Method for growing high-nitrogen large-size monocrystal diamond by using cobalt catalyst
By using metal cobalt sheets as catalysts in high-pressure equipment, the nitrogen content of artificial synthetic diamonds is improved, and the problem of the nitrogen content and form differences between artificial synthetic diamonds and natural diamonds is solved, and the large size, integrity and natural diamonds are achieved. Nitrogen content.
Patent Information
- Application Number
- CN202411136551.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the nitrogen content and existence form of artificially synthesized diamonds differ from that of natural diamonds, making it difficult to synthesize diamonds with complete crystal forms.
Using metal cobalt sheets as catalysts, single crystal diamonds are synthesized in the synthesis cavity under specific conditions through high-pressure equipment, allowing carbon elements to enter the diamond lattice and increasing the nitrogen content of the diamond.
The nitrogen content of single crystal diamond was successfully increased, and the nitrogen presence form was close to that of natural diamond, so the size and integrity of the crystal were guaranteed.
Smart Images

Figure CN118996598A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of diamond preparation, and in particular to a method for growing large-size single crystal diamond with high nitrogen using a cobalt catalyst. Background Art
[0002] Diamond has a series of excellent properties such as high hardness, extremely high thermal conductivity, high refractive index and excellent chemical stability, and is used in many fields such as drill bits, abrasives, handicrafts and decorations. Artificial diamond is mainly synthesized by high temperature and high pressure and chemical vapor deposition.
[0003] Diamonds can be divided into two categories according to their nitrogen content: Type I and Type II. Synthetic diamonds are Type Ib, which contain about 300 ppm of nitrogen, and the nitrogen exists in the form of a single substitution atom, i.e., a diffuse state. The nitrogen content of natural diamonds is about 2×10 3 ppm, in which nitrogen exists in aggregated form, mostly (Ia type. There are great differences in nitrogen concentration and existence form between artificial diamond and natural diamond, resulting in differences in the properties of the two types of diamond. Synthesizing high nitrogen content diamond with complete crystal form can become a problem of concern to those skilled in the art. Summary of the invention
[0004] In order to solve the problems and shortcomings in the prior art, the present invention provides a method for growing large-size single-crystal diamond with high nitrogen using a cobalt catalyst, wherein a metal cobalt sheet is used as a catalyst to synthesize diamond. Because the nitrogen dissolving capacity of metal cobalt is lower than that of traditional alloy catalysts, the carbon element in the synthesis cavity enters the diamond lattice and replaces the carbon atoms in the lattice, thereby increasing the nitrogen content of the diamond crystal.
[0005] Specifically, the present invention provides a method for growing large-sized single-crystal diamond with high nitrogen content using a cobalt catalyst, the method comprising:
[0006] Assembling a carbon source, a metal catalyst and a diamond seed crystal into a synthesis block;
[0007] The synthesis block is placed in a synthesis chamber of a high-pressure device, and a single crystal diamond is obtained under the conditions of a synthesis pressure of 5.5 GPa to 6.0 GPa, a synthesis temperature of 1400° C. to 1500° C., and a synthesis time of 20 h to 25 h;
[0008] The carbon source is flake graphite with a purity of not less than 99.99%, the catalyst is a metal cobalt sheet with a purity of not less than 99.99%, and the diamond seed crystal is a {100} face or a {111} face of diamond.
[0009] Optionally, the high-voltage equipment is a hinged six-sided top.
[0010] Optionally, the internal temperature of the synthesis cavity is calibrated according to a relationship curve between input power and temperature measured by a double platinum-rhodium thermocouple;
[0011] The internal pressure of the synthetic cavity is calibrated by a calibration curve of oil pressure and internal pressure of the cavity established according to the high-pressure phase transition points of bismuth, barium and thallium.
[0012] Optionally, before being assembled into the synthetic block, the carbon source, the metal catalyst and the diamond seed crystal are stored in a drying oven.
[0013] Optionally, before the synthetic block is placed in the high-pressure equipment, it is dried in an oven for 1 hour to 3 hours for dehydration treatment, and the drying temperature is 110° C. to 130° C.
