Composite current collector, preparation method thereof and secondary battery

By introducing electroless nickel-phosphorus plating and silane sealing processes before copper plating of the magnetron sputtering film, the problems of insufficient density and adhesion in the copper plating process of the magnetron sputtering film were solved, achieving lower magnetron film thickness and sheet resistance requirements, and improving the finished product qualification rate and production efficiency.

CN118996419APending Publication Date: 2024-11-22JIANGYIN NANOPORE INNOVATIVE MATERIALS TECH LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411097808.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing magnetron sputtering copper plating process produces finished products with poor density and low adhesion, and has high requirements for the thickness and sheet resistance of the magnetron sputtering film, resulting in a low finished product qualification rate.

Method used

Before copper plating, an electroless nickel-phosphorus plating process and a silane sealing process are introduced to increase the density and adhesion of the film surface, reduce the requirements for the thickness and sheet resistance of the magnetron sputtering film, and adopt a low-phosphorus weak alkaline electroless nickel plating process and ultrasonic-assisted plating, combined with silane sealing treatment.

Benefits of technology

It improves the yield of composite current collectors, reduces the energy and difficulty of magnetron coating production, reduces the probability of magnetron film pores, and achieves lower sheet resistance and thickness requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004988492370000201
    Figure BDA0004988492370000201
Patent Text Reader

Abstract

The invention provides a composite current collector, a preparation method thereof and a secondary battery, and belongs to the technical field of battery materials, the preparation method comprises the following steps: (1) unreeling a magnetic control film, and carrying out pretreatment; (2) plating a nickel-phosphorus alloy layer on the surface of at least one side of the magnetic control film by adopting a chemical nickel-phosphorus plating process; (3) carrying out hole sealing treatment on the composite film obtained in the step (2) by adopting a silane hole sealing process, wherein the silane hole sealing process specifically comprises the following steps: carrying out hole sealing treatment on the obtained composite film by adopting a hole sealing solution; and (4) carrying out double-sided copper plating on the composite film subjected to hole sealing treatment, and then carrying out post-treatment to obtain the composite current collector. The chemical nickel and phosphorus plating process and the silane hole sealing process are introduced before copper plating of the magnetic control film, the compactness and the bonding force of the film surface are improved, the percent of pass is increased, the requirements for the thickness and the sheet resistance of the magnetic control film layer are reduced, and the probability that the magnetic control film goes out of holes is synchronously reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery materials, and in particular relates to a composite current collector and a preparation method thereof, and a secondary battery. Background Art

[0002] At present, the double-sided copper plating process for the surface of various types of plastic ultra-thin films (such as PP film or PET film, but not limited to these two types) is to perform double-sided water-plated acid copper plating on the magnetron film (which has been double-sided magnetron copper plating). This process has high requirements for the magnetron film, requiring the square resistance of both sides of the acid copper front film to be at least below 1Ω, and the thickness to reach 40-60nm. High energy is required during the magnetron plating process, and it is very easy to perforate or de-copperize, which makes the probability of unqualified density of the finished product high, and the qualified rate of physical properties such as adhesion is also relatively low.

[0003] Therefore, there is an urgent need to provide a method that can not only solve the problems of poor density and poor adhesion of the finished film produced by the magnetron film copper plating process, but also significantly reduce the requirements for the thickness and square resistance of the magnetron film layer, thereby improving the qualified rate of the finished product. Summary of the invention

[0004] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a composite current collector and a preparation method thereof and a secondary battery. The present invention introduces a chemical nickel-phosphorus plating process and a silane sealing process before copper plating the magnetron film, which, on the one hand, increases the density and adhesion of the film surface and improves the qualified rate of the composite current collector, and on the other hand, reduces the requirements for the thickness and square resistance of the magnetron film layer, with the square resistance being below 2Ω and the thickness being 20-40nm, thereby reducing the total energy and process difficulty of the magnetron coating production process and simultaneously reducing the probability of the magnetron film having holes.

[0005] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a composite current collector, the preparation method comprising the following steps:

[0007] (1) Unwinding the magnetron film and performing pretreatment;

[0008] (2) using a chemical nickel-phosphorus plating process to plate a nickel-phosphorus alloy layer on both sides of the magnetron film; the specific steps of the silane sealing process include:

[0009] The obtained composite membrane is sealed with a sealing solution;

[0010] (3) sealing the composite membrane obtained in step (2) by using a silane sealing process;

[0011] (4) copper plating is performed on both sides of the composite film after the sealing treatment, and then post-treatment is performed to obtain the composite current collector.

[0012] The present invention introduces a chemical nickel-phosphorus plating process and a silane sealing process before copper plating the magnetron film, which, on the one hand, increases the density and adhesion of the film surface and improves the qualified rate of the composite current collector, and on the other hand, reduces the requirements for the thickness and square resistance of the magnetron film layer, with the square resistance being below 2Ω and the thickness being 20-40nm, thereby reducing the total energy and process difficulty of the magnetron coating production process and simultaneously reducing the probability of holes in the magnetron film.

[0013] As a preferred technical solution of the present invention, the pre-treatment step in step (1) includes water washing.

[0014] Preferably, the magnetron film in step (1) comprises a base film and copper layers arranged on both side surfaces of the base film.

[0015] Preferably, the material of the base film includes PP (polypropylene) and / or PET (polyethylene terephthalate).

[0016] Preferably, the sheet resistance of both sides of the magnetron film in step (1) is 1-2Ω, for example, 1Ω, 1.5Ω or 2Ω.

[0017] Preferably, the thickness of the copper layer on one side is 20-40 nm, for example, 20 nm, 30 nm or 40 nm.

[0018] As a preferred technical solution of the present invention, the chemical nickel-phosphorus plating process in step (2) is a low-phosphorus weak alkaline chemical nickel process, and the specific steps of the low-phosphorus weak alkaline chemical nickel process include:

[0019] (a) mixing a nickel plating solution, a coordination compound, an accelerator, a stabilizer, a wetting agent and a phosphorus plating solution to obtain a chemical plating solution;

[0020] (b) placing the magnetron film in the chemical plating solution to perform a plating reaction to obtain a nickel-phosphorus alloy layer.

