High-strength foamy copper and preparation method thereof
By optimizing the preparation method of copper foam, adopting a high porosity structure and a specific electroplating process, the pollution and mechanical property problems in the existing copper foam preparation process have been solved, and high-strength and high-conductivity copper foam materials have been realized.
Patent Information
- Application Number
- CN202411208499.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
Existing methods for preparing copper foam suffer from serious pollution, high costs, cumbersome processes, and poor mechanical properties.
High-strength copper foam with a porosity >95% is used. Impurities in the template matrix are removed through pretreatment, and the graphene mixture is immersed in ultrasonic-assisted stirring. Copper ions are deposited and the template matrix is removed by electroplating. Specific electroplating solutions and additives are used to optimize the electroplating process.
It improves the mechanical strength and conductivity of copper foam, reduces production costs, ensures uniformity and adhesion during the electroplating process, and is suitable for high-performance applications.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-strength copper foam preparation, in particular to high-strength copper foam and a preparation method thereof. Background Art
[0002] In the negative electrode of lithium batteries, copper foam acts as both a carrier of negative electrode active materials and a negative electrode electron collector and conductor, which collects the current generated by the active substances in the battery to generate a larger output current. The specific surface area advantage of copper foam can increase the amount of active substances contained in the battery per unit volume and improve the battery energy density. As a new type of negative electrode material, it has broad application prospects in lithium-ion batteries and can effectively alleviate the problem of separation between negative electrode materials and current collectors, thereby extending the cycle life of batteries. Copper foam also has good electrical conductivity, thermal conductivity, machinability, mature manufacturing technology, and outstanding cost advantages. It will become the preferred material for negative electrode current collectors of lithium batteries.
[0003] In view of the above-mentioned related technologies, the inventors found that the existing use of polyurethane foam for metallization pretreatment and chemical copper plating process results in large wastewater pollution, high investment costs, and complicated processes. At the same time, the SPS precursor for preparing foam copper needs to be sintered and removed. The removal process uses a temperature higher than 700°C, which changes the crystallization mode of the foam copper after electrodeposition, thereby reducing the mechanical properties of the foam copper material. Summary of the invention
[0004] In order to improve the defect of poor mechanical properties of the currently produced copper foam, the present application provides a high-strength copper foam and a preparation method thereof.
[0005] In a first aspect, the present application provides a high-strength copper foam, which adopts the following technical solution: A high-strength copper foam, wherein the porosity of the copper foam is greater than 95%.
[0006] Through the above technical scheme, the present application further limits the porosity of high-strength copper foam. By designing it into a structure with a porosity > 95%, the density of the material is reduced, thereby reducing the weight of the overall product without sacrificing mechanical strength, further meeting the needs of application scenarios of copper foam materials in lithium battery materials.
[0007] In a second aspect, the present application provides a method for preparing high-strength copper foam, using the following technical solution: A method for preparing high-strength copper foam includes the following technical solutions: Taking the template substrate and pre-treating the surface thereof, washing and drying the template substrate, and collecting the pre-treated template substrate; The pre-treated template substrate is immersed in the graphene mixed solution, and stirred and mixed and wetted under ultrasonic assisted treatment; After the infiltration is completed, the infiltrated template substrate is placed in an electroplating solution, electroplated, washed, dried, and the foamed copper substrate is collected; The foam copper substrate is then placed in a template substrate removal liquid, immersed and dissolved, and then washed and dried to prepare the high-strength foam copper.
[0008] Through the above technical solution, the present application optimizes the preparation method of high-strength copper foam, first removes impurities on the surface of the template matrix through pretreatment, and significantly improves its surface activity. This treatment step can enhance the adhesion during the subsequent infiltration and electroplating process, and ensure the integrity and uniformity of the copper plating layer.
[0009] Secondly, ultrasonic-assisted stirring promotes the full infiltration of the graphene mixture and the template matrix. The infiltrated mixture not only maintains the high strength and high conductivity of graphene, but also utilizes the excellent elasticity and adhesion of polyurethane materials, providing a good foundation for the subsequent electroplating process.
[0010] Finally, during the electroplating process, the present invention deposits copper ions evenly on the template surface to form a dense copper layer, ensuring the strength and durability of the copper foam. Then, by removing the template matrix, the high-strength copper foam obtained has excellent porosity and strength, and is suitable for a variety of high-performance applications.
