Dicing blade electroplating liquid composition and preparation method thereof

By using specific plating solution compositions and plating parameters on the scribing knife, the problems of insufficient strength and poor corrosion resistance of the scribing knife are solved, high hardness, low stress and good corrosion resistance are achieved, ensuring the chip cutting process Stability and efficiency.

CN118996550APending Publication Date: 2024-11-22JIANGSU SANJING SEMICON MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411416606.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the semiconductor packaging manufacturing process, insufficient strength of the scribble knife leads to serpentine cutting or bevel cutting, and due to the corrosion of carbon dioxide in the cooling water, the adhesive is prone to rupture, affecting the normal progress of the cutting process.

Method used

Using an electroplating solution composition, including nickel sulfamate, nickel chloride, boric acid, benzyl disulfonic acid, 2-mercaptobenzimidazole, dibenzyl sulfonyl propylamine and sodium benzyl sulfinate, by electroplating the nickel layer, combined with Sodium benzenesulfinate regulates internal stress and controls pH and temperature during electroplating to reduce the void ratio of the coating to improve corrosion resistance.

Benefits of technology

The high hardness (650~700 HV) of the slashing knife is achieved and the low internal stress is low, which significantly improves corrosion resistance and service life, and reduces the risk of corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996550A_ABST
    Figure CN118996550A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of scribing blade preparation, and discloses a scribing blade electroplating liquid composition and a preparation method thereof. The preparation method of the dicing blade comprises the following steps: providing a base body; electroplating diamond on the substrate to obtain a dicing blade crude product; trimming, polishing and edging the dicing blade crude product to obtain the dicing blade, the electroplating liquid composition for electroplating comprises the following components: 45 to 90 g / L of nickel aminosulfonate, 5 to 15 g / L of nickel chloride, 30 to 45 g / L of boric acid, 10 to 15 g / L of benzene disulfonic acid, 10 to 15 g / L of 2-mercaptobenzimidazole, 5 to 10 g / L of dibenzenesulfonyl propylamine, 0.1 to 0.5 g / L of sodium benzenesulfinate and 4 to 8 mL / L of sodium dodecyl sulfate. The scribing cutter manufactured through the manufacturing method has the advantages of being high in hardness, low in stress, high in corrosion resistance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of dicing blades, and discloses a dicing blade electroplating liquid composition and a preparation method thereof. Background Art

[0002] In the semiconductor packaging manufacturing process, there is a process called dicing, which uses a dicing knife with diamond as abrasive and electroplated nickel as adhesive to cut and separate chip units. This is a high-precision processing that has an important impact on chip quality and cost.

[0003] With the development of miniaturization and integration of chip size, the thickness of chips is developing towards two extremes, one is thinning and the other is thickening. Thin chips require less impact force during the dicing process and faster feed speed, some of which are as high as 180mm / s. This requires the dicing knife blade to have sufficient strength, otherwise it is easy to cause serpentine cutting; while the most common problem of thick chips during the dicing process is bevel cutting, which is mainly caused by insufficient blade strength and deformation of the blade due to internal stress.

[0004] In order to eliminate static electricity during the chip dicing process, carbon dioxide gas is added to the cutting cooling water to make the cooling water weakly acidic, which will corrode the adhesive of the dicing knife, causing the dicing knife blade to break and affecting the normal dicing process. Summary of the invention

[0005] In view of the shortcomings of the prior art mentioned above, the purpose of the present invention is to provide a dicing knife electroplating liquid composition and a preparation method thereof. In view of the above situation, in order to solve the defects of the prior art, the purpose of the present invention is to provide a dicing knife electroplating liquid composition and a preparation method thereof, so as to improve the strength of the dicing knife, reduce the internal stress of the dicing knife, and improve the corrosion resistance of the dicing knife.

[0006] In order to solve the above technical problems, the present invention first provides a dicing knife electroplating liquid composition, the formula of the electroplating liquid composition includes the following components: 45-90 g / L nickel sulfamate, 5-15 g / L nickel chloride, 30-45 g / L boric acid, 10-15 g / L benzene disulfonic acid, 10-15 g / L 2-mercaptobenzimidazole, 5-10 g / L diphenylsulfonylpropylamine, 0.1-0.5 g / L sodium benzenesulfinate, and 4-8 mL / L sodium dodecyl sulfate.

