Stainless steel clamp passivation process

Through a stainless steel clamp passivation process including ultrasonic oil removal, passivation treatment and neutralization treatment, a dense passivation film is formed using components such as sodium molybdate, which solves the problem of poor corrosion of existing stainless steel clamps and achieves high Corrosion resistance and low cost passivation effect.

CN118996403APending Publication Date: 2024-11-22YU YAO SHI HENG WEI KA GU YOU XIAN GONG SI
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411092420.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing stainless steel clamps are prone to corrosion during long-term use, affecting their corrosion resistance and service life. Chemical passivation method has limitations of environmental protection and production efficiency, and a new high corrosion resistance passivation process is needed.

Method used

Using a stainless steel clamp passivation process including ultrasonic oil removal, passivation treatment, neutralization treatment and drying steps, using sodium molybdate, sorbic acid, modified nano Ce-galactic acid-titanium dioxide composite material, complexing agent The passivation liquid composed of corrosion inhibitors and lubricants forms a dense passivation film to improve corrosion resistance and surface hardness.

Benefits of technology

It achieves excellent corrosion resistance and surface hardness of stainless steel clamps, is simple to operate, low cost, is environmentally friendly, extends service life, and improves the stability and density of the passivation film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004986953370000081
    Figure BDA0004986953370000081
  • Figure BDA0004986953370000091
    Figure BDA0004986953370000091
Patent Text Reader

Abstract

The invention relates to the technical field of metal surface treatment, in particular to a stainless steel clamp passivation process. The stainless steel clamp passivation technology comprises the following steps that S1, ultrasonic oil removal treatment is conducted; s2, passivating treatment is conducted, sodium molybdate, sorbic acid and other components in a passivating solution and the surface of the stainless steel clamp are subjected to a chemical reaction, a protective passivating film is formed, and the corrosion resistance of the stainless steel clamp is improved; step S3: carrying out neutralization treatment; and S4, performing ultrasonic rinsing and drying. The stainless steel clamp passivation technology can effectively improve the corrosion resistance and the surface hardness of the stainless steel clamp, has the advantages of being simple in technology, low in cost, environmentally friendly and the like, and is suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metal surface treatment, and in particular to a stainless steel clamp passivation process. Background Art

[0002] The clamp is made of stainless steel 304 or 316, which is prone to corrosion during long-term use, affecting the product's appearance and service life.

[0003] As an important surface treatment method in the field of metal processing, passivation can help stainless steel improve its corrosion resistance and stability in various corrosive media. The passivation technology has a long history, and currently the passivation mainly adopts chemical passivation. Chemical passivation is the most widely used method because it is simple and does not require special equipment, has low cost, and is one of the earliest developed methods. However, since chemical passivation mainly relies on the action of the oxidant or polarizer in the passivator to form an oxidation or adsorption film on the metal surface to achieve the mechanism of improving corrosion resistance, the reaction time is usually longer, and it is also inseparable from some strong acid or strong alkaline media. Therefore, there are certain limitations in terms of environmental protection performance and production efficiency. Therefore, a new high-corrosion-resistant stainless steel clamp passivation process is needed to meet market demand. Summary of the invention

[0004] The purpose of this application is to address the deficiencies of current technology and provide a stainless steel clamp passivation process. The stainless steel clamp passivated in this application has excellent corrosion resistance and surface hardness. At the same time, the stainless steel clamp passivation process is simple to operate, low in cost, and environmentally friendly.

[0005] The following technical solutions are adopted: A stainless steel clamp passivation process comprises the following steps: S1. Place the stainless steel clamp in a degreasing liquid at a temperature of 55-60°C for ultrasonic degreasing treatment for 3-5 minutes, and then rinse with two overflow pure water. The degreasing liquid includes the following raw materials by mass concentration: 2-4 g / L sodium hydroxide, 4-6 g / L sodium carbonate, and the rest is deionized water; S2, the stainless steel clamp treated in step S1 is placed in a passivation solution at a temperature of 40-45°C for passivation treatment for 55-60 minutes, and then rinsed with two overflow pure water, wherein the passivation solution, by mass concentration, includes the following preparation raw materials: sodium molybdate 3-5g / L, sorbic acid 5-7g / L, modified nano Ce-gallic acid-titanium dioxide composite material 2-3g / L, complexing agent 0.7-0.9g / L, corrosion inhibitor 0.08-0.12g / L, lubricant 0.2-0.3g / L, silane coupling agent 0.3-0.5g / L, and the rest is deionized water; S3, neutralizing the stainless steel clamp treated in step S2 in a neutralizing solution for 1 minute, and then rinsing with two overflow pure water; S4. The stainless steel clamp treated in step S3 is subjected to two ultrasonic rinses with overflow pure water at a temperature of 55-60° C., and then dried in an oven at a temperature of 90-110° C. for 5-15 minutes to obtain a passivated stainless steel clamp.

