectronics, optoelectronics, optics and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a flow chart of the present invention;
[0033] Figure 2 This is a current-power curve diagram of the solution of the present invention;
[0034] Figure 3 This is the current-power curve of the comparison scheme. DETAILED DESCRIPTION
[0035] The present invention will be further described below by way of embodiments in conjunction with the accompanying drawings, but is not limited thereto.
[0036] Embodiment 1:
[0037] A method for preparing an AlN film on a semiconductor laser cavity surface comprises the following steps:
[0038] 1) Use a scriber to cleave the 808nm GaAs / AlGaAs semiconductor laser chip into bars of the required cavity length, and place the cleaved bars into a special fixture to expose the resonant cavity surface; the semiconductor laser can also be GaN or other Ga-containing III-V compounds.
[0039] 2) Clean the coating chamber of the ECR coating equipment in advance to ensure that the chamber is clean and tidy, and put in the GaAs material of the coating laser and epitaxial material system as a companion piece.
[0040] 3) Place the specific bar fixture into the ECR transfer chamber, start the coating process, and immediately evacuate the chamber. When the vacuum degree reaches 3.0~10×10-5Torr, the robotic arm will move the bar fixture in the transfer chamber into the coating chamber, and the robotic arm will be retracted.
[0041] 4) After the fixture carrying the bar enters the coating chamber, the front cavity surface is first cleaned at room temperature using ions. During cleaning, the RF source on the target is turned off, the 2.45 GHz microwave source is turned on, the microwave source power is set to 300 W, and 10 sccm of plasma gas N2 is introduced. This process condition is used to remove unstable oxides on the laser cavity surface, increase the activity of the coating front cavity surface, and provide an excellent attachment for the attachment of the anti-reflection film. The cleaning is carried out for 10 minutes.
[0042] 5) After the ion source cleans the cavity surface, the heating is not turned on, and the AlN film is evaporated. Pre-coating is first performed before coating. During pre-coating, the coating shield is closed, and the RF source on the Al target is turned on. The RF power of the RF source is 400W, the microwave power is 500W, and 30sccmAr and 4sccmN2 gas are introduced for pre-reaction for 3min; the coating shield is turned on to coat the AlN film. The thickness of the AlN film is 181nm, and the coating rate is about 3nm / min.
[0043] 6) After the front cavity surface is coated, the cavity surface is turned over to deposit on the back cavity surface. Like the front cavity surface, the light-emitting cavity surface is first cleaned with ions. During cleaning, the RF source on the target is turned off, and the 2.45GHz microwave source is turned on. The microwave source power is set to 300W, and 10sccm of plasma gas N2 is introduced. This process condition is used to remove unstable oxides on the laser cavity surface, increase the activity of the cavity surface before coating, and provide an excellent attachment for the attachment of the anti-reflection film. Cleaning is carried out for 10 minutes.
[0044] 7) Carry out ion source assisted high reflective film evaporation, the high reflective film layer is AlN+(SiO2 / Si)^6, and the thickness is 20nm+(138nm / 59nm)^6; the method for coating a layer of AlN is the same as the above description, as follows: firstly, pre-coating is carried out, the coating shield is closed during pre-coating, the RF source on the Al target is turned on, the RF power is 400W, the microwave power is 500W, and 30sccmAr and 4sccmN2 gases are introduced, the pre-reaction is 3min, the coating shield is opened, and the AlN thin film is coated at a coating rate of about 3nm / min. After AlN coating, the Al target shield is closed.
[0045] Turn on the RF source on the Si target with an RF power of 600W, and introduce 30sccm of Ar gas and 6.8sccm of O2, set the microwave power to 500W, and the coating rate to 7.5nm / min; after SiO2 coating, coat the Si thin film according to the film system design structure, using 600W of RF power, 30sccm of Ar, and 500W of microwave power for coating, with a Si film deposition rate of 4nm / min; then evaporate SiO2 and Si in turn according to the film system design, and a total of 6 pairs of SiO2 / Si thin films with high and low refractive index materials are evaporated.