[0021] In the present invention, a low-phosphorus weakly alkaline chemical nickel process is used to plate a nickel-phosphorus alloy layer. If the copper layer on the previous magnetron film has poor plating performance, a thin coating can also be formed to form a cover, thereby preventing the magnetron copper layer from being corroded in an acid environment. At the same time, the weakly alkaline environment also avoids the pressure of the subsequent water washing step, thereby preventing the nickel plating solution from contaminating the sealing solution and the subsequent acid copper solution.

[0022] As a preferred technical solution of the present invention, the nickel plating solution in step (a) includes a nickel salt, and the nickel salt includes any one of nickel chloride, nickel sulfate or nickel acetate, or a combination of at least two of them.

[0023] Preferably, the concentration of the nickel plating solution in step (a) is 20-40 g / L, for example, it can be 20 g / L, 25 g / L, 30 g / L, 35 g / L or 40 g / L.

[0024] Preferably, the nickel plating solution in step (a) is prepared by dissolving nickel salt in water and heating the solution, and the heating temperature is 60-80°C, for example, 60°C, 65°C, 70°C, 75°C or 80°C.

[0025] It should be noted that the nickel plating solution is configured by an independent tank body, and 1 / 3 of the total volume of the tank is used to heat and dissolve the nickel salt.

[0026] Preferably, the phosphorus plating solution in step (a) comprises a phosphorus salt, and the phosphorus salt comprises sodium hypophosphite monohydrate and / or sodium dihydrogen phosphate.

[0027] It should be noted that sodium hypophosphite monohydrate is also used as a reducing agent. When used as a reducing agent, it can reduce metal ions in the plating solution into metals and deposit them on the surface of the plated part.

[0028] Preferably, the concentration of the phosphorus plating solution in step (a) is 10-40 g / L, for example, 10 g / L, 20 g / L, 30 g / L or 40 g / L.

[0029] Preferably, the mass ratio of nickel ions in the nickel plating solution in step (a) to phosphate ions in the phosphorus plating solution is (0.3-0.6):1, for example, it can be 0.3:1, 0.4:1, 0.5:1 or 0.6:1, etc., preferably (0.3-0.4):1.

[0030] In the present invention, when the mass ratio of nickel ions in the nickel plating solution to phosphate ions in the phosphorus plating solution is too small or too large, that is, less than 0.3 or greater than 0.6, the plating rate of the nickel-phosphorus alloy layer is low and the plated layer is dark.

[0031] It should be noted that, for the preparation of the phosphorus plating solution, an independent tank is prepared in advance, that is, 1 / 3 of the water volume of the main tank is used to dissolve the phosphate salt.

[0032] As a preferred technical solution of the present invention, the specific steps of mixing in step (a) include:

[0033] The coordination compound, accelerator, stabilizer and wetting agent are mixed once to obtain a primary mixed solution, and then the primary mixed solution and the nickel plating solution are mixed twice to obtain a secondary mixed solution, and then the secondary mixed solution and the phosphorus plating solution are mixed three times.

[0034] It should be noted that the primary mixed liquid is obtained by dissolving 1 / 3 of the total volume of the preparation tank in the main tank.

[0035] Preferably, the coordination compound comprises any one of ammonium salt, citrate or potassium pyrophosphate or a combination of at least two thereof, preferably a combination of ammonium salt, citrate and potassium pyrophosphate.

[0036] Preferably, in the primary mixed solution, the mass ratio of ammonium salt, citrate and potassium pyrophosphate is (20-50):(20-50):(30-50), wherein the selection range of ammonium salt "20-50" exemplarily includes 20, 30, 40 or 50, etc., the selection range of citrate "20-50" exemplarily includes 20, 30, 40 or 50, etc., and the selection range of potassium pyrophosphate "30-50" exemplarily includes 30, 40 or 50, etc.

[0037] Preferably, the coordination compound further comprises a lactic acid solution.

[0038] It should be noted that the mass fraction of the lactic acid solution is not specifically limited in the present invention, and by way of example, it may be 80%.

[0039] Preferably, the ammonium salt comprises ammonium chloride and / or ammonium sulfate.

[0040] Preferably, the citrate comprises sodium citrate and / or ammonium citrate.

[0041] Preferably, the accelerator comprises any one of ammonia water, fatty acid, propionic acid, succinic acid, malic acid, triethanolamine, fluoride or lithium salt, or a combination of at least two thereof, preferably ammonia water.

[0042] Preferably, the mass concentration of the accelerator in the primary mixed solution is 10-30 g / L, for example, 10 g / L, 15 g / L, 20 g / L, 25 g / L or 30 g / L.

[0043] Preferably, the stabilizer includes any one of thiourea, 3-5-isothiourea propane sulfonate, phthalic anhydride, hexamethylenetetraphthalic anhydride, mercaptobenzothiazole, xanthate or sodium thiosulfate, or a combination of at least two thereof, preferably a combination of thiourea, 3-5-isothiourea propane sulfonate, hexamethylenetetraphthalic anhydride and sodium thiosulfate.

[0044] Preferably, in the primary mixed solution, the mass ratio of thiourea, 3-5-isothiourea propane sulfonate, hexamethylenetetraphthalic anhydride and sodium thiosulfate is (0.0008-0.001):(10-20):(1-2):(0.001-0.002), wherein the selection range of thiourea "0.0008-0.001" can be, for example, 0.0008, 0.0009 or 0.001, and the mass ratio of 3-5-isothiourea propane sulfonate is (0.0008-0.001):(10-20):(1-2):(0.001-0.002). The selection range of sulfonate "10-20" can be, for example, 10, 12, 14, 16, 18 or 20, the selection range of hexamethylenetetraphthalic anhydride "1-2" can be, for example, 1, 1.2, 1.4, 1.6, 1.8 or 2, and the selection range of sodium thiosulfate "0.001-0.002" can be, for example, 0.001, 0.0012, 0.0014, 0.0016, 0.0018 or 0.002, etc.

[0045] In the present invention, the wetting agent is a surfactant suitable for the coating environment, and illustratively, it may be sodium dodecylbenzene sulfonate or sodium dodecyl sulfate.

[0046] Preferably, the mass concentration of the wetting agent in the primary mixed liquid is 50-100 g / L, for example, it can be 50 g / L, 60 g / L, 70 g / L, 80 g / L, 90 g / L or 100 g / L.