[0006] By adopting the above technical scheme, each step of the passivation process of the stainless steel clamp has its specific role, and there is a synergistic effect between these steps, which jointly improves the corrosion resistance and surface hardness of the stainless steel clamp. Step S1: Ultrasonic degreasing treatment, by placing the stainless steel clamp in a degreasing liquid at a temperature of 55-60°C for ultrasonic degreasing treatment, the grease and other contaminants on the surface can be effectively removed. This provides a clean and uniform reaction surface for subsequent passivation treatment. The clean surface is conducive to the passivation liquid to react more evenly with the stainless steel clamp, thereby forming a more uniform and dense passivation layer. Step S2: Passivation treatment, sodium molybdate, sorbic acid and other components in the passivation solution react chemically with the surface of the stainless steel clamp to form a protective passivation film to improve its corrosion resistance. In step S2, each component of the passivation solution plays a specific role, and there is a synergistic effect between them, which jointly promotes the formation of a passivation film with excellent corrosion resistance and surface hardness on the surface of the stainless steel clamp. As one of the main components in the passivation solution, sodium molybdate participates in chemical reactions to help form a stable passivation layer on the surface of the stainless steel clamp. It works together with other components such as sorbic acid and modified nano Ce-gallic acid-titanium dioxide composite materials to form a more uniform and dense passivation layer and improve corrosion resistance. As an organic acid, sorbic acid can react with the metal surface to form a stable compound to enhance the protective effect of the passivation film. Together with sodium molybdate and other components, it forms a complex protective layer through chemical adsorption and reaction to enhance the corrosion resistance and hardness of the passivation film. As a functional additive, the modified nano Ce-gallic acid-titanium dioxide composite material is firmly combined in the passivation layer through the bridging effect of the silane coupling agent, exerting an anti-corrosion and corrosion-inhibiting effect, greatly improving the stability, corrosion resistance and surface hardness of the passivation film. Complexing agents such as ethylenediaminetetramethylenephosphonic acid, methylbenzotriazole and sodium glucoheptonic acid can complex Fe3+ produced in the passivation reaction and accelerate the reaction rate. By inhibiting the deposition rate of iron ions, the rough and dull coating caused by excessive deposition is avoided, thereby improving the corrosion resistance of the stainless steel clamp. The corrosion inhibitor can slow down the corrosion process on the metal surface and protect the metal from the erosion of the corrosive medium. It works together with other components in the passivation solution to form a more stable and durable passivation film, extending the service life of the stainless steel clamp. The lubricant can reduce the surface tension of the passivator and reduce defects such as gas pinholes and pitting on the surface of the stainless steel clamp. By shortening the contact time between the passivator and the stainless steel clamp, the surface lattice of the passivation film is refined, and the density of the passivation film is increased, thereby enhancing the corrosion resistance. The silane coupling agent acts as a bridging agent to help the modified nano Ce-gallic acid-titanium dioxide composite material to be more firmly bonded to the passivation layer. Enhance the bonding force between the composite material and the surface of the stainless steel clamp and improve the stability and surface hardness of the passivation film. Step S3: Neutralization treatment, the neutralization treatment can remove acidic or alkaline substances that may remain on the surface of the stainless steel clamp after the passivation treatment, and prevent these substances from affecting the quality of the passivation film.Neutralization treatment ensures the chemical stability of the passivation film and avoids possible damage to the passivation film during subsequent rinsing and drying. Step S4: Ultrasonic rinsing and drying. Ultrasonic rinsing can completely remove the chemical substances remaining on the surface of the stainless steel clamp after passivation and neutralization treatment, while drying removes moisture to prevent corrosion caused by moisture. Thorough rinsing and drying help maintain the integrity of the passivation film and ensure its long-term protective effect. Overall, the stainless steel clamp passivation process of the present application not only improves the corrosion resistance and surface hardness of the stainless steel clamp through a series of sophisticated chemical treatment steps, but also ensures the high quality and long-term stability of the passivation film through the synergistic effect of each step. In addition, the process is simple to operate, low in cost, environmentally friendly, and meets the needs of modern industrial production.