[0046] The heating power source is not turned on during the film coating process, and the film coating is carried out at a low temperature throughout the process.
[0047] 8) After the high-reflective film is evaporated, the coated bars are taken out and the laser bars are divided into individual laser chips using a fully automatic dicing machine and a chip splitting machine;
[0048] 9) Use a fully automatic die bonding machine to mount the cleaved laser chip on a gold-tin heat sink to form a COS assembly, mount the COS assembly on a TO tube, use an automatic wire bonding machine to complete the electrical connection of the laser, use a fully automatic capping machine to cap, and finally package the laser into a TO5.6 sample.
[0049] The AlN film plated by the present invention has a smooth surface and uniform film thickness. The packaged laser is placed in an environment of 85°C high temperature and 85% high humidity for 200 hours, and the film layer does not fall off. The maximum working current is 1600mA when tested with a working current of 2000mA.
[0050] Compared with the comparative example 1, the maximum operating current is increased by 290mA. Figure 2 , Figure 3 .
[0051] Example 2
[0052] A method for preparing an AlN film on the cavity surface of a semiconductor laser, wherein the steps are as described in Example 1, except that in steps 4) and 6), the microwave source power is set to 200W, 8sccm of plasma gas is introduced, and cleaning is performed for 5 minutes. In steps 4) and 6), the plasma gas is Ar or H2. In step 5), the RF source has a RF power of 300W and a microwave power of 400W, 20sccmAr and 3sccm N2 gases are introduced, and pre-reaction is performed for 2 minutes. In step 7), the high-reflective film layer is AlN+(Al2O3 / TiO2)^6, and the thickness is 20nm+(124nm / 93nm)^6.
[0053] Example 3
[0054] A method for preparing an AlN film on the cavity surface of a semiconductor laser, wherein the steps are as described in Example 1, except that in steps 4) and 6), the microwave source power is set to 400W, 20sccm of plasma gas is introduced, and cleaning is performed for 10 minutes. In steps 4) and 6), the plasma gas is NH3 or methane. In step 5), the RF source has a RF power of 500W and a microwave power of 600W, 40sccmAr and 5sccm N2 gases are introduced, and pre-reaction is performed for 4 minutes. In step 7), the high-reflective film layer is AlN+(Al2O3 / Si)^6, and the thickness is 20nm+(124nm / 59nm)^6.
[0055] Example 4
[0056] A method for preparing an AlN film on the cavity surface of a semiconductor laser, wherein the steps are as described in Example 1, except that in step 7), the high reflective film layer is AlN+(SiO2 / Ta2O5)^6, and the thickness is 20nm+(138nm / 99nm)^6.
[0057] Comparative Example 1
[0058] The process of preparing a semiconductor laser cavity facet comprises the following steps:
[0059] 1) Use a scriber to cleave the 808nm GaAs / AlGaAs semiconductor laser chip into bars of the required cavity length, and place the cleaved bars into a special fixture to expose the resonant cavity surface.
[0060] 2) Clean the coating chamber of the ECR coating equipment in advance to ensure that the chamber is clean and tidy, and put in the GaAs material of the coating laser and epitaxial material system as a companion piece.
[0061] 3) Place the specific bar fixture into the ECR transfer chamber, start the coating process, and immediately evacuate the chamber. When the vacuum degree reaches 3.0~10×10-5Torr, the robotic arm will move the bar fixture in the transfer chamber into the coating chamber, and the robotic arm will be retracted.
[0062] 4) Carry out front cavity surface coating, and pre-coating is first carried out before coating. During pre-coating, the coating shield is closed, the RF source on the Al target is turned on, and O2 gas is introduced for pre-reaction; the coating shield is opened, and Al2O3 thin film is coated, specifically, the RF source on the Si target is turned on, the RF power is 600W, and 20sccm of Ar gas and 4.5sccm of O2 are introduced, the microwave power is set to 500W, and the coating rate is 6.5nm / min.