[0014] In the present invention, metal cobalt is used as a catalyst to synthesize single crystal diamond. Compared with traditional alloy catalysts, Co has a weaker nitrogen dissolving capacity, so that more nitrogen in the synthesis cavity enters the diamond lattice and replaces C in the diamond lattice, thereby increasing the nitrogen content in the single crystal diamond.
[0015] Based on the following detailed description of specific embodiments of the present invention in conjunction with the accompanying drawings, those skilled in the art will become more aware of the above and other objects, advantages and features of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Hereinafter, some specific embodiments of the present invention will be described in detail in an exemplary and non-limiting manner with reference to the accompanying drawings. The same reference numerals in the accompanying drawings indicate the same or similar components or parts. It should be understood by those skilled in the art that these drawings are not necessarily drawn to scale. In the accompanying drawings:
[0017] Figure 1 is a flow chart of a method for growing large-size single crystal diamond with high nitrogen using a cobalt catalyst according to an embodiment of the present invention;
[0018] Figure 2 is a SEM picture of the diamond crystal synthesized in Example 1;
[0019] Figure 3 is a SEM picture of the diamond crystal synthesized in Example 2;
[0020] Figure 4 is a SEM picture of the diamond crystal synthesized in Example 3;
[0021] Figure 5 is a SEM picture of the diamond crystal synthesized in Example 4;
[0022] Figure 6 It is the infrared absorption spectrum of the diamond crystal synthesized in Example 4, Comparative Example and Comparative Example 2. DETAILED DESCRIPTION
[0023] Refer to the following Figures 1 to 6 To describe a method for growing large-size single crystal diamond with high nitrogen using a cobalt catalyst according to an embodiment of the present invention. In the description of this embodiment, it should be understood that the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features, that is, include one or more of the features. In the description of the present invention, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. When a feature "includes or contains" one or some of the features it covers, unless otherwise specifically described, this indicates that other features are not excluded and may further include other features.
[0024] In the description of the present embodiment, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0025] Figure 1 FIG. 1 is a flow chart of a method for growing large-size single crystal diamond using a cobalt catalyst and high nitrogen content according to an embodiment of the present invention. Figure 1 As shown, the present invention provides a method for growing large-sized single-crystal diamond with high nitrogen and cobalt catalyst. The above-mentioned method for growing large-sized single-crystal diamond with high nitrogen and cobalt catalyst comprises:
[0026] Step S20, assembling the carbon source, the metal catalyst and the diamond seed crystal into a synthetic block;
[0027] Step S40, placing the synthesis block into a synthesis chamber of a high-pressure device, and obtaining single crystal diamond under the conditions of a synthesis pressure of 5.5 GPa to 6.0 GPa, a synthesis temperature of 1400° C. to 1500° C., and a synthesis time of 20 h to 25 h;
[0028] The carbon source is flake graphite with a purity of not less than 99.99%, the catalyst is a metal cobalt sheet with a purity of not less than 99.99%, and the diamond seed crystal is the {100} face of diamond.
[0029] In other embodiments of the present invention, the diamond seed crystal is a {111} face of diamond.
[0030] The specific preparation process of the above embodiment includes: first, assembling selected flake graphite with a purity of not less than 99.99%, metal cobalt flakes with a purity of not less than 99.99% and the {100} face of diamond into a synthesis block. Secondly, placing the synthesis block into a synthesis chamber of a high-pressure device to obtain a single crystal diamond. During the synthesis process, because the nitrogen solubility of metal cobalt is relatively weak, more nitrogen in the synthesis chamber enters the diamond lattice and replaces C in the diamond lattice.
[0031] In the above embodiment, a metal cobalt sheet with a purity of not less than 99.99% is selected as a catalyst, and a single crystal diamond with a size of more than 1.4 mm and a complete crystal form can be obtained, and the nitrogen content of the single crystal diamond is significantly higher than that of the traditional preparation process. In some embodiments of the present invention, the high-voltage equipment is a hinged six-sided top. Compared with the two-sided top, when the six-sided top is selected to synthesize diamond, the force in the synthesis cavity is more ideal.