[0007] Preferably, in step S2, the method for preparing the modified nano Ce-gallic acid-titanium dioxide composite material comprises the following steps: S21. At room temperature, 100 mL of tetra-n-butyl titanate was added to a solution consisting of 150 mL of ethanol and 20 mL of deionized water, and stirred for 30 min to form solution A. S22, add 50 mL of 0.06 mol / L cerium nitrate ethanol solution to solution A, stir evenly, to form solution B; S23, add 60 mL of 0.03 mol / L gallic acid ethanol solution to solution B, stir evenly, and obtain a mixed solution C; S24, adding 50-60 mL of aqueous ammonia to the mixed solution C, stirring the mixture at room temperature for 12 h, then centrifuging, washing, drying at 90° C. for 12 h, and cooling to obtain a nano Ce-gallic acid-titanium dioxide composite material; S25, mixing 1 g of γ-(methacryloyloxy)propyltrimethoxysilane with 120 g of ethanol and 30 g of water, and hydrolyzing for 1 h to obtain a mixture D; S26. Add the obtained nano Ce-gallic acid-titanium dioxide composite material to mixture D, then heat to 43°C, stir at 200 r / min for 150 min, and finally filter, wash, dry and grind at 80°C to obtain a modified nano Ce-gallic acid-titanium dioxide composite material with a particle size of 50 nanometers.

[0008] By adopting the above technical scheme, steps S21-S23: preparing a nano Ce-gallic acid-titanium dioxide composite material, using tetrabutyl titanate as a titanium source, cerium nitrate to provide cerium elements, and gallic acid as an organic ligand through a sol-gel method, to form a Ce-gallic acid complex-doped titanium dioxide composite material. This composite material combines the stability of titanium dioxide and the anti-corrosion and corrosion inhibition properties of Ce-gallic acid complexes. The complex formed by Ce ions and gallic acid can improve the corrosion resistance and surface hardness of titanium dioxide, and titanium dioxide provides a stable carrier for these complexes, so that the composite material has better dispersibility and reactivity in the passivation solution. Step S24: synthesizing nanoparticles: by adding ammonia water and stirring the reaction, then centrifugation, washing and drying, a nano Ce-gallic acid-titanium dioxide composite material is obtained. This step ensures the purity and nanometer-scale particle size of the composite material, thereby enhancing its functionality in the passivation solution. The nanometer-scale particle size makes the composite material have a higher specific surface area, improves its contact efficiency with the surface of the stainless steel clamp, and thus more effectively plays an anti-corrosion and corrosion-inhibiting role during the passivation process. Step S25-S26: Modified nanocomposite material: Use γ-(methacryloyloxy)propyltrimethoxysilane to modify the nano Ce-gallic acid-titanium dioxide composite material, introduce a silane coupling agent, and enhance the bonding force between the composite material and the surface of the stainless steel clamp. The bridging effect of the silane coupling agent makes the composite material more firmly bonded to the passivation layer, improving the stability and corrosion resistance of the passivation film. At the same time, the dispersibility of the modified composite material in the passivation solution is improved, which is conducive to the formation of a uniform and dense passivation layer. In general, the steps involved in the preparation method of the modified nano Ce-gallic acid-titanium dioxide composite material are all aimed at improving the performance of the composite material in the passivation solution, including its stability, corrosion resistance and bonding ability with the surface of the stainless steel clamp. The improvement of these properties helps to form a denser and more corrosion-resistant passivation layer during the passivation process, greatly improving the stability, corrosion resistance and surface hardness of the passivation film.

[0009] Preferably, in step S2, the complexing agent is composed of ethylenediaminetetramethylenephosphonic acid, methylbenzotriazole and sodium glucoheptonate in a mass ratio of 3:3:4.