[0011] Furthermore, the template matrix comprises a polyurethane foam matrix material with a pore size of 40-60 PPI.
[0012] Through the above technical solution, the present application adopts a polyurethane foam material with a pore size of 40-60 PPI, which provides an ideal structural basis. The selection of this pore size range ensures the formation of a uniform coating during the electroplating process while maintaining the lightweight characteristics of the foam. The elasticity and chemical resistance of the polyurethane material enable it to withstand the necessary physical and chemical pressures during the dipping and electroplating processes, ensuring the integrity and performance of the final foam copper. The selection of this specific template material can also minimize defects during electroplating and improve the mechanical strength and stability of the foam copper.
[0013] Further, the surface pretreatment adopts the following scheme: Taking the template substrate and placing it in a sodium hydroxide solution for soaking treatment; After the soaking is completed, deionized water is used for rinsing and soaking until the pH value of the washing solution is 6-7, and then the template matrix is removed and dried at room temperature.
[0014] Through the above technical scheme, the present application can effectively remove the oil and impurities of the template matrix by soaking in sodium hydroxide solution, and significantly improve its surface activity. Such treatment ensures that in the subsequent infiltration and electroplating process, the template matrix can form good adhesion with the copper plating layer, reducing the probability of defects that may occur during the electroplating process. By rinsing the template matrix to a pH value of 6-7, the stability of its surface chemical environment can be ensured, and the abnormal electroplating reaction caused by too high or too low pH value can be avoided. This series of processing steps ultimately provides a good foundation for electroplating, ensures the high quality and uniformity of the foamed copper, and improves its reliability and performance in practical applications.
[0015] Furthermore, the electroplating solution includes the following substances in parts by weight: 15-25 parts of copper sulfate pentahydrate; Sulfuric acid 5.5-7.0 parts; 2.5-8.0 parts of hydrochloric acid.
[0016] Through the above technical solution, the present application optimizes the composition ratio of the electroplating solution, improves the electroplating efficiency, reduces deposition defects, and further improves the physical and chemical properties of the copper layer, such as corrosion resistance and conductivity, through the rationally proportioned electroplating solution. The use of this electroplating solution ensures that the final product performs well in a variety of high-demand applications, broadens the scope of application of foamed copper, and makes its application in high-end manufacturing, new energy, and electronic devices more reliable.
[0017] Furthermore, the electroplating further comprises a plating treatment agent, and the plating treatment agent comprises the following substances in parts by weight: 15-30 parts of sodium polydipropane disulfide sulfonate; Fatty amine ethoxylate AESS 180-220 parts; Thiamidopropane disulfide sulfonic acid 15-25 parts.
[0018] Through the above technical solution, the present application adds sodium polydisulfide propane sulfonate, fatty amine ethoxy sulfonate and thiazolinyl disulfide propane sulfonic acid as additives during the electroplating process. Sodium polydisulfide propane sulfonate and fatty amine ethoxy sulfonate are used as brighteners and leveling agents, which can effectively improve the brightness and leveling of the coating; and thiazolinyl disulfide propane sulfonic acid is used as a strong leveling agent, and its grain refining effect can significantly improve the hardness of the foamed copper.
[0019] Furthermore, the template matrix removing liquid includes one or more of acetone, N-methylpyrrolidone, dimethylformamide, methanol, and ethanol.
[0020] Through the above technical solution, the present application optimizes the template matrix removal liquid so that it can effectively remove the foam matrix while taking into account good solubility and selectivity, and does not damage the foam copper structure that has been formed. This efficient removal process ensures the integrity of the pore structure of the foam copper and improves the strength and stability of the material. In addition, the ability to quickly dissolve the template matrix can significantly improve production efficiency, reduce production costs, and ensure the consistency of product quality.
[0021] Furthermore, the voltage of the electroplating treatment is 1-2V, and the electroplating time is 30-60min.
[0022] Through the above technical solution, the present application optimizes the electroplating voltage and electroplating time. By adjusting to moderate voltage and time, it can promote the stable deposition of copper ions to form a dense and uniform coating, thereby improving the strength and conductivity of foamed copper.