[0047] Preferably, a brightener is also added during the primary mixing process, and the brightener includes copper sulfate and / or potassium iodate.

[0048] In the present invention, the nickel-phosphorus alloy layer is the middle coating layer, and the brightness requirement is not high. In order to achieve the purpose of minimizing the pollution of the downstream, copper sulfate and / or potassium iodate are used as brighteners. In addition, thiourea and sodium thiosulfate in the stabilizer can also produce a bright coating effect simultaneously.

[0049] Preferably, when the brightener is copper sulfate, the mass concentration of the brightener in the primary mixed solution is 10-20 mg / L, for example, 10 mg / L, 12 mg / L, 14 mg / L, 16 mg / L, 18 mg / L or 20 mg / L.

[0050] Preferably, when the brightener is potassium iodate, the mass concentration of the brightener in the primary mixed solution is 2-6 mg / L, for example, 2 mg / L, 3 mg / L, 4 mg / L, 5 mg / L or 6 mg / L.

[0051] Preferably, a pH buffer is also added during the primary mixing process.

[0052] Preferably, the pH buffer comprises any one of boric acid, glycolic acid, acetic acid, oxalic acid, succinic acid, aqueous ammonia, sodium hydroxide, potassium hydroxide or sodium bicarbonate, or a combination of at least two thereof, preferably boric acid or aqueous ammonia.

[0053] In the present invention, if it is necessary to adjust the pH value to a lower value, boric acid, glycolic acid, acetic acid, oxalic acid or succinic acid can be used, preferably 10-20 g / L (for example, 10 g / L, 15 g / L or 20 g / L, etc.) of boric acid, which is the concentration of boric acid added as a buffer to a mixed solution; if it is necessary to adjust the pH value to a higher value, ammonia water, sodium hydroxide, potassium hydroxide or sodium bicarbonate can be used, and ammonia water is preferred in view of the comprehensive cost.

[0054] It should be noted that the mass fraction of aqueous ammonia is not limited in the present invention, and by way of example, it may be 25-28%, such as 25%, 26%, 27% or 28%.

[0055] Preferably, the pH value of the primary mixed solution is 7.5-10, for example, it can be 7.5, 8, 8.5, 9, 9.5 or 10, etc., preferably 8-9.5.

[0056] As a preferred technical solution of the present invention, the volume ratio of the nickel plating solution, the primary mixed solution and the phosphorus plating solution is (0.8-1.2):(0.8-1.2):(0.8-1.2), wherein the selection range of the nickel plating solution "0.8-1.2" can be, for example, 0.8, 0.9, 1, 1.1 or 1.2, etc., the selection range of the primary mixed solution "0.8-1.2" can be, for example, 0.8, 0.9, 1, 1.1 or 1.2, etc., and the selection range of the phosphorus plating solution "0.8-1.2" can be, for example, 0.8, 0.9, 1, 1.1 or 1.2, etc.

[0057] Preferably, the pH value of the chemical plating solution in step (a) is 8-9.5, for example, it can be 8, 8.5, 9 or 9.5.

[0058] In the present invention, if the pH value of the chemical plating solution is too low, the reaction speed is slow and the deposition speed is low; if the pH value of the chemical plating solution is too high, the reaction is intense, the plating solution is boiling, the plating layer is rough, and dark gray nickel powder appears in the plating solution.

[0059] As a preferred technical solution of the present invention, the plating reaction in step (b) is accompanied by ultrasound, and the frequency of the ultrasound is 20-40KHz, for example, it can be 20KHz, 25KHz, 30KHz, 35KHz or 40KHz, etc., preferably 25-30KHz.

[0060] In the present invention, ultrasound is used for assistance, which has the following effects: 1) lowering the temperature of the plating solution, and plating can be started at a minimum of 30° C.; 2) increasing the deposition rate of the coating; 3) improving the quality of the coating.

[0061] It should be noted that, in order to prevent the chemical plating solution from being decomposed under the action of ultrasound, limiting the frequency of ultrasound to 20-40 KHz can alleviate the instability of the chemical plating solution.

[0062] Preferably, the temperature of the plating reaction in step (b) is 30-65°C, for example, 30°C, 40°C, 50°C, 60°C or 65°C, etc., preferably 40-55°C.

[0063] In the present invention, if the temperature of the plating reaction is too low, the reaction speed is slow and the deposition speed is low; if the temperature of the plating reaction is too high, the reaction is intense, the plating solution is boiling, the plating layer is rough, and dark gray nickel powder appears in the plating solution.

[0064] Preferably, during the plating reaction in step (b), the film drawing line speed is 3-6 m / min, for example, 3 m / min, 4 m / min, 5 m / min or 6 m / min.

[0065] In the present invention, the chemical nickel-phosphorus plating process lengthens the film drawing distance of the subsequent copper plating, so after the introduction of this process, the line speed should not be increased too fast, and it is best to maintain it at 3-6m / min. If the film drawing line speed is too slow, the overall efficiency will be reduced and the production capacity will be reduced; if the film drawing line speed is too fast, the film will not be formed in time, resulting in the thickness of the chemical plating layer not meeting the process requirements.

[0066] Preferably, the plating reaction time in step (b) is 0.5-3 min, for example, 0.5 min, 1 min, 1.5 min, 2 min, 2.5 min or 3 min.

[0067] In the present invention, if the plating reaction time is too long, the overall efficiency is reduced and the production capacity becomes smaller; if the plating reaction time is too short, the film is not formed in time, resulting in the thickness of the chemical plating layer failing to meet the process requirements.

[0068] Preferably, the step of preparing the sealing solution comprises: mixing a silane coupling agent, ethanol and water, and performing a hydrolysis treatment.

[0069] Preferably, the silane coupling agent includes glycidoxypropyltrimethoxysilane.

[0070] Preferably, the volume ratio of the silane coupling agent, ethanol and water is (40-50):(40-45):(5-20), wherein the selection range of the silane coupling agent "40-50" can be, for example, 40, 42, 44, 46, 48 or 50, etc., the selection range of ethanol "40-45" can be, for example, 40, 41, 42, 43, 44 or 45, etc., and the selection range of water "5-20" can be, for example, 5, 10, 15 or 20, etc.