[0010] By adopting the above technical solution, ethylenediaminetetramethylenephosphonic acid, as a powerful chelating agent, can form a stable complex with metal ions, thereby preventing these metal ions from participating in harmful chemical reactions. Toluenetriazole has anti-corrosion properties and can be used as an anodic corrosion inhibitor to prevent further oxidation of the metal by forming a protective complex film on the metal surface. Sodium glucoheptonate, as an organic compound, can also form a stable complex with metal ions, thereby slowing down the corrosion process on the metal surface. When ethylenediaminetetramethylenephosphonic acid, toluenetriazole and sodium glucoheptonate are mixed in a specific proportion, a synergistic effect is produced between them. This synergistic effect enables the mixture to more effectively bind to the Fe generated on the surface of the stainless steel clamp. 3+ Ion complexation speeds up the reaction rate, thereby accelerating the formation of the passivation film. This combination of complexing agents can inhibit the deposition rate of iron ions, avoiding the roughness and dullness of the coating caused by too fast deposition, thereby improving the corrosion resistance and aesthetics of the stainless steel clamp. Through their combined effect, these complexing agents not only slow down the release of metal ions, but also help to form a more uniform and dense passivation film on the metal surface, further enhancing the corrosion resistance of the stainless steel clamp.

[0011] Preferably, in step S2, the corrosion inhibitor is hydroxyethylidene diphosphonic acid.

[0012] Preferably, in step S2, the lubricant is composed of nonylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether and polyethylene glycol in a mass ratio of 2:2:1.

[0013] By adopting the above technical scheme, both nonylphenol polyoxyethylene ether and fatty alcohol polyoxyethylene ether have lower surface tension, which can effectively reduce the surface tension of the passivator, and is conducive to the uniform coating of the passivator on the surface of the stainless steel clamp. Polyethylene glycol has good lubricity, which can reduce the friction between the passivator and the surface of the stainless steel clamp, is conducive to the rapid flow of the passivator on the surface of the stainless steel clamp, and shortens the passivation time. The three substances have good compatibility and can form a stable mixture in the passivator, which is conducive to the stable use of the passivator. The synergistic effect between the three substances reduces the surface tension of the passivator, reduces or eliminates the gas pinholes and pits on the surface of the stainless steel clamp, shortens the contact time between the passivator and the stainless steel clamp, thereby shortening the passivation time, refining the surface lattice of the passivation film, and improving the density of the passivation film, thereby improving the corrosion resistance of the stainless steel clamp. In summary, by using a lubricant composed of nonylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether and polyethylene glycol, the corrosion resistance and surface hardness of the passivated stainless steel clamp can be effectively improved while ensuring the passivation process of the stainless steel clamp is simple, low-cost and environmentally friendly.

[0014] Preferably, the silane coupling agent is composed of γ-(methacryloyloxy)propyltrimethoxysilane and vinyltriethoxysilane in a mass ratio of 3:1.

[0015] Preferably, in step S3, the neutralization solution comprises the following raw materials, measured by mass concentration: 5-10 g / L of sodium carbonate and the remainder being deionized water.

[0016] In summary, the beneficial technical effects of this application are: 1. Excellent corrosion resistance and surface hardness: By using the Ce-gallic acid complex formed by gallic acid and Ce ions to dope nano-titanium dioxide composite materials as functional additives for the passivation solution, a denser and more corrosion-resistant passivation layer can be formed. The bridging effect of the silane coupling agent makes the composite material more firmly bonded to the passivation layer, thereby greatly improving the stability, corrosion resistance and surface hardness of the passivation film.

[0017] 2. Simple operation, low cost and environmentally friendly: The passivation process is simple to operate, does not require complex equipment and high-cost materials, and the environmentally friendly chemicals used will not pollute the environment.

[0018] 3. Improve the quality of the passivation film: The use of lubricant reduces the surface tension of the passivator, reduces defects such as gas pinholes and pitting on the surface of the stainless steel clamp, shortens the passivation time, refines the surface lattice of the passivation film, and increases the density of the passivation film, thereby significantly improving the corrosion resistance of the stainless steel clamp.