[0023] In summary, this application has the following beneficial effects: First, the present application optimizes the preparation method of high-strength copper foam by removing impurities on the surface of the template substrate through pretreatment, significantly improving its surface activity. This treatment step can enhance the adhesion during subsequent wetting and electroplating processes, ensuring the integrity and uniformity of the copper plating layer.
[0024] Secondly, ultrasonic-assisted stirring promotes the full infiltration of the graphene mixture and the template matrix. The infiltrated mixture not only maintains the high strength and high conductivity of graphene, but also utilizes the excellent elasticity and adhesion of polyurethane materials, providing a good foundation for the subsequent electroplating process.
[0025] Finally, during the electroplating process, the present invention deposits copper ions evenly on the template surface to form a dense copper layer, ensuring the strength and durability of the copper foam. Then, by removing the template matrix, the high-strength copper foam obtained has excellent porosity and strength, and is suitable for a variety of high-performance applications.
[0026] Second, in the electroplating process, the present application adds sodium polydisulfide propane sulfonate, fatty amine ethoxy sulfonate and thiazolinyl disulfide propane sulfonic acid as additives. Sodium polydisulfide propane sulfonate and fatty amine ethoxy sulfonate are used as brighteners and leveling agents, which can effectively improve the brightness and leveling of the coating; while thiazolinyl disulfide propane sulfonic acid is used as a strong leveling agent, and its grain refining effect can significantly improve the hardness of the foamed copper.
[0027] Third, the present application can effectively remove the oil and impurities of the template matrix by soaking in sodium hydroxide solution, and significantly improve its surface activity. Such treatment ensures that in the subsequent infiltration and electroplating process, the template matrix can form good adhesion with the copper plating layer, reducing the probability of defects that may occur during the electroplating process. By rinsing the template matrix to a pH value of 6-7, the stability of its surface chemical environment can be ensured, and the abnormal electroplating reaction caused by too high or too low pH value can be avoided. This series of processing steps ultimately provides a good foundation for electroplating, ensures the high quality and uniformity of the foamed copper, and improves its reliability and performance in practical applications. DETAILED DESCRIPTION
[0028] The present application is further described in detail below with reference to the embodiments.
[0029] In the examples of the present application, the raw materials and instruments used are as follows, but not limited thereto. Raw materials not otherwise described are of analytical grade: Preparation Example 1 Plating solution 1 Take 150-250 g of anhydrous copper sulfate, 5.5-7.5 g of 5% sulfuric acid and 25-80 g of 20% hydrochloric acid, stir and mix, and adjust the volume to 1 L to prepare electroplating solution 1.
[0030] Preparation Example 2 Plating solution 2 Take 150-250 g of anhydrous copper sulfate, 5.5-7.5 g of 5% sulfuric acid and 25-80 g of 20% hydrochloric acid, stir and mix, and dilute to 1 L to prepare electroplating solution 2.
[0031] Preparation Example 3 Plating solution 3 Take 150 g of anhydrous copper sulfate, 5.5 g of 5% sulfuric acid and 25 g of 20% hydrochloric acid, stir and mix, and adjust the volume to 1 L to prepare electroplating solution 3.
[0032] Preparation Example 4 Plating solution 4 Take 175g of anhydrous copper sulfate, 6g of 5% sulfuric acid and 55g of 20% hydrochloric acid, stir and mix, and adjust the volume to 1L. Then add plating treatment agents according to the mass concentration of 20ppm of sodium polydisulfide propane sulfonate, 200ppm of fatty amine ethoxy sulfonate AESS and 20ppm of thiazolinyl disulfide propane sulfonic acid to prepare electroplating solution 4.
[0033] Preparation Example 5 Plating solution 5 Take 175g of anhydrous copper sulfate, 6g of 5% sulfuric acid and 55g of 20% hydrochloric acid, stir and mix, and adjust the volume to 1L. Then add plating treatment agents according to the mass concentration of 20ppm of sodium polydisulfide propane sulfonate, 200ppm of fatty amine ethoxy sulfonate AESS and 30ppm of thiazolinyl disulfide propane sulfonic acid to prepare electroplating solution 5.
[0034] Preparation Example 6 Plating solution 6 Take 175g of anhydrous copper sulfate, 6g of 5% sulfuric acid and 55g of 20% hydrochloric acid, stir and mix, and adjust the volume to 1L. Then add plating treatment agents according to the mass concentration of 20ppm of sodium polydisulfide propane sulfonate, 200ppm of fatty amine ethoxy sulfonate AESS and 40ppm of thiazolinyl disulfide propane sulfonic acid to prepare electroplating solution 6.