[0071] Preferably, the temperature of the hydrolysis treatment is room temperature, and the time of the hydrolysis treatment is 70-80 hours, for example, it can be 70 hours, 72 hours, 75 hours, 78 hours or 80 hours.

[0072] It should be noted that the present invention does not limit the specific temperature of normal temperature. For example, it can be 25±5°C, such as 20°C, 25°C or 30°C.

[0073] Preferably, the sealing treatment time is 1-3 min, for example, 1 min, 1.5 min, 2 min, 2.5 min or 3 min.

[0074] As a preferred technical solution of the present invention, the double-sided copper plating method in step (4) includes a double-sided acid copper electroplating method.

[0075] Preferably, the post-treatment steps in step (4) include washing, anti-oxidation process, drying and winding processes performed in sequence.

[0076] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0077] (1) Unwinding the magnetron film and then washing it with water;

[0078] Wherein, the magnetron film is a base film coated with a copper layer with a thickness of 20-40nm on both sides;

[0079] (2) using a low-phosphorus weakly alkaline chemical nickel process to plate a nickel-phosphorus alloy layer on both sides of the magnetron film, the specific steps comprising:

[0080] (a) heating and dissolving a nickel salt in water at 60-80° C. to obtain a nickel salt solution with a concentration of 20-40 g / L; preparing a phosphate salt solution with a concentration of 10-40 g / L; wherein the mass ratio of nickel ions in the nickel salt solution to phosphate ions in the phosphate salt solution is (0.3-0.6):1;

[0081] The coordination compound, the accelerator, the stabilizer, the wetting agent, the brightener and the pH buffer are mixed once to obtain a primary mixed solution with a pH value of 7.5-10, and then the primary mixed solution and the nickel salt solution are mixed twice to obtain a secondary mixed solution, and then the secondary mixed solution and the phosphate salt solution are mixed three times to obtain a chemical plating solution with a pH value of 8-9.5;

[0082] Wherein, in the first mixed solution, the coordination compound includes lactic acid solution, ammonium salt, citrate and potassium pyrophosphate in a mass ratio of (5-20):(20-50):(20-50):(30-50); the accelerator is ammonia water, and the mass concentration of ammonia water in the first mixed solution is 10-30g / L; in the first mixed solution, the stabilizer includes thiourea, 3- 5-isothiourea salt propane sulfonate, hexamethylenetetraphthalic anhydride and sodium thiosulfate; the mass concentration of the wetting agent in the primary mixed solution is 50-100 g / L; in the primary mixed solution, the brightener is copper sulfate with a mass concentration of 10-20 mg / L or potassium iodate with a mass concentration of 2-6 mg / L; the pH buffer is boric acid or ammonia water; the volume ratio of the nickel salt solution, the primary mixed solution and the phosphate solution is (0.8-1.2):(0.8-1.2):(0.8-1.2);

[0083] (b) placing the magnetron film in the chemical plating solution and performing a plating reaction at 30-65° C. for 0.5-3 min to obtain a nickel-phosphorus alloy layer;

[0084] The plating reaction is accompanied by ultrasound, and the frequency of the ultrasound is 20-40KHz; during the plating reaction, the film drawing line speed is 3-6m / min;

[0085] (3) sealing the composite membrane obtained in step (2) by using a silane sealing process, the specific steps comprising:

[0086] (c) mixing a silane coupling agent, ethanol and water in a volume ratio of (40-50):(40-45):(5-20) at room temperature, and performing a hydrolysis treatment for 70-80 hours under stirring conditions to obtain a sealing solution;

[0087] (d) immersing the composite membrane obtained in step (2) in the sealing solution for 1-3 minutes;

[0088] (4) After the sealing treatment, the composite membrane is washed with water, and then subjected to a double-sided electroplating process of acid copper, and then subjected to a double countercurrent washing process, an anti-oxidation process, a drying process and a winding process in sequence, wherein the winding process includes slitting, to obtain the composite current collector.

[0089] It should be noted that double countercurrent water washing refers to using two water washing tanks for water washing, the second water washing tank enters with fresh water flowing to the first water washing tank, and the first water washing tank (i.e. the first membrane-entering water washing tank) discharges dirty water.

[0090] In a second aspect, the present invention provides a composite current collector prepared by the preparation method described in the first aspect, wherein the elongation of the composite current collector in the MD direction is ≥9%, for example, it can be 9%, 10%, 11% or 12%, and the elongation in the TD direction is ≥5%, for example, it can be 5%, 9%, 10%, 11% or 12%, etc.

[0091] It should be noted that the MD direction refers to the length direction of the film, that is, along the machine direction, and the TD direction refers to the width direction.

[0092] Preferably, the square resistance of the composite current collector is ≤2Ω, for example, it can be 2Ω, 1.5Ω, 1Ω or 0.5Ω.

[0093] In a third aspect, the present invention provides a secondary battery, wherein the secondary battery comprises a composite current collector prepared by the preparation method as described in the first aspect, or comprises a composite current collector as described in the second aspect.

[0094] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0095] Compared with the prior art, the present invention has the following beneficial effects:

[0096] The present invention introduces a chemical nickel-phosphorus plating process and a silane sealing process before copper plating the magnetron film, which, on the one hand, increases the density and adhesion of the film surface and improves the qualified rate of the composite current collector, and on the other hand, reduces the requirements for the thickness and square resistance of the magnetron film layer, with the square resistance being below 2Ω and the thickness being 20-40nm, thereby reducing the total energy and process difficulty of the magnetron coating production process and simultaneously reducing the probability of holes in the magnetron film. DETAILED DESCRIPTION

[0097] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0098] Example 1

[0099] This embodiment provides a method for preparing a composite current collector, which has the following disadvantages:

[0100] (1) Unwinding the magnetron film and then washing it with water;

[0101] The magnetron film is a base film coated with a 40nm thick copper layer on both sides, the base film is a PP film, and the square resistance of the magnetron film is 1.5Ω;

[0102] (2) using a low-phosphorus weakly alkaline chemical nickel process to plate a nickel-phosphorus alloy layer on at least one side of the magnetron film, the specific steps comprising:

[0103] (a) using 1 / 3 of the total volume of water in the preparation tank to heat and dissolve nickel salt (nickel chloride) at a heating temperature of 70° C. to obtain a nickel salt solution with a concentration of 30 g / L; using 1 / 3 of the water in the main tank to dissolve phosphate salt (sodium hypophosphite monohydrate) to prepare a phosphate solution with a concentration of 25 g / L; the mass ratio of nickel ions in the nickel salt solution to phosphate ions in the phosphate solution is 0.45:1;

[0104] The coordination compound, accelerator, stabilizer, wetting agent, brightener and pH buffer are mixed once in the main tank with 1 / 3 of the total volume of the preparation tank to obtain a primary mixed solution with a pH value of 8.5, and then the primary mixed solution is added to the nickel salt solution under stirring conditions for secondary mixing to obtain a secondary mixed solution, and then the secondary mixed solution and the phosphate salt solution after stirring and filtering are mixed three times, and diluted to the total volume of the main tank to obtain a chemical plating solution with a pH value of 8;

[0105] Wherein, in the primary mixed solution, the coordination compound includes lactic acid solution (mass fraction is 80%), ammonium sulfate, ammonium citrate and potassium pyrophosphate in a mass ratio of 5:35:35:40; the accelerator is ammonia water, and the mass concentration of ammonia water in the primary mixed solution is 20g / L; in the primary mixed solution, the stabilizer includes thiourea, 3-5 isothiourea propane sulfonate, hexamethylenetetraphthalic anhydride and sodium thiosulfate in a mass ratio of 0.0009:15:1.5:0.0015; the mass concentration of the wetting agent in the primary mixed solution is 75g / L, and the wetting agent is sodium dodecylbenzene sulfonate; in the primary mixed solution, the brightener is copper sulfate with a mass concentration of 15mg / L; the pH buffer is boric acid; the volume ratio of the nickel salt solution, the primary mixed solution and the phosphate solution is 1:1:1;

[0106] (b) placing the magnetron film in the chemical plating solution, turning on the ultrasonic equipment, and performing a plating reaction at 45° C. for 1.5 min to obtain a nickel-phosphorus alloy layer;

[0107] The frequency of the ultrasonic equipment is 30KHz, and during the plating reaction, the film drawing line speed is 4.5m / min;

[0108] (3) sealing the composite membrane obtained in step (2) by using a silane sealing process, the specific steps comprising:

[0109] (c) mixing a silane coupling agent (glycidoxypropyltrimethoxysilane), ethanol and water in a volume ratio of 45:45:10 at room temperature (i.e., 25° C.), and performing a hydrolysis treatment for 72 hours under stirring conditions to obtain a sealing solution;

[0110] (d) immersing the composite membrane obtained in step (2) in the sealing solution for 2 minutes;

[0111] (4) After the sealing treatment, the composite membrane is washed with pure water, and then subjected to a double-sided electroplating process of acid copper, and then sequentially subjected to a double countercurrent washing process, an anti-oxidation process, a drying process and a winding process, wherein the winding process includes slitting, to obtain the composite current collector.

[0112] Example 2

[0113] This embodiment provides a method for preparing a composite current collector, which has the following disadvantages:

[0114] (1) Unwinding the magnetron film and then washing it with water;

[0115] The magnetron film is a base film coated with a 40nm thick copper layer on both sides, the base film is a PP film, and the square resistance of the magnetron film is 1.5Ω;

[0116] (2) using a low-phosphorus weakly alkaline chemical nickel process to plate a nickel-phosphorus alloy layer on both sides of the magnetron film, the specific steps comprising:

[0117] (a) using 1 / 3 of the total volume of water in the preparation tank to heat and dissolve nickel salt (nickel chloride) at a temperature of 60° C. to obtain a nickel salt solution with a concentration of 20 g / L; using 1 / 3 of the water in the main tank to dissolve phosphate salt (sodium hypophosphite monohydrate) to prepare a phosphate solution with a concentration of 10 g / L; the mass ratio of nickel ions in the nickel salt solution to phosphate ions in the phosphate solution is 0.6:1;

[0118] The coordination compound, accelerator, stabilizer, wetting agent, brightener and pH buffer are mixed once in the main tank with 1 / 3 of the total volume of the preparation tank to obtain a primary mixed solution with a pH value of 9, and then the primary mixed solution is added to the nickel salt solution under stirring conditions for secondary mixing to obtain a secondary mixed solution, and then the secondary mixed solution and the phosphate salt solution after stirring and filtering are mixed three times, and diluted to the total volume of the main tank to obtain a chemical plating solution with a pH value of 8.5;

[0119] Wherein, in the primary mixed solution, the coordination compound includes lactic acid solution (mass fraction is 80%), ammonium sulfate, ammonium citrate and potassium pyrophosphate in a mass ratio of 5:20:20:30; the accelerator is ammonia water, and the mass concentration of ammonia water in the primary mixed solution is 10g / L; in the primary mixed solution, the stabilizer includes thiourea, 3-5 isothiouronium salt propane sulfonate, hexamethylenetetraphthalic anhydride and sodium thiosulfate in a mass ratio of 0.0008:10:1:0.001; the mass concentration of the wetting agent in the primary mixed solution is 50g / L, and the wetting agent is sodium dodecylbenzene sulfonate; in the primary mixed solution, the brightener is potassium iodate with a mass concentration of 4mg / L; the pH buffer is boric acid; the volume ratio of the nickel salt solution, the primary mixed solution and the phosphate solution is 1:1:1;

[0120] (b) placing the magnetron film in the chemical plating solution, turning on the ultrasonic equipment, and performing a plating reaction at 30° C. for 0.5 min to obtain a nickel-phosphorus alloy layer;

[0121] The frequency of the ultrasonic equipment is 20KHz, and during the plating reaction, the film drawing line speed is 3m / min;

[0122] (3) sealing the composite membrane obtained in step (2) by using a silane sealing process, the specific steps comprising:

[0123] (c) mixing a silane coupling agent (glycidoxypropyltrimethoxysilane), ethanol and water in a volume ratio of 40:40:20 at room temperature (i.e., 25° C.), and performing a hydrolysis treatment for 70 hours under stirring conditions to obtain a sealing solution;

[0124] (d) immersing the composite membrane obtained in step (2) in the sealing solution for 1 min;

[0125] (4) After the sealing treatment, the composite membrane is washed with pure water, and then subjected to a double-sided electroplating process of acid copper, and then sequentially subjected to a double countercurrent washing process, an anti-oxidation process, a drying process and a winding process, wherein the winding process includes slitting, to obtain the composite current collector.