[0032] In some embodiments of the present invention, the internal temperature of the synthesis cavity is calibrated according to the relationship curve between input power and temperature measured by a double platinum-rhodium thermocouple. The internal pressure of the synthesis cavity is calibrated by a calibration curve of oil pressure and cavity internal pressure established according to the high-pressure phase transition point of bismuth, barium, and thallium.
[0033] In this embodiment, a suitable temperature and pressure control method is selected to make the temperature and pressure control during synthesis more precise.
[0034] In some embodiments of the present invention, the carbon source, metal catalyst and diamond seed crystal are stored in a drying oven before being assembled into a synthetic block. In this embodiment, the carbon source, metal catalyst and diamond seed crystal are stored in a drying oven to prevent water from being contained in the carbon source, metal catalyst and diamond seed crystal.
[0035] In some embodiments of the present invention, before the synthetic block is placed in the high-pressure equipment, it is dried in an oven for 1 hour to 3 hours for dehydration treatment, and the drying temperature is 110° C. to 130° C.
[0036] In this embodiment, drying the synthetic block is to keep the surface of the synthetic block dry, which is beneficial to the growth of crystal grains.
[0037] The present invention also provides a single crystal diamond, which is prepared by the preparation method described in any of the above embodiments. The size of the single crystal diamond is 1.4-3.0 mm.
[0038] The present invention is specifically explained below using several embodiments, and the technical solutions in the embodiments of the present invention are clearly and completely described. The described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments.
[0039] Example 1
[0040] A method for growing large-size single crystal diamond with high nitrogen content using a cobalt catalyst comprises the following steps:
[0041] Step S11, selecting flake graphite with a purity of 99.99%, cobalt metal sheets with a purity of 99.99% and diamond seed crystals stored in a drying oven to assemble into a synthetic block, wherein the growth surface of the diamond in the synthetic block is a {111} surface.
[0042] Step S12, placing the synthesized block in a drying oven and drying it at 110° C. for 1 hour.
[0043] Step S13, placing the synthesis block into a synthesis chamber with a hinged six-sided top, and obtaining single crystal diamond after 20 hours at a synthesis pressure of 5.5 GPa and a synthesis temperature of 1400°C.
[0044] Example 2
[0045] A method for growing large-size single crystal diamond with high nitrogen content using a cobalt catalyst comprises the following steps:
[0046] Step S11, selecting flake graphite with a purity of 99.99%, cobalt metal sheets with a purity of 99.99% and diamond seed crystals stored in a drying oven to assemble into a synthetic block, wherein the growth surface of the diamond in the synthetic block is a {111} surface.
[0047] Step S12, placing the synthesized block into a drying oven and drying it at 130° C. for 1 hour.
[0048] Step S13, placing the synthesis block into a synthesis chamber with a hinged six-sided top, and obtaining single crystal diamond after 20 hours at a synthesis pressure of 6.0 GPa and a synthesis temperature of 1500°C.
[0049] Example 3
[0050] A method for growing large-size single crystal diamond with high nitrogen content using a cobalt catalyst comprises the following steps:
[0051] Step S11, selecting flake graphite with a purity of 99.99%, cobalt metal sheets with a purity of 99.99% and diamond seed crystals stored in a drying oven to assemble into a synthetic block, wherein the growth surface of the diamond in the synthetic block is the {100} surface.
[0052] Step S12, placing the synthesized block in a drying oven and drying it at 110° C. for 3 hours.
[0053] Step S13, placing the synthesis block into a synthesis chamber with a hinged six-sided top, and obtaining single crystal diamond after 20 hours at a synthesis pressure of 5.6 GPa and a synthesis temperature of 1450°C.
[0054] Example 4
[0055] A method for growing large-size single crystal diamond with high nitrogen content using a cobalt catalyst comprises the following steps:
[0056] Step S11, selecting flake graphite with a purity of 99.99%, cobalt metal sheets with a purity of 99.99% and diamond seed crystals stored in a drying oven to assemble into a synthetic block, wherein the growth surface of the diamond in the synthetic block is a {111} surface.