[0019] 4. Accelerate the reaction rate: The complexing agent composed of specific raw materials, such as ethylenediaminetetramethylenephosphonic acid, methylbenzotriazole and sodium glucoheptonic acid, can complex the Fe3+ produced in the passivation reaction, accelerate the reaction rate, inhibit the deposition rate of iron ions, avoid rough and dull coating, and further improve the corrosion resistance of stainless steel clamps. DETAILED DESCRIPTION

[0020] The embodiments of the present application will be described in detail below in conjunction with the examples, but those skilled in the art will understand that the following examples are only used to illustrate the present application and should not be considered to limit the scope of the present application. If the specific conditions are not specified in the examples, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially, and the stainless steel clamp is made of stainless steel 304.

[0021] Preparation Example 1 Preparation of modified nano Ce-gallic acid-titanium dioxide composite material The preparation method of the modified nano Ce-gallic acid-titanium dioxide composite material comprises the following steps: S21. At room temperature, 100 mL of tetra-n-butyl titanate was added to a solution consisting of 150 mL of ethanol and 20 mL of deionized water, and stirred for 30 min to form solution A. S22, add 50 mL of 0.06 mol / L cerium nitrate ethanol solution to solution A, stir evenly, to form solution B; S23, add 60 mL of 0.03 mol / L gallic acid ethanol solution to solution B, stir evenly, and obtain a mixed solution C; S24, adding 55 mL of aqueous ammonia to the mixed solution C, stirring the mixture at room temperature for 12 h, then centrifuging, washing, drying at 90° C. for 12 h, and cooling to obtain a nano Ce-gallic acid-titanium dioxide composite material; S25, mixing 1 g of γ-(methacryloyloxy)propyltrimethoxysilane with 120 g of ethanol and 30 g of water, and hydrolyzing for 1 h to obtain a mixture D; S26. Add the obtained nano Ce-gallic acid-titanium dioxide composite material to mixture D, then heat to 43°C, stir at 200 r / min for 150 min, and finally filter, wash, dry and grind at 80°C to obtain a modified nano Ce-gallic acid-titanium dioxide composite material with a particle size of 50 nanometers.

[0022] Preparation of Comparative Example 1 Preparation of Nano Ce-Gallic Acid-Titanium Dioxide Composite Material The same as Preparation Example 1, except that steps S25 and S26 are omitted.

[0023] Example 1 A stainless steel clamp passivation process comprises the following steps: S1. Place the stainless steel clamp in a degreasing solution at a temperature of 55°C for ultrasonic degreasing treatment for 5 minutes, and then rinse with two overflow pure water. The degreasing solution includes the following raw materials by mass concentration: 4 g / L sodium hydroxide, 4 g / L sodium carbonate, and the rest is deionized water; S2. The stainless steel clamp treated in step S1 is placed in a passivation solution at a temperature of 40° C. for passivation treatment for 60 minutes, and then rinsed with two overflow pure water, wherein the passivation solution, by mass concentration, comprises the following preparation raw materials: 3 g / L sodium molybdate, 5 g / L sorbic acid, 2 g / L modified nano Ce-gallic acid-titanium dioxide composite material, 0.7 g / L complexing agent, 0.08 g / L hydroxyethylidene diphosphonic acid, and 0.2 g / L lubricant. , silane coupling agent 0.3g / L, the rest is deionized water; the complexing agent is composed of ethylenediaminetetramethylenephosphonic acid, methylbenzotriazole and sodium glucoheptonic acid in a mass ratio of 3:3:4; the lubricant is composed of nonylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether and polyethylene glycol in a mass ratio of 2:2:1; the silane coupling agent is composed of γ-(methacryloyloxy)propyltrimethoxysilane and vinyltriethoxysilane in a mass ratio of 3:1; S3, neutralizing the stainless steel clamp treated in step S2 in a neutralizing solution for 1 minute, and then rinsing with two overflow pure water, wherein the neutralizing solution, by mass concentration, includes the following preparation raw materials: 5 g / L sodium carbonate and the rest is deionized water; S4. The stainless steel clamp treated in step S3 is subjected to two ultrasonic rinses at 55° C. with overflow pure water, and then dried in an oven at 90° C. for 15 minutes to obtain a passivated stainless steel clamp.