[0126] Example 3

[0127] This embodiment provides a method for preparing a composite current collector, which has the following disadvantages:

[0128] (1) Unwinding the magnetron film and then washing it with water;

[0129] The magnetron film is a base film coated with a 40nm thick copper layer on both sides, the base film is a PP film, and the square resistance of the magnetron film is 1.5Ω;

[0130] (2) using a low-phosphorus weakly alkaline chemical nickel process to plate a nickel-phosphorus alloy layer on both sides of the magnetron film, the specific steps comprising:

[0131] (a) using 1 / 3 of the total volume of water in the preparation tank to heat and dissolve nickel salt (nickel chloride) at a heating temperature of 80° C. to obtain a nickel salt solution with a concentration of 40 g / L; using 1 / 3 of the water in the main tank to dissolve phosphate salt (sodium hypophosphite monohydrate) to prepare a phosphate solution with a concentration of 40 g / L; the mass ratio of nickel ions in the nickel salt solution to phosphate ions in the phosphate solution is 0.3:1;

[0132] The coordination compound, accelerator, stabilizer, wetting agent, brightener and pH buffer are mixed once in the main tank with 1 / 3 of the total volume of the preparation tank to obtain a primary mixed solution with a pH value of 9.5, and then the primary mixed solution is added to the nickel salt solution under stirring conditions for secondary mixing to obtain a secondary mixed solution, and then the secondary mixed solution and the phosphate salt solution after stirring and filtering are mixed three times, and diluted to the total volume of the main tank to obtain a chemical plating solution with a pH value of 9;

[0133] Wherein, in the primary mixed solution, the coordination compound includes lactic acid solution (mass fraction is 80%), ammonium sulfate, ammonium citrate and potassium pyrophosphate in a mass ratio of 20:50:50:50; the accelerator is ammonia water, and the mass concentration of ammonia water in the primary mixed solution is 30g / L; in the primary mixed solution, the stabilizer includes thiourea, 3-5 isothiouronium salt propane sulfonate, hexamethylenetetraphthalic anhydride and sodium thiosulfate in a mass ratio of 0.001:20:2:0.002; the mass concentration of the wetting agent in the primary mixed solution is 100g / L, and the wetting agent is sodium dodecylbenzene sulfonate; in the primary mixed solution, the brightener is copper sulfate with a mass concentration of 15mg / L; the pH buffer is boric acid; the volume ratio of the nickel salt solution, the primary mixed solution and the phosphate solution is 1:1:1;

[0134] (b) placing the magnetron film in the chemical plating solution, turning on the ultrasonic equipment, and performing a plating reaction at 65° C. for 3 min to obtain a nickel-phosphorus alloy layer;

[0135] The frequency of the ultrasonic equipment is 40KHz, and during the plating reaction, the film drawing line speed is 6m / min;

[0136] (3) sealing the composite membrane obtained in step (2) by using a silane sealing process, the specific steps comprising:

[0137] (c) mixing a silane coupling agent (glycidoxypropyltrimethoxysilane), ethanol and water in a volume ratio of 50:45:5 at room temperature (i.e., 25° C.), and performing a hydrolysis treatment for 80 hours under stirring conditions to obtain a sealing solution;

[0138] (d) immersing the composite membrane obtained in step (2) in the sealing solution for 3 minutes;

[0139] (4) After the sealing treatment, the composite membrane is washed with pure water, and then subjected to a double-sided electroplating process of acid copper, and then sequentially subjected to a double countercurrent washing process, an anti-oxidation process, a drying process and a winding process, wherein the winding process includes slitting, to obtain the composite current collector.

[0140] Example 4

[0141] The difference between this embodiment and embodiment 1 is that in step (a), the mass ratio of nickel ions in the nickel salt solution to phosphate ions in the phosphate salt solution is 0.2:1.

[0142] The rest of the preparation methods and parameters were the same as those in Example 1.

[0143] Example 5

[0144] The difference between this embodiment and embodiment 1 is that in step (a), the mass ratio of nickel ions in the nickel salt solution to phosphate ions in the phosphate salt solution is 0.7:1.

[0145] The rest of the preparation methods and parameters were the same as those in Example 1.

[0146] Example 6

[0147] The difference between this embodiment and embodiment 1 is that the pH value of the chemical plating solution in step (a) is 7.

[0148] The rest of the preparation methods and parameters were the same as those in Example 1.

[0149] Example 7

[0150] The difference between this embodiment and embodiment 1 is that the pH value of the chemical plating solution in step (a) is 10.

[0151] The rest of the preparation methods and parameters were the same as those in Example 1.

[0152] Example 8

[0153] The difference between this embodiment and embodiment 1 is that no ultrasonic equipment is provided in step (b), that is, no ultrasonic treatment is performed during the plating reaction.

[0154] The rest of the preparation methods and parameters were the same as those in Example 1.

[0155] Example 9

[0156] The difference between this embodiment and embodiment 1 is that the temperature of the plating reaction in step (b) is 20° C. The rest of the preparation method and parameters are the same as those in embodiment 1.

[0157] Example 10

[0158] The difference between this embodiment and embodiment 1 is that the temperature of the plating reaction in step (b) is 70° C. The rest of the preparation method and parameters are the same as those in embodiment 1.

[0159] Embodiment 11

[0160] The difference between this embodiment and embodiment 1 is that the film drawing line speed in step (b) is 2 m / min. The other preparation methods and parameters are the same as those in embodiment 1.

[0161] Example 12

[0162] The difference between this embodiment and embodiment 1 is that the film drawing line speed in step (b) is 7 m / min. The other preparation methods and parameters are the same as those in embodiment 1.

[0163] Embodiment 13

[0164] The difference between this embodiment and embodiment 1 is that the plating reaction time in step (b) is 10 seconds. The rest of the preparation method and parameters are the same as those in embodiment 1.

[0165] Embodiment 14

[0166] The difference between this embodiment and embodiment 1 is that the plating reaction time in step (b) is 5 minutes. The other preparation methods and parameters are the same as those in embodiment 1.