[0035] Preparation Example 7 Plating solution 7 Take 175g of anhydrous copper sulfate, 6g of 5% sulfuric acid and 55g of 20% hydrochloric acid, stir and mix, and adjust the volume to 1L. Then add plating treatment agents according to the mass concentration of 20ppm of sodium polydisulfide propane sulfonate, 200ppm of fatty amine ethoxy sulfonate AESS and 50ppm of thiazolinyl disulfide propane sulfonic acid, stir and mix to prepare electroplating solution 6.
[0036] Embodiment 1-6 The following is described by taking Embodiment 1-3 as an example: Example 1 A method for preparing high-strength copper foam comprises the following preparation steps: A polyurethane foam with a pore size of 40-60 PPI is taken as a template matrix, and it is placed in a sodium hydroxide solution with a mass fraction of 10% and infiltrated for 5 minutes. After the infiltration is completed, it is rinsed and immersed in deionized water until the pH of the washing solution of the polyurethane foam is 6, and then the template matrix is removed and dried at room temperature, washed and dried, and the pretreated template matrix is collected; The pretreated template substrate was immersed in a 100 mg / L graphene mixed solution, and stirred and mixed and wetted under 200 W ultrasonic assisted treatment; After the impregnation is completed, the impregnated polyurethane foam is placed in the electroplating solution 1, electroplated at a voltage of 1.5 V for 40 minutes, rinsed with deionized water and naturally dried, and the foam copper matrix is collected; The copper foam substrate is then placed in dimethylformamide, a template substrate removal liquid, and soaked and dissolved. After being rinsed with deionized water, the substrate is placed at room temperature and dried naturally, thereby preparing the high-strength copper foam 1.
[0037] Example 2 A method for preparing high-strength copper foam comprises the following preparation steps: A polyurethane foam with a pore size of 50 PPI is taken as a template matrix, and it is placed in a sodium hydroxide solution with a mass fraction of 10%, and the solution is soaked for 5-10 minutes. After the soaking is completed, the polyurethane foam is rinsed and soaked with deionized water until the pH of the washing solution of the polyurethane foam is 6.5, and the template matrix is removed and dried at room temperature, washed and dried, and the pretreated template matrix is collected; The pretreated template substrate was immersed in a 100 mg / L graphene mixed solution, and stirred and mixed and wetted under 200 W ultrasonic assisted treatment; After the impregnation is completed, the impregnated polyurethane foam is placed in the electroplating solution 2, and electroplated at a voltage of 1.5 V for 40 minutes, and then naturally dried after rinsing with deionized water to collect the foam copper matrix; The copper foam substrate is then placed in dimethylformamide, a template substrate removal liquid, and soaked and dissolved. After being rinsed with deionized water, the substrate is placed at room temperature and dried naturally, thereby preparing the high-strength copper foam 2.
[0038] Example 3 A method for preparing high-strength copper foam comprises the following preparation steps: A polyurethane foam with a pore size of 60 PPI is taken as a template matrix, and it is placed in a sodium hydroxide solution with a mass fraction of 10%, and the solution is soaked for 5-10 minutes. After the soaking is completed, the polyurethane foam is rinsed and soaked with deionized water until the pH of the washing solution of the polyurethane foam is 7, and the template matrix is removed and dried at room temperature, washed and dried, and the pretreated template matrix is collected; The pretreated template substrate was immersed in a 100 mg / L graphene mixed solution, and stirred and mixed and wetted under 200 W ultrasonic assisted treatment; After the impregnation is completed, the impregnated polyurethane foam is placed in the electroplating solution 3, electroplated at a voltage of 1.5 V for 40 minutes, rinsed with deionized water and naturally dried to collect the foam copper matrix; The copper foam substrate is then placed in dimethylformamide, a template substrate removal liquid, and soaked and dissolved. After being rinsed with deionized water, the substrate is placed at room temperature and dried naturally, thereby preparing the high-strength copper foam 3.