[0024] Example 2 A stainless steel clamp passivation process comprises the following steps: S1. Place the stainless steel clamp in a degreasing solution at a temperature of 60°C for ultrasonic degreasing treatment for 3 minutes, and then rinse with two overflow pure water. The degreasing solution includes the following raw materials by mass concentration: 2 g / L sodium hydroxide, 6 g / L sodium carbonate, and the rest is deionized water; S2. The stainless steel clamp treated in step S1 is placed in a passivation solution at a temperature of 45° C. for passivation treatment for 55 minutes, and then rinsed with two overflow pure water, wherein the passivation solution, by mass concentration, comprises the following preparation raw materials: 5 g / L sodium molybdate, 7 g / L sorbic acid, 3 g / L modified nano Ce-gallic acid-titanium dioxide composite material, 0.9 g / L complexing agent, 0.12 g / L hydroxyethylidene diphosphonic acid, and 0.3 g / L lubricant. , silane coupling agent 0.5g / L, the rest is deionized water; the complexing agent is composed of ethylenediaminetetramethylenephosphonic acid, methylbenzotriazole and sodium glucoheptonic acid in a mass ratio of 3:3:4; the lubricant is composed of nonylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether and polyethylene glycol in a mass ratio of 2:2:1; the silane coupling agent is composed of γ-(methacryloyloxy)propyltrimethoxysilane and vinyltriethoxysilane in a mass ratio of 3:1; S3, neutralizing the stainless steel clamp treated in step S2 in a neutralizing solution for 1 minute, and then rinsing with two overflow pure water, wherein the neutralizing solution, by mass concentration, includes the following preparation raw materials: 10 g / L sodium carbonate and the rest is deionized water; S4. The stainless steel clamp treated in step S3 is subjected to two ultrasonic rinses at 60° C. with overflow pure water, and then dried in an oven at 110° C. for 5 minutes to obtain a passivated stainless steel clamp.

[0025] Example 3 A stainless steel clamp passivation process comprises the following steps: S1. Place the stainless steel clamp in a degreasing solution at a temperature of 58°C for ultrasonic degreasing treatment for 4 minutes, and then rinse with two overflow pure water. The degreasing solution includes the following raw materials by mass concentration: 3 g / L sodium hydroxide, 5 g / L sodium carbonate, and the rest is deionized water; S2, the stainless steel clamp treated in step S1 is placed in a passivation solution at a temperature of 43°C for passivation treatment for 57 minutes, and then rinsed with two overflow pure water, wherein the passivation solution, by mass concentration, includes the following preparation raw materials: 4g / L sodium molybdate, 6g / L sorbic acid, 2.5g / L modified nano Ce-gallic acid-titanium dioxide composite material, 0.8g / L complexing agent, 0.1g / L hydroxyethylidene diphosphonic acid, 0.25g / L lubricant, 0.4g / L silane coupling agent, and the rest is deionized water; the complexing agent is ethylenediaminetetramethylenephosphonic acid, methylbenzotriazine The azole and sodium glucoheptonic acid are composed of a mass ratio of 3:3:4; the lubricant is composed of nonylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether and polyethylene glycol in a mass ratio of 2:2:1; the silane coupling agent is composed of γ-(methacryloyloxy)propyltrimethoxysilane and vinyltriethoxysilane in a mass ratio of 3:1; S3, the stainless steel clamp treated in step S2 is neutralized in a neutralizing solution for 1 minute, and then rinsed with two overflow pure water, wherein the neutralizing solution, by mass concentration, includes the following preparation raw materials: 7g / L sodium carbonate and the rest is deionized water; S4. The stainless steel clamp treated in step S3 is subjected to two ultrasonic rinses at 58° C. with overflow pure water, and then dried in an oven at 100° C. for 10 minutes to obtain a passivated stainless steel clamp.

[0026] Comparative Example 1 The same as Example 3, except that an equal amount of the nano Ce-gallic acid-titanium dioxide composite material prepared in Comparative Example 1 is used to replace the modified nano Ce-gallic acid-titanium dioxide composite material.

[0027] Comparative Example 2 The same as Example 3, except that the complexing agent is ethylenediaminetetramethylenephosphonic acid.