[0167] Comparative Example 1

[0168] The difference between this comparative example and Example 1 is that step (2) is not performed.

[0169] The rest of the preparation methods and parameters were the same as those in Example 1.

[0170] Comparative Example 2

[0171] The difference between this comparative example and Example 1 is that step (3) is not performed.

[0172] The rest of the preparation methods and parameters were the same as those in Example 1.

[0173] Comparative Example 3

[0174] The difference between this comparative example and Example 1 is that steps (2) and (3) are not performed.

[0175] The rest of the preparation methods and parameters were the same as those in Example 1.

[0176] Performance Testing

[0177] The density and elongation of the composite current collectors prepared in the above examples and comparative examples were tested.

[0178] Density testing method: In a dark room, place the composite current collector sample prepared as above close to an ordinary flat backlight (brightness is 1200mL), the length and width of the sample is larger than the backlight board by 30cm*30cm, and photos taken at a vertical angle show that the light-transmitting area is the non-dense area, and the opaque area is the dense area of ​​the copper layer; Density = area of ​​the dense area of ​​the copper layer / area of ​​the backlight board ≥90% is qualified.

[0179] Elongation test method: bake the composite current collector at 150℃ for 3min, cut into 15mm wide copper film strips in MD or TD direction, the edge of the strip to be tested should not have gaps, burrs, and soft or hard defects on the film surface. Set the running speed of the tensile testing machine to 50mm / min and the stretching distance to 50mm, place the copper film strip of the sample to be tested in the upper and lower chucks, so that the copper film strip is clamped and tensioned on the tensile testing machine, and perform tensile testing: the elongation in MD or TD direction ≥3% is qualified.

[0180] The test results are shown in Table 1.

[0181] Table 1

[0182]

[0183] analyze:

[0184] It can be seen from the above table that the present invention introduces a chemical nickel-phosphorus plating process and a silane sealing process before copper plating the magnetron film. On the one hand, the density and adhesion of the film surface are increased, and the qualified rate of the composite current collector is improved. On the other hand, the requirements for the thickness and square resistance of the magnetron film layer are reduced. The square resistance is below 2Ω and the thickness is 20-40nm, which reduces the total energy and process difficulty of the magnetron coating production process, and simultaneously reduces the probability of holes in the magnetron film.

[0185] It can be seen from Example 1 and Examples 4-5 that if the mass ratio of nickel ions in the nickel plating solution to phosphate ions in the phosphorus plating solution is too small or too large, the plating rate of the nickel-phosphorus alloy layer will be low and the coating will be dark, resulting in the chemical plating layer being too thin and insufficiently dense.

[0186] It can be seen from Example 1 and Examples 6-7 that if the pH value of the chemical plating solution is too low, the chemical plating layer will be too thin and not dense enough; if the pH value of the chemical plating solution is too high, the reaction will be too intense, the chemical plating layer will be rough, and also not dense enough.

[0187] It can be seen from Example 1 and Example 8 that if ultrasonic treatment is not performed during the plating reaction, the chemical plating layer will be too thin and not dense enough.

[0188] It can be seen from Examples 1 and 9-10 that if the temperature of the plating reaction is too low, the chemical plating layer will be too thin and not dense enough; if the temperature of the plating reaction is too high, the reaction will be too intense, the chemical plating layer will be rough, and also not dense enough.

[0189] It can be seen from Example 1 and Examples 11-12 that if the film drawing speed is too slow, the efficiency will be reduced; if the film drawing speed is too fast, the chemical plating layer will be too thin and the density will be insufficient.

[0190] It can be seen from Example 1 and Examples 13-14 that if the plating reaction time is too long, the efficiency will be reduced; if the plating reaction time is too short, the chemical plating layer will be too thin and the density will be insufficient.

[0191] It can be seen from Example 1 and Comparative Example 1 that if the nickel-phosphorus alloy layer is not plated on both surfaces of the magnetron film using the chemical nickel-phosphorus plating process, the density is insufficient.

[0192] It can be seen from Example 1 and Comparative Example 2 that if the silane sealing process is not used for sealing, the density is insufficient.

[0193] It can be seen from Example 1 and Comparative Example 3 that if the chemical nickel-phosphorus plating process and the silane sealing process are not adopted, the density is insufficient and the elongation cannot be significantly improved.

[0194] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a composite current collector, characterized in that: The preparation method comprises the following steps: (1) Unwinding the magnetron film and performing pretreatment; (2) plating a nickel-phosphorus alloy layer on both sides of the magnetron film using a chemical nickel-phosphorus plating process; (3) using a silane sealing process to seal the composite membrane obtained in step (2), wherein the specific steps of the silane sealing process include: The obtained composite membrane is sealed with a sealing solution; (4) copper plating is performed on both sides of the composite film after the sealing treatment, and then post-treatment is performed to obtain the composite current collector.

2. The preparation method according to claim 1, characterized in that: The pre-treatment step in step (1) includes water washing; The magnetron film in step (1) comprises a base film and a copper layer disposed on both sides of the base film; The sheet resistance of both sides of the magnetron film in step (1) is 1-2Ω; The thickness of the copper layer on one side is 20-40 nm.

3. The preparation method according to claim 1, characterized in that: The chemical nickel-phosphorus plating process in step (2) is a low-phosphorus weak alkaline chemical nickel process, and the specific steps of the low-phosphorus weak alkaline chemical nickel process include: (a) mixing a nickel plating solution, a coordination compound, an accelerator, a stabilizer, a wetting agent and a phosphorus plating solution to obtain a chemical plating solution; (b) placing the magnetron film in the chemical plating solution to perform a plating reaction to obtain a nickel-phosphorus alloy layer.

4. The preparation method according to claim 3, characterized in that: The nickel plating solution in step (a) comprises a nickel salt, and the nickel salt comprises any one of nickel chloride, nickel sulfate or nickel acetate, or a combination of at least two thereof; The concentration of the nickel plating solution in step (a) is 20-40 g / L; The phosphorus plating solution in step (a) comprises a phosphorus salt, and the phosphorus salt comprises sodium hypophosphite monohydrate and / or sodium dihydrogen phosphate; The concentration of the phosphorus plating solution in step (a) is 10-40 g / L; The mass ratio of nickel ions in the nickel plating solution of step (a) to phosphate ions in the phosphorus plating solution is (0.3-0.6):

1.