[0057] Step S12, placing the synthesized block into a drying oven and drying it at 130° C. for 2 hours.
[0058] Step S13, placing the synthesis block into a synthesis chamber with a hinged six-sided top, and obtaining single crystal diamond after 25 hours at a synthesis pressure of 5.6 GPa and a synthesis temperature of 1450°C.
[0059] Comparative Example 1
[0060] A method for preparing large-size single-crystal diamond comprises the following steps:
[0061] Step S11, selecting flake graphite with a purity of 99.99% stored in a drying oven, iron-nickel alloy and diamond seed crystals to assemble into a synthetic block, wherein the growth surface of the diamond in the synthetic block is a {111} surface.
[0062] Step S12, placing the synthesized block into a drying oven and drying it at 130° C. for 2 hours.
[0063] Step S13, placing the synthesis block into a synthesis chamber with a hinged six-sided top, and obtaining single crystal diamond after 24 hours at a synthesis pressure of 5.6 GPa and a synthesis temperature of 1450°C.
[0064] Comparative Example 2
[0065] A method for preparing large-size single-crystal diamond comprises the following steps:
[0066] Step S11, selecting flake graphite, nickel-manganese-cobalt and diamond seed crystals with a purity of 99.99% stored in a drying oven and assembling them into a synthetic block, wherein the growth surface of the diamond in the synthetic block is a {111} surface.
[0067] Step S12, placing the synthesized block in a drying oven and drying it at 130° C. for 3 hours.
[0068] Step S13, placing the synthesis block into a synthesis chamber with a hinged six-sided top, and obtaining single crystal diamond after 24 hours at a synthesis pressure of 5.6 GPa and a synthesis temperature of 1450°C.
[0069] In the above-mentioned Examples 1 to 4, and Comparative Examples 1 and 2, the internal temperature of the synthesis cavity is calibrated according to the relationship curve between the input power and the temperature measured by the double platinum-rhodium thermocouple. The internal pressure of the synthesis cavity is calibrated by the calibration curve of the oil pressure and the internal pressure of the cavity established according to the high-pressure phase transition point of bismuth, barium and thallium.
[0070] The single crystal diamonds obtained in Examples 1 to 4, Comparative Examples 1 and 2 were processed according to the following steps and then tested and characterized. The specific processing steps include:
[0071] Step S40, placing the obtained single crystal diamond into heated dilute nitric acid to strip the single crystal diamond from the cobalt catalyst.
[0072] Step S50, placing the single crystal diamond in a mixture of H2SO4:HNO3 (3:1) and heating it to remove impurities such as graphite remaining on the surface of the crystal.
[0073] Step S60, the single crystal diamond after acid treatment is placed in a beaker filled with alcohol for ultrasonic cleaning.
[0074] from Figures 2 to 5 It can be seen that the diamond prepared in the Co-C system is a single crystal with brown or yellow-green color, and the crystal form of the single crystal is complete. Regardless of whether the {100} or {111} plane is selected as the growth plane of the diamond, the {100} of the final synthesized diamond single crystal disappears, and the existing crystal plane is the {111} crystal plane. The specific color and size are shown in Table 1:
[0075] Table 1 Color and size of single crystal diamond prepared under different process conditions
[0076] Serial number Pressure / Gpa Temperature / ℃ Growth surface color Dimensions / mm Example 1 5.5 1400 {111} Brown 1.8 Example 2 6.0 1500 {111} Brown 1.8 Example 3 5.6 1450 {100} Brown 1.4 Example 4 5.6 1450 {111} Green and yellow 2.0
[0077] Figure 6 The three spectral lines a, b and c correspond to the infrared absorption spectra of diamond single crystals grown in the Co-C system, FeNi-C system and NiMnCo-C system respectively. All three spectral lines have a peak at 1130 cm -1 and 1344cm -1 Peak, 1130cm -1 and 1344cm -1 The peak is C-center nitrogen, and the strength of the peak represents the concentration of C-center nitrogen. There is also a 1282cm -1 peak, while the general line c does not exist at 1282cm -1 Peak, this peak is A-center nitrogen, the strength of the peak represents the concentration of A-center nitrogen. Analyze the spectrum for N content analysis, and calculate the nitrogen content in the crystal using the nitrogen content calculation formula. The results are shown in Table 2:
[0078] Table 2 Nitrogen content of synthetic diamond
[0079] Serial number Growth surface color <![CDATA[N C / ppm]]> <![CDATA[N A / ppm]]> <![CDATA[N 总 ]]> Example 4 {111} Green and yellow 710 270 980 Comparative Example 1 {111} yellow 330 41 371 Comparative Example 2 {111} Light yellow 97 0 97
[0080] As can be seen from Table 2, the diamond crystal grown in the Co catalyst system has a C-center nitrogen content of 710ppm, an A-center nitrogen content of 270ppm, and a total nitrogen content of 980ppm. The diamond grown in the FeNi catalyst system has a C-center nitrogen content of 330ppm, an A-center nitrogen content of 41ppm, and a total nitrogen content of 371ppm. The diamond grown in the NiMnCo catalyst system has a C-center nitrogen content of 97ppm and no A-center nitrogen. By comparing the nitrogen content, it is found that whether it is the C-center nitrogen content, the A-center nitrogen content, or the total nitrogen content, the nitrogen content of diamond synthesized using pure Co as a catalyst is higher than that of traditional iron-based and nickel-based catalysts. The increase in the A-center nitrogen content indicates that the nitrogen content in the aggregated form has increased, which is closer to natural diamond.
[0081] At this point, those skilled in the art should recognize that, although multiple exemplary embodiments of the present invention have been shown and described in detail herein, many other variations or modifications that conform to the principles of the present invention can still be directly determined or derived based on the content disclosed in the present invention without departing from the spirit and scope of the present invention. Therefore, the scope of the present invention should be understood and recognized as covering all these other variations or modifications.
Claims
1. A method for growing large-size single crystal diamond with high nitrogen content using a cobalt catalyst, characterized in that: Assembling a carbon source, a metal catalyst and a diamond seed crystal into a synthesis block; The synthesis block is placed in a synthesis chamber of a high-pressure device, and a single crystal diamond is obtained under the conditions of a synthesis pressure of 5.5 GPa to 6.0 GPa, a synthesis temperature of 1400° C. to 1500° C., and a synthesis time of 20 h to 25 h; The carbon source is flake graphite with a purity of not less than 99.99%, the catalyst is a metal cobalt sheet with a purity of not less than 99.99%, and the diamond seed crystal is a {100} face or a {111} face of diamond.
2. The method for growing large-size single crystal diamond with high nitrogen using cobalt catalyst according to claim 1, characterized in that: The high-voltage equipment is a hinged six-sided top.
3. The method for growing large-size single crystal diamond with high nitrogen content using a cobalt catalyst according to claim 1 or 2, characterized in that: The internal temperature of the synthesis cavity is calibrated according to the relationship curve between input power and temperature measured by a double platinum-rhodium thermocouple; The internal pressure of the synthetic cavity is calibrated by a calibration curve of oil pressure and internal pressure of the cavity established according to the high-pressure phase transition points of bismuth, barium and thallium.
4. The method for growing large-size single crystal diamond with high nitrogen content using a cobalt catalyst according to claim 3, characterized in that: Before being assembled into the synthetic block, the carbon source, the metal catalyst and the diamond seed crystal are stored in a drying oven.
5. The method for growing large-size single crystal diamond with high nitrogen using cobalt catalyst according to claim 3, characterized in that: Before the synthetic block is placed in the high-pressure equipment, it is dried in an oven for 1 hour to 3 hours for dehydration treatment, and the drying temperature is 110° C. to 130° C.
Citation Information
Patent Citations
Method for growing large-particle diamond at high temperature and high pressure
CN112892411A
Method for batch growth and regulation of high-nitrogen gem-grade diamond single crystals
CN117888195A
A method for producing diamond material
WO2008007336A2