[0028] Comparative Example 3 The same as Example 3, except that the complexing agent is methylbenzotriazole.

[0029] Comparative Example 4 The same as Example 3, except that the complexing agent is sodium glucoheptonate.

[0030] Comparative Example 5 The same as Example 3, except that the lubricant is nonylphenol polyoxyethylene ether.

[0031] Comparative Example 6 The same as Example 3, except that the lubricant is fatty alcohol polyoxyethylene ether.

[0032] Comparative Example 7 Same as Example 3, except that the lubricant is polyethylene glycol.

[0033] Performance Testing The stainless steel clamps prepared in Examples 1 to 3 and Comparative Examples 1 to 7 were subjected to performance tests, and the results are shown in Table 1.

[0034] Salt spray corrosion performance: neutral salt spray test is carried out in accordance with GB / T 10125-2021 "Salt spray test for corrosion test in artificial atmosphere". The test results are evaluated in accordance with GB / T 6461-2002 "Rating of samples and test pieces of metal and other inorganic coatings on metal substrates after corrosion tests". The time until the surface reaches level 9 is recorded and observed every 12 hours; Boil salt water, put the sample into the pressure cooker, add 1% salt water to the maximum scale line, close the lid and work continuously. During the test, check once every 8 hours and record the time when rust appears; Surface hardness: Use Vickers hardness tester to test the hardness of the passivation film; Table 1 Performance test Analyzing the data in Table 1, we can see that: 1) The stainless steel clamps prepared in Examples 1 to 3 have excellent corrosion resistance and surface hardness. At the same time, the passivation process of the stainless steel clamp is simple to operate, low in cost, and environmentally friendly.

[0035] 2) The performance comparison analysis of the stainless steel clamps prepared in Example 3 and Comparative Example 1 shows that the nano Ce-gallic acid-titanium dioxide composite material is modified by using γ-(methacryloyloxy)propyltrimethoxysilane, and the silane coupling agent is introduced to enhance the bonding force between the composite material and the surface of the stainless steel clamp. The bridging effect of the silane coupling agent makes the composite material more firmly bonded to the passivation layer, thereby improving the stability and corrosion resistance of the passivation film. At the same time, the dispersibility of the modified composite material in the passivation solution is improved, which is conducive to the formation of a uniform and dense passivation layer.

[0036] 3) The performance comparison analysis of the stainless steel clamps prepared in Example 3 and Comparative Examples 2-4 shows that the complexing agent is composed of ethylenediaminetetramethylenephosphonic acid, methylbenzotriazole and sodium glucoheptonic acid in a mass ratio of 3:3:4. When ethylenediaminetetramethylenephosphonic acid, methylbenzotriazole and sodium glucoheptonic acid are mixed in a specific ratio, a synergistic effect is generated between them. This synergistic effect enables the mixture to more effectively bind to the Fe generated on the surface of the stainless steel clamp. 3+ Ion complexation speeds up the reaction rate, thereby accelerating the formation of the passivation film. This combination of complexing agents can inhibit the deposition rate of iron ions, avoiding the roughness and dullness of the coating caused by too fast deposition, thereby improving the corrosion resistance and aesthetics of the stainless steel clamp. Through their combined effect, these complexing agents not only slow down the release of metal ions, but also help to form a more uniform and dense passivation film on the metal surface, further enhancing the corrosion resistance of the stainless steel clamp.

[0037] 4) The performance comparison analysis of the stainless steel clamps prepared in combination with Example 3 and Comparative Examples 5-7 shows that the lubricant is composed of nonylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether and polyethylene glycol in a mass ratio of 2:2:1. These three substances have good compatibility and can form a stable mixture in the passivator, which is conducive to the stable use of the passivator. The synergistic effect between the three substances reduces the surface tension of the passivator, reduces or eliminates the gas pinholes and pits on the surface of the stainless steel clamp, shortens the contact time between the passivator and the stainless steel clamp, thereby shortening the passivation time, refining the surface lattice of the passivation film, improving the density of the passivation film, and effectively improving the corrosion resistance and surface hardness of the stainless steel clamp after passivation.