[0063] 5) After the front cavity surface is coated, the cavity surface is turned over to perform ion source assisted high-reflective film evaporation. The high-reflective film layer is (SiO2 / Si)^6 with a thickness of (138nm / 59nm)^6. Specifically, the RF source on the Si target is turned on with an RF power of 600W, and 30sccm of Ar gas and 6.8sccm of O2 are introduced. The microwave power is set to 500W, and the coating rate is 7.5nm / min. After SiO2 coating, Si thin film is plated according to the film system design structure. During coating, 600W of RF power, 30sccm of Ar, and 500W of microwave power are used, and the Si film deposition rate is 4nm / min. Then SiO2 and Si are sequentially evaporated according to the film system design, and a total of 6 pairs of SiO2 / Si thin films with high and low refractive index materials are evaporated.
[0064] 6) The high reflective film can also be (Al2O3 / TiO2)^6, or (Al2O3 / Si)^6, or (SiO2 / Ta2O5)^6; and the Moshi structure used can also be (Al2O3 / TiO2)^6=(124nm / 93nm)^6, or (Al2O3 / Si)^6=(124nm / 59nm)^6, or (SiO2 / Ta2O5)^6)=(138nm / 99nm)^6.
[0065] 7) After the high-reflective film is evaporated, the coated bars are taken out and the laser bars are divided into individual laser chips using a fully automatic dicing machine and a splitting machine.
[0066] 8) Use a fully automatic die bonding machine to mount the cleaved laser chip on a gold-tin heat sink to form a COS assembly, mount the COS assembly on a TO tube, use an automatic wire bonding machine to complete the electrical connection of the laser, use a fully automatic capping machine to cap, and finally package the laser into a TO5.6 sample. Tested with a 2000mA operating current, the maximum operating current is 1310mA.
Claims
1. A method for preparing an AlN film on a semiconductor laser cavity surface, characterized in that: The steps include: 1) Use a scriber to cleave the 808nm semiconductor laser chip into bars of the required cavity length, and place the cleaved bars into a fixture to expose the resonant cavity surface; 2) Clean the coating chamber of the ECR coating equipment to ensure that the chamber is clean and tidy, and put the materials of the coating laser and epitaxial material system as companion pieces; 3) Place the bar fixture in the ECR transfer chamber, start the coating process, and immediately evacuate the chamber. When the vacuum reaches 3.0 to 10×10-5 Torr, the robotic arm moves the bar fixture in the transfer chamber into the coating chamber, and the robotic arm is retracted; 4) After the fixture carrying the bar enters the coating chamber, the front cavity surface is first cleaned at room temperature using ions. During cleaning, the RF source on the target is turned off, the 2.45 GHz microwave source is turned on, the microwave source power is set, and plasma gas is introduced for cleaning; 5) After the ion source cleans the cavity surface, the heating is not turned on and the AlN film is evaporated. Before coating, pre-coating is first performed. During pre-coating, the coating shield is closed, the RF source on the Al target is turned on, and N2 gas is introduced for pre-reaction; the coating shield is turned on and the AlN film is coated; 6) After the front cavity surface is coated, the cavity surface is turned over to deposit on the back cavity surface. Like the front cavity surface, the light-emitting cavity surface is first cleaned with ions. During cleaning, the RF source on the target is turned off, the 2.45 GHz microwave source is turned on, the microwave source power is set, and plasma gas is introduced for cleaning; 7) Performing ion source assisted high reflective film evaporation, the high reflective film layer is AlN+(SiO2 / Si)^6, or AlN+(Al2O3 / TiO2)^6, or AlN+(Al2O3 / Si)^6, or AlN+(SiO2 / Ta2O5)^6; 8) After the high-reflective film is evaporated, the coated bars are taken out and the laser bars are divided into individual laser chips using a fully automatic dicing machine and a chip splitting machine; 9) Use a fully automatic die bonding machine to mount the cleaved laser chip on a gold-tin heat sink to form a COS assembly, mount the COS assembly on a TO tube, use an automatic wire bonding machine to complete the electrical connection of the laser, use a fully automatic capping machine to cap, and finally package the laser into a TO5.6 sample.