[0007] The present invention firstly provides a method for preparing a dicing knife electroplating liquid composition, which comprises mixing the following components: 45-90 g / L nickel sulfamate, 5-15 g / L nickel chloride, 30-45 g / L boric acid, 10-15 g / L benzene disulfonic acid, 10-15 g / L 2-mercaptobenzimidazole, 5-10 g / L diphenylsulfonylpropylamine, 0.1-0.5 g / L sodium benzenesulfinate, and 4-8 mL / L sodium dodecyl sulfate.

[0008] The present invention also provides a method for preparing a dicing knife, the method comprising the following steps:

[0009] providing a substrate;

[0010] Electroplating diamond on the substrate to obtain a rough dicing knife;

[0011] The rough dicing knife is trimmed, polished and sharpened to obtain the dicing knife;

[0012] The electroplating solution composition for electroplating includes the following components: 45-90 g / L nickel sulfamate, 5-15 g / L nickel chloride, 30-45 g / L boric acid, 10-15 g / L benzene disulfonic acid, 10-15 g / L 2-mercaptobenzimidazole, 5-10 g / L diphenylsulfonylpropylamine, 0.1-0.5 g / L sodium benzenesulfinate, and 4-8 mL / L sodium dodecylsulfonate.

[0013] More optimally, the substrate is alkaline washed in 5% sodium hydroxide for 2 minutes, acid washed in 5% nitric acid for 40 seconds, and zinc precipitated in DSN-4 zinc precipitator for 1 minute.

[0014] Preferably, the substrate is an aluminum substrate.

[0015] Preferably, the substrate is subjected to alkali washing, acid washing and zinc deposition steps before electroplating.

[0016] More optimally, the electroplating parameters include: pH 3.5-4.5, temperature 40°C-45°C, and current density 1.6-3.5 ASD.

[0017] More optimally, the diamond electroplating includes adding artificial diamond powder into the electroplating tank and stirring it, and the stirring method is cathode movement.

[0018] More optimally, the rough product trimming of the dicing knife includes wire cutting, bevel turning and etching of the substrate.

[0019] More optimally, sodium hydroxide etching solution is used during the etching.

[0020] Preferably, the polishing includes using a polishing liquid, which is a mixture of 50% phosphoric acid and 50% sulfuric acid.

[0021] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0022] 1. The electroplating solution formula of the dicing knife uses sulfur-containing benzene ring primary and secondary brighteners, namely benzene disulfonic acid, 2-mercaptobenzimidazole, and hardener diphenylsulfonyl propylamine to obtain an electrodeposited nickel binder with a Vickers hardness of up to 650-700.

[0023] 2. An additive, sodium benzenesulfinate, is added to adjust the internal stress of the coating, so that the internal stress of the electrodeposited nickel is close to 0.

[0024] 3. The plating solution formula and plating parameters are designed to greatly reduce the porosity of the coating and improve the corrosion resistance, so that the corrosion of the dicing knife is very slight and the quality is stable throughout its life cycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a diagram of an electroplated aluminum substrate of the present invention;

[0026] Figure 2 This is a diagram of the oblique turning process of the electroplated aluminum substrate of the present invention; DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] S1 blank processing, purchased aluminum bars, after machining, processed into Figure 1 Aluminum blank substrate shown.

[0030] S2 electroplating, the aluminum blank substrate is washed with 5% sodium hydroxide for 2 minutes to remove oil, 5% nitric acid for 40 seconds, and then zinc is deposited with Shenzhen Disen DSN-4 zinc depositing agent for 1 minute before entering the electroplating tank. The formula of the electroplating solution composition is: nickel aminosulfonate, 45g / L; nickel chloride, 5g / L; boric acid, 30g / L; benzene disulfonic acid, 10g / L; 2-mercaptobenzimidazole, 10g / L; diphenylsulfonylpropylamine, 5g / L; sodium benzenesulfinate, 0.1g / L; sodium dodecylsulfonate, 4mL / L. The electroplating parameters are: pH3.5; temperature 40℃, current density 1.6ASD, artificial diamond powder is added to the electroplating tank for stirring, the stirring mode is cathode movement, and the electroplating stops when the specified thickness is reached.

[0031] S3 uses wire-cutting electrospark to trim the outer circle of the electroplated body.

[0032] S4 inclined car, such as Figure 2 As shown, the back blank aluminum substrate of the electroplated nickel layer is processed to prepare for the next etching.