[0039] Example 4 A method for preparing high-strength copper foam comprises the following preparation steps: A polyurethane foam with a pore size of 50 PPI is taken as a template matrix, and it is placed in a sodium hydroxide solution with a mass fraction of 10% and infiltrated for 8 minutes. After the infiltration is completed, it is rinsed and immersed in deionized water until the pH of the washing solution of the polyurethane foam is 6.5, and the template matrix is removed and dried at room temperature, washed and dried, and the pretreated template matrix is collected; The pretreated template substrate was immersed in a 100 mg / L graphene mixed solution, and stirred and mixed and wetted under 200 W ultrasonic assisted treatment; After the impregnation is completed, the impregnated polyurethane foam is placed in the electroplating solution 4, electroplated at a voltage of 1.5 V for 40 minutes, rinsed with deionized water and naturally dried to collect the foam copper matrix; The copper foam substrate is then placed in dimethylformamide, a template substrate removal liquid, and soaked to dissolve, then rinsed with deionized water, and then dried naturally at room temperature to prepare the high-strength copper foam 4.
[0040] Example 5 A method for preparing high-strength copper foam comprises the following preparation steps: A polyurethane foam with a pore size of 50 PPI is taken as a template matrix, and it is placed in a sodium hydroxide solution with a mass fraction of 10% and infiltrated for 7 minutes. After the infiltration is completed, it is rinsed and immersed in deionized water until the pH of the washing solution of the polyurethane foam is 6.5, and the template matrix is removed and dried at room temperature, washed and dried, and the pretreated template matrix is collected; The pretreated template substrate was immersed in a 100 mg / L graphene mixed solution, and stirred and mixed and wetted under 200 W ultrasonic assisted treatment; After the impregnation is completed, the impregnated polyurethane foam is placed in the electroplating solution 5, electroplated at a voltage of 1.5 V for 40 minutes, rinsed with deionized water and naturally dried to collect the foam copper matrix; The copper foam substrate is then placed in dimethylformamide, a template substrate removal liquid, and soaked and dissolved. After being rinsed with deionized water, the substrate is placed at room temperature and dried naturally, thereby preparing the high-strength copper foam 5.
[0041] Example 6 A method for preparing high-strength copper foam comprises the following preparation steps: A polyurethane foam with a pore size of 50 PPI is taken as a template matrix, and it is placed in a sodium hydroxide solution with a mass fraction of 10% and infiltrated for 7 minutes. After the infiltration is completed, it is rinsed and immersed in deionized water until the pH of the washing solution of the polyurethane foam is 6.5, and the template matrix is removed and dried at room temperature, washed and dried, and the pretreated template matrix is collected; The pretreated template substrate was immersed in a 100 mg / L graphene mixed solution, and stirred and mixed and wetted under 200 W ultrasonic assisted treatment; After the impregnation is completed, the impregnated polyurethane foam is placed in the electroplating solution 6, electroplated at a voltage of 1.5 V for 40 minutes, rinsed with deionized water and naturally dried to collect the foam copper matrix; The copper foam substrate is then placed in dimethylformamide, a template substrate removal liquid, and soaked and dissolved. After being rinsed with deionized water, the substrate is placed at room temperature and dried naturally, thereby preparing the high-strength copper foam 6.
[0042] Example 7 A method for preparing high-strength copper foam comprises the following preparation steps: A polyurethane foam with a pore size of 50 PPI is taken as a template matrix, and it is placed in a sodium hydroxide solution with a mass fraction of 10% and infiltrated for 7 minutes. After the infiltration is completed, it is rinsed and immersed in deionized water until the pH of the washing solution of the polyurethane foam is 6.5, and the template matrix is removed and dried at room temperature, washed and dried, and the pretreated template matrix is collected; The pretreated template substrate was immersed in a 100 mg / L graphene mixed solution, and stirred and mixed and wetted under 200 W ultrasonic assisted treatment; After the impregnation is completed, the impregnated polyurethane foam is placed in the electroplating solution 7, electroplated at a voltage of 1.5 V for 40 minutes, rinsed with deionized water and naturally dried to collect the foam copper matrix; The copper foam substrate is then placed in dimethylformamide, a template substrate removal liquid, and soaked and dissolved. After being rinsed with deionized water, the substrate is placed at room temperature and dried naturally, thereby preparing the high-strength copper foam 7.