5. The preparation method according to claim 3, characterized in that: The specific steps of mixing in step (a) include: The coordination compound, the accelerator, the stabilizer and the wetting agent are mixed once to obtain a primary mixed solution, the primary mixed solution and the nickel plating solution are mixed twice to obtain a secondary mixed solution, and the secondary mixed solution and the phosphorus plating solution are mixed three times; The coordination compound includes any one of ammonium salt, citrate or potassium pyrophosphate or a combination of at least two thereof; The coordination compound also includes a lactic acid solution; The accelerator includes any one or a combination of at least two of ammonia, fatty acid, propionic acid, succinic acid, malic acid, triethanolamine, fluoride or lithium salt; The mass concentration of the accelerator in the primary mixed solution is 10-30 g / L; The stabilizer includes any one of thiourea, 3-5-isothiourea propane sulfonate, phthalic anhydride, hexamethylenetetraphthalic anhydride, mercaptobenzothiazole, xanthate or sodium thiosulfate, or a combination of at least two thereof; The mass concentration of the wetting agent in the primary mixed solution is 50-100 g / L; A brightener is also added during the primary mixing process, wherein the brightener includes copper sulfate and / or potassium iodate; A pH buffer is also added during the primary mixing process; The pH value of the primary mixed solution is 7.5-10.

6. The preparation method according to claim 5, characterized in that: The volume ratio of the nickel plating solution, the primary mixed solution and the phosphorus plating solution is (0.8-1.2):(0.8-1.2):(0.8-1.2); The pH value of the chemical plating solution in step (a) is 8-9.

5.

7. The preparation method according to claim 3, characterized in that: The plating reaction in step (b) is accompanied by ultrasound, and the frequency of the ultrasound is 20-40KHz; The temperature of the plating reaction in step (b) is 30-65° C.; During the plating reaction in step (b), the film drawing line speed is 3-6 m / min; The plating reaction time in step (b) is 0.5-3 minutes.

8. The preparation method according to claim 1, characterized in that: The steps of preparing the sealing solution include: mixing a silane coupling agent, ethanol and water, and performing a hydrolysis treatment; The volume ratio of the silane coupling agent, ethanol and water is (40-50):(40-45):(5-20); The temperature of the hydrolysis treatment is room temperature, and the time of the hydrolysis treatment is 70-80 hours; The sealing treatment time is 1-3 minutes.

9. The preparation method according to claim 1, characterized in that: The double-sided copper plating method in step (4) includes a double-sided acid copper plating method; Preferably, the post-treatment steps in step (4) include washing, anti-oxidation process, drying and winding processes performed in sequence.

10. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: (1) Unwinding the magnetron film and then washing it with water; Wherein, the magnetron film is a base film coated with a copper layer with a thickness of 20-40nm on both sides; (2) using a low-phosphorus weakly alkaline chemical nickel process to plate a nickel-phosphorus alloy layer on both sides of the magnetron film, the specific steps comprising: (a) heating and dissolving a nickel salt in water at 60-80° C. to obtain a nickel salt solution with a concentration of 20-40 g / L; preparing a phosphate salt solution with a concentration of 10-40 g / L; wherein the mass ratio of nickel ions in the nickel salt solution to phosphate ions in the phosphate salt solution is (0.3-0.6):1; The coordination compound, the accelerator, the stabilizer, the wetting agent, the brightener and the pH buffer are mixed once to obtain a primary mixed solution with a pH value of 7.5-10, and then the primary mixed solution and the nickel salt solution are mixed twice to obtain a secondary mixed solution, and then the secondary mixed solution and the phosphate salt solution are mixed three times to obtain a chemical plating solution with a pH value of 8-9.5; Wherein, in the first mixed solution, the coordination compound includes lactic acid solution, ammonium salt, citrate and potassium pyrophosphate in a mass ratio of (5-20):(20-50):(20-50):(30-50); the accelerator is ammonia water, and the mass concentration of ammonia water in the first mixed solution is 10-30g / L; in the first mixed solution, the stabilizer includes thiourea, 3- 5 isothiouronium salt propane sulfonate, hexamethylenetetraphthalic anhydride and sodium thiosulfate; the mass concentration of the wetting agent in the primary mixed solution is 50-100g / L; in the primary mixed solution, the brightener is copper sulfate with a mass concentration of 10-20mg / L or potassium iodate with a mass concentration of 2-6mg / L; the pH buffer is boric acid or ammonia water; the volume ratio of the nickel salt solution, the primary mixed solution and the phosphate solution is (0.8-1.2):(0.8-1.2):(0.8-1.2); (b) placing the magnetron film in the chemical plating solution and performing a plating reaction at 30-65° C. for 0.5-3 min to obtain a nickel-phosphorus alloy layer; The plating reaction is accompanied by ultrasound, and the frequency of the ultrasound is 20-40 KHz; during the plating reaction, the film drawing line speed is 3-6 m / min; (3) sealing the composite membrane obtained in step (2) by using a silane sealing process, the specific steps comprising: (c) mixing a silane coupling agent, ethanol and water in a volume ratio of (40-50):(40-45):(5-20) at room temperature, and performing a hydrolysis treatment for 70-80 hours under stirring conditions to obtain a sealing solution; (d) immersing the composite membrane obtained in step (2) in the sealing solution for 1-3 minutes; (4) After the sealing treatment, the composite membrane is washed with water, and then subjected to a double-sided electroplating process of acid copper, and then subjected to a double countercurrent washing process, an anti-oxidation process, a drying process and a winding process in sequence, wherein the winding process includes slitting, to obtain the composite current collector.

11. A composite current collector prepared by the preparation method according to any one of claims 1 to 10, characterized in that: The elongation of the composite current collector in the MD direction is ≥9%, and the elongation in the TD direction is ≥5%; The square resistance of the composite current collector is ≤2Ω.

12. A secondary battery, characterized in that: The secondary battery comprises the composite current collector prepared by the preparation method according to any one of claims 1 to 10, or comprises the composite current collector according to claim 11.

Citation Information

Cited By

  • Composite current collector, preparation method therefor, and secondary battery

    WO2026036833A1