[0033] S5 etching, using sodium hydroxide etching solution to etch the residual blank substrate after the back of the electroplated body is tilted to remove part of the substrate to meet the specified specifications.

[0034] S6 electrochemical polishing: electrochemical polishing is performed on the electroplated nickel to fully expose the artificial diamond powder embedded therein. The polishing liquid is a mixture of 50% phosphoric acid and 50% sulfuric acid.

[0035] S7 sharpening, use a dicing machine to sharpen on a sharpening board.

[0036] S8 inspection and packaging: the finished dicing knives are inspected for appearance, blade length and thickness and then packaged after passing the inspection.

[0037] Example 2

[0038] S1 blank processing, purchased aluminum bars, after machining, processed into Figure 1 Aluminum blank substrate shown.

[0039] S2 electroplating, the aluminum blank substrate is washed with 5% sodium hydroxide for 2 minutes to remove oil, 5% nitric acid for 40 seconds, and then zinc is deposited with Shenzhen Disen DSN-4 zinc depositing agent for 1 minute before entering the electroplating tank. The formula of the electroplating solution composition is: nickel aminosulfonate, 90g / L; nickel chloride, 15g / L; boric acid, 45g / L; benzene disulfonic acid, 15g / L; 2-mercaptobenzimidazole, 15g / L; diphenylsulfonylpropylamine, 10g / L; sodium benzenesulfinate, 0.5g / L; sodium dodecylsulfonate, 8mL / L. The electroplating parameters are: pH 4; temperature 43℃, current density 2.5ASD, artificial diamond powder is added to the electroplating tank for stirring, the stirring mode is cathode movement, and the electroplating stops when the specified thickness is reached.

[0040] S3 uses wire-cutting electrospark to trim the outer circle of the electroplated body.

[0041] S4 inclined car, such as Figure 2 As shown, the back blank aluminum substrate of the electroplated nickel layer is processed to prepare for the next etching.

[0042] S5 etching, using sodium hydroxide etching solution to etch the residual blank substrate after the back of the electroplated body is tilted to remove part of the substrate to meet the specified specifications.

[0043] S6 electrochemical polishing: electrochemical polishing is performed on the electroplated nickel to fully expose the artificial diamond powder embedded therein. The polishing liquid is a mixture of 50% phosphoric acid and 50% sulfuric acid.

[0044] S7 sharpening, use a dicing machine to sharpen on a sharpening board.

[0045] S8 inspection and packaging: the finished dicing knives are inspected for appearance, blade length and thickness and then packaged after passing the inspection.

[0046] Example 3

[0047] S1 blank processing, purchased aluminum bars, after machining, processed into Figure 1 Aluminum blank substrate shown.

[0048] S2 electroplating, the aluminum blank substrate is washed with 5% sodium hydroxide for 2 minutes to remove oil, 5% nitric acid for 40 seconds, and then zinc is deposited with Shenzhen Disen DSN-4 zinc depositing agent for 1 minute before entering the electroplating tank. The formula of the electroplating solution composition is: nickel aminosulfonate, 60g / L; nickel chloride, 10g / L; boric acid, 40g / L; benzene disulfonic acid, 12g / L; 2-mercaptobenzimidazole, 12g / L; diphenylsulfonylpropylamine, 6g / L; sodium benzenesulfinate, 0.4g / L; sodium dodecylsulfonate, 6mL / L. The electroplating parameters are: pH 4.5; temperature 45℃, current density 3.5ASD, artificial diamond powder is added to the electroplating tank for stirring, the stirring mode is cathode movement, and the electroplating stops when the specified thickness is reached.

[0049] S3 uses wire-cutting electrospark to trim the outer circle of the electroplated body.

[0050] S4 inclined car, such as Figure 2 As shown, the back blank aluminum substrate of the electroplated nickel layer is processed to prepare for the next etching.

[0051] S5 etching, using sodium hydroxide etching solution to etch the residual blank substrate after the back of the electroplated body is tilted to remove part of the substrate to meet the specified specifications.

[0052] S6 electrochemical polishing: electrochemical polishing is performed on the electroplated nickel to fully expose the artificial diamond powder embedded therein. The polishing liquid is a mixture of 50% phosphoric acid and 50% sulfuric acid.

[0053] S7 sharpening, use a dicing machine to sharpen on a sharpening board.