[0043] Comparative Example Commercially available copper foam: Brand: TMAX Item No.: TMAX-Nickel Foam02 (Xiamen Tianmeifu Machinery Equipment Co., Ltd.) Performance Testing The properties of the high-strength copper foam prepared in Examples 1-7 and commercially available copper foam were tested, specifically the tensile strength thereof: (2) Tensile strength: According to the national standard GB / T 6344-2008 tensile strength test. The results are shown in Table 1 below: Table 1 Performance test table
[0044] From the above examples 1-6 and comparative example 1, combined with the test results of Table 1, it can be found that: The present application optimizes the preparation method of high-strength copper foam, first removes impurities on the surface of the template matrix by pretreatment, and significantly improves its surface activity. Secondly, ultrasonic-assisted stirring promotes the graphene mixture to be fully infiltrated with the template matrix. The infiltrated mixture not only maintains the high strength and high conductivity of graphene, but also utilizes the excellent elasticity and adhesion of polyurethane materials, providing a good foundation for the subsequent electroplating process. Finally, during the electroplating process, the present application evenly deposits copper ions on the template surface to form a dense copper layer to ensure the strength and durability of the copper foam. By removing the step of the template matrix, the high-strength copper foam obtained has excellent porosity and strength, and is suitable for a variety of high-performance applications.
[0045] Comparisons are made with Examples 1-3 and 4-7 to further illustrate that the technical solution of the present application adds sodium polydisulfide propane sulfonate, fatty amine ethoxy sulfonate and thiazolinyl disulfide propane sulfonic acid as additives during the electroplating process. Sodium polydisulfide propane sulfonate and fatty amine ethoxy sulfonate as brighteners and levelers can effectively improve the brightness and leveling of the coating; and thiazolinyl disulfide propane sulfonic acid as a strong leveler can significantly improve the hardness of the foamed copper by its grain refining effect.
[0046] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
[0047] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definition in this specification shall prevail.
[0048] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.
[0049] In the context of the present specification, any matters or items not mentioned are directly applicable to those known in the art without any changes except those explicitly stated.
Claims
1. A high-strength copper foam, It is characterized in that The porosity of the copper foam is >95%.
2. A method for preparing a high-strength copper foam according to claim 1, It is characterized in that The method comprises the following preparation steps: Taking the template substrate and pre-treating the surface thereof, washing and drying the template substrate, and collecting the pre-treated template substrate; The pre-treated template substrate is immersed in the graphene mixed solution, and stirred and mixed and wetted under ultrasonic assisted treatment; After the infiltration is completed, the infiltrated template substrate is placed in an electroplating solution, electroplated, washed, dried, and the foamed copper substrate is collected; The foam copper substrate is then placed in a template substrate removal liquid, immersed and dissolved, and then washed and dried to prepare the high-strength foam copper.
3. A method for preparing a high-strength copper foam according to claim 2, It is characterized in that The template matrix comprises a polyurethane foam matrix material with a pore size of 40-60 PPI.
4. The method for preparing a high-strength copper foam according to claim 2, It is characterized in that The surface pretreatment adopts the following scheme: Taking the template substrate and placing it in a sodium hydroxide solution for soaking treatment; After the soaking is completed, deionized water is used for rinsing and soaking until the pH value of the washing solution is 6-7, and then the template matrix is removed and dried at room temperature.
5. The method for preparing a high-strength copper foam according to claim 2, It is characterized in that The electroplating solution comprises the following substances in parts by weight: 15-25 parts of copper sulfate pentahydrate; Sulfuric acid 5.5-7.0 parts; 2.5-8.0 parts of hydrochloric acid.
6. The method for preparing a high-strength copper foam according to claim 5, It is characterized in that The electroplating further comprises a plating treatment agent, and the plating treatment agent comprises the following substances in parts by weight: 15-30 parts of sodium polydipropane disulfide sulfonate; Fatty amine ethoxylate AESS 180-220 parts; Thiamidopropane disulfide sulfonic acid 15-25 parts.
7. The method for preparing a high-strength copper foam according to claim 2, It is characterized in that The template matrix removing liquid includes one or more of acetone, N-methylpyrrolidone, dimethylformamide, methanol, and ethanol.
8. The method for preparing a high-strength copper foam according to claim 2, It is characterized in that The voltage of the electroplating treatment is 1-2V, and the electroplating time is 30-60min.