2. The method for preparing an AlN thin film for a semiconductor laser cavity surface according to claim 1, characterized in that: In step 1), the semiconductor laser is GaAs or AlGaAs or GaN or other III-V compounds containing Ga.
3. The method for preparing AlN thin film for semiconductor laser cavity surface according to claim 1, characterized in that: In step 4), the microwave source power is set to 200-400 W, 8-20 sccm of plasma gas is introduced, and cleaning is performed for 5-10 minutes; Preferably, in step 6), the microwave source power is set to 200-400 W, 8-20 sccm of plasma gas is introduced, and cleaning is performed for 5-10 minutes.
4. The method for preparing an AlN thin film for a semiconductor laser cavity surface according to claim 3, characterized in that: In step 4) and step 6), the microwave source power is set to 300 W, 10 sccm of plasma gas is introduced, and cleaning is performed for 10 minutes.
5. The method for preparing AlN thin film for semiconductor laser cavity surface according to claim 1, characterized in that: In step 4) and step 6), the plasma gas is a non-oxide, and the selected ones include N2, Ar, H2, NH3, and methane.
6. The method for preparing AlN thin film for semiconductor laser cavity surface according to claim 1, characterized in that: In step 5), the RF power of the RF source is 300-500W, the microwave power is 400-600W, 20-40sccmAr and 3-5sccmN2 gases are introduced, and the pre-reaction is 2-4min; the thickness of the AlN film is 181nm, and the coating rate is about 3nm / min.
7. The method for preparing an AlN film for a semiconductor laser cavity surface according to claim 6, characterized in that: In step 5), the RF power of the RF source is 400 W, the microwave power is 500 W, 30 sccm Ar and 4 sccm N2 gases are introduced, and the pre-reaction is carried out for 3 minutes.
8. The method for preparing AlN thin film for semiconductor laser cavity surface according to claim 1, characterized in that: In step 7), when the high reflective film layer is AlN+(SiO2 / Si)^6, the thickness is 20nm+(138nm / 59nm)^6; when the high reflective film layer is AlN+(Al2O3 / TiO2)^6, the thickness is 20nm+(124nm / 93nm)^6; when the high reflective film layer is AlN+(Al2O3 / Si)^6, the thickness is 20nm+(124nm / 59nm)^6; when the high reflective film layer is AlN+(SiO2 / Ta2O5)^6), the thickness is 20nm+(138nm / 99nm)^6.
9. The method for preparing AlN thin film for semiconductor laser cavity surface according to claim 8, characterized in that: In step 7), a layer of AlN coating is performed as follows: first, pre-coating is performed, during which the coating shield is closed, the RF source on the Al target is turned on, the RF power is 400W, the microwave power is 500W, and 30sccmAr and 4sccmN2 gases are introduced, the pre-reaction is performed for 3min, the coating shield is turned on, and the AlN thin film is coated at a coating rate of 3nm / min. After AlN coating, the Al target shield is closed; Turn on the RF source on the Si target with an RF power of 600W, and introduce 30sccm of Ar gas and 6.8sccm of O2, set the microwave power to 500W, and the coating rate to 7.5nm / min; after SiO2 coating, coat the Si thin film according to the film system design structure, using 600W of RF power, 30sccm of Ar, and 500W of microwave power for coating, with a Si film deposition rate of 4nm / min; then evaporate SiO2 and Si in turn according to the film system design, and a total of 6 pairs of SiO2 / Si thin films with high and low refractive index materials are evaporated.
10. A laser prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The cavity surface is coated with AlN film.