[0054] S8 inspection and packaging: the finished dicing knives are inspected for appearance, blade length and thickness and then packaged after passing the inspection.

[0055] Comparative Example 1

[0056] The difference between Comparative Example 1 and Example 1 is that sodium benzenesulfinate is not added to the formula of the electroplating solution in S2, and the remaining steps are the same as those in Example 1.

[0057] Comparative Example 2

[0058] The difference between Comparative Example 2 and Example 1 is that benzene disulfonic acid and 2-mercaptobenzimidazole are not added to the formula of the electroplating solution in S2, and the remaining steps are the same as those in Example 1.

[0059] evaluate

[0060] 1. The Vickers hardness was measured using a Shimadzu micro Vickers hardness tester.

[0061] 2. Use a spiral shrinkage instrument to measure stress.

[0062] 3. Use the filter paper method to determine the porosity of the coating.

[0063] Table 1 Technical effect evaluation of embodiments and comparative examples

[0064]

[0065]

[0066] Conclusion: The electroplating parameters of this formula are: pH 3.5-4.5; temperature 40-45℃, current density 1.6-3.5ASD, stirring mode is cathode moving, the electroplated nickel hardness is 650-700 HV, and the electroplated nickel internal stress is -0.5kN / mm 2 ~0.5kN / mm 2 , porosity is 0~2 blue spots / cm 2 .

[0067] The electroplated nickel layer produced by the formula has a corrosion rate of 8 to 12 um / a in an aqueous solution with a pH of 3 to 4. The plated layer produced by the formula has high hardness, low stress and strong corrosion resistance.

[0068] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0069] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A dicing blade electroplating liquid composition, characterized in that: The formula of the electroplating solution composition includes the following components: 45-90 g / L nickel sulfamate, 5-15 g / L nickel chloride, 30-45 g / L boric acid, 10-15 g / L benzene disulfonic acid, 10-15 g / L 2-mercaptobenzimidazole, 5-10 g / L diphenylsulfonylpropylamine, 0.1-0.5 g / L sodium benzenesulfinate, and 4-8 mL / L sodium dodecylsulfonate.

2. A method for preparing a dicing blade electroplating liquid composition, characterized in that: The method comprises mixing the following components: 45-90 g / L nickel sulfamate, 5-15 g / L nickel chloride, 30-45 g / L boric acid, 10-15 g / L benzene disulfonic acid, 10-15 g / L 2-mercaptobenzimidazole, 5-10 g / L diphenylsulfonylpropylamine, 0.1-0.5 g / L sodium benzenesulfinate, and 4-8 mL / L sodium dodecylsulfonate.

3. A method for preparing a slicing knife, characterized in that: The method comprises the following steps: providing a substrate; Electroplating diamond on the substrate to obtain a rough dicing knife; The rough dicing knife is trimmed, polished and sharpened to obtain the dicing knife; The electroplating solution composition for electroplating includes the following components: 45-90 g / L nickel sulfamate, 5-15 g / L nickel chloride, 30-45 g / L boric acid, 10-15 g / L benzene disulfonic acid, 10-15 g / L 2-mercaptobenzimidazole, 5-10 g / L diphenylsulfonylpropylamine, 0.1-0.5 g / L sodium benzenesulfinate, and 4-8 mL / L sodium dodecylsulfonate.

4. The preparation method according to claim 3, characterized in that: The substrate is an aluminum substrate.

5. The preparation method according to claim 3, characterized in that: The substrate is subjected to the steps of alkali washing, acid washing and zinc deposition before electroplating.

6. The preparation method according to claim 3, characterized in that: The electroplating parameters include: pH of 3.5-4.5, temperature of 40° C.-45° C., and current density of 1.6-3.5 ASD.

7. The preparation method according to claim 3, characterized in that: The diamond electroplating comprises adding artificial diamond powder into the electroplating tank and stirring it, and the stirring method is cathode movement.

8. The preparation method according to claim 3, characterized in that: The rough product trimming of the dicing knife includes wire cutting, bevel turning and etching of the substrate.

9. The preparation method according to claim 8, characterized in that: When performing the etching, a sodium hydroxide etching solution is used.

10. The preparation method according to claim 3, characterized in that: The polishing includes using a polishing liquid, which is a mixture of 50% phosphoric acid and 50% sulfuric acid.

Citation Information

Cited By

  • Manufacturing method of diamond blade suitable for cutting inductor and diamond blade

    CN120791355A