[0038] The above embodiments are only used to explain the technical solutions of the present invention rather than to limit the same. Although the above embodiments specifically describe the present invention, relevant technical personnel should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A stainless steel clamp passivation process, characterized in that: The following steps are involved: S1. Place the stainless steel clamp in a degreasing liquid at a temperature of 55-60°C for ultrasonic degreasing for 3-5 minutes, and then rinse with two overflow pure water; S2, the stainless steel clamp treated in step S1 is placed in a passivation solution at a temperature of 40-45°C for passivation treatment for 55-60 minutes, and then rinsed with two overflow pure water, wherein the passivation solution, by mass concentration, includes the following preparation raw materials: sodium molybdate 3-5g / L, sorbic acid 5-7g / L, modified nano Ce-gallic acid-titanium dioxide composite material 2-3g / L, complexing agent 0.7-0.9g / L, corrosion inhibitor 0.08-0.12g / L, lubricant 0.2-0.3g / L, silane coupling agent 0.3-0.5g / L, and the rest is deionized water; S3, neutralizing the stainless steel clamp treated in step S2 in a neutralizing solution for 1 minute, and then rinsing with two overflow pure water; S4. The stainless steel clamp treated in step S3 is subjected to two ultrasonic rinses with overflow pure water at a temperature of 55-60° C., and then dried in an oven at a temperature of 90-110° C. for 5-15 minutes to obtain a passivated stainless steel clamp.

2. A stainless steel clamp passivation process according to claim 1, characterized in that: In step S1, the degreasing liquid includes the following raw materials, measured by mass concentration: 2-4 g / L of sodium hydroxide, 4-6 g / L of sodium carbonate, and the remainder is deionized water.

3. A stainless steel clamp passivation process according to claim 1, characterized in that: In step S2, the method for preparing the modified nano Ce-gallic acid-titanium dioxide composite material comprises the following steps: S31. At room temperature, 100 mL of tetra-n-butyl titanate was added to a solution consisting of 150 mL of ethanol and 20 mL of deionized water, and stirred for 30 min to form solution A. S32, add 50 mL of 0.06 mol / L cerium nitrate ethanol solution to solution A, stir evenly, to form solution B; S33, dropwise add 60 mL of 0.03 mol / L gallic acid ethanol solution into solution B, stir evenly, and obtain a mixed solution C; S34, adding 50-60 mL of aqueous ammonia to the mixed solution C, stirring the mixture at room temperature for 12 h, then centrifuging, washing, drying at 90° C. for 12 h, and cooling to obtain a nano Ce gallic acid-titanium dioxide composite material; S35, mixing 1 g of γ-(methacryloyloxy)propyltrimethoxysilane with 120 g of ethanol and 30 g of water, and hydrolyzing for 1 h to obtain a mixture D; S36. Add the obtained nano Ce-gallic acid-titanium dioxide composite material to mixture D, then heat it to 43°C, stir it at 200 r / min for 150 min, and finally filter, wash, dry and grind it at 80°C to obtain a modified nano Ce-gallic acid-titanium dioxide composite material with a particle size of 50 nanometers.

4. A stainless steel clamp passivation process according to claim 1, characterized in that: In step S2, the complexing agent is composed of ethylenediaminetetramethylenephosphonic acid, methylbenzotriazole and sodium glucoheptonate in a mass ratio of 3:3:

4.

5. A stainless steel clamp passivation process according to claim 1, characterized in that: In step S2, the corrosion inhibitor is hydroxyethylidene diphosphonic acid.

6. A stainless steel clamp passivation process according to claim 1, characterized in that: In step S2, the lubricant is composed of nonylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether and polyethylene glycol in a mass ratio of 2:2:

1.

7. A stainless steel clamp passivation process according to claim 1, characterized in that: The silane coupling agent is composed of γ-(methacryloyloxy)propyltrimethoxysilane and vinyltriethoxysilane in a mass ratio of 3:

1.

8. A stainless steel clamp passivation process according to claim 1, characterized in that: In step S3, the neutralization solution includes the following raw materials in terms of mass concentration: 5-10 g / L of sodium carbonate and the remainder is deionized water.

Citation Information

Cited By

  • Stainless steel surface passivation treatment process

    CN119615140A

  • A passivation treatment process for stainless steel surface

    CN119615140B