High-performance polyacrylonitrile carbon fiber precursor as well as preparation method and application thereof

By adopting a gradient cooling drying and densification process in the carbon fiber preparation process, the problem of electrostatic wear of wet fibers is solved, the mechanical properties and production efficiency of carbon fibers are improved, and the continuous production of high-performance carbon fibers is achieved.

CN118996652APending Publication Date: 2024-11-22CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310555546.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

There are problems of excessive ash and poor mechanical properties in the existing carbon fiber preparation processes, especially due to the electrostatic phenomenon caused by the rough surface structure of wet fibers, resulting in fiber wear and holes, which affects the performance of carbon fibers.

Method used

The drying densification process of gradient cooling is adopted. During the drying process, the temperature difference is controlled within 28℃, which reduces friction between fibers and static electricity generation, optimizes the charge distribution on the surface of fibers, reduces the generation of wool filaments, and improves the strength and mode of carbon fibers. quantity.

Benefits of technology

It effectively reduces the generation of ash during carbonization, improves the tensile strength, modulus and elongation of carbon fibers, realizes the preparation of high-performance carbon fibers, and supports continuous production, improving production efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a high-performance polyacrylonitrile carbon fiber precursor and a preparation method thereof, and mainly solves the problems of high ash content and poor mechanical properties of carbon fibers in the carbonization process in the prior art. According to the technical scheme, wet spinning is adopted, the method comprises the step of drying and densifying, in the drying and densifying process of oiled fibers, gradient cooling is conducted between at least two adjacent temperature zones, the temperature difference is not higher than 28 DEG C, and the temperature of the last drying temperature zone is not higher than 100 DEG C. By adopting the technical scheme provided by the invention, the technical problems are well solved, and the method can be applied to industrial production of the polyacrylonitrile carbon fiber precursor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon fiber, and specifically relates to a high-performance polyacrylonitrile carbon fiber precursor and a preparation method and application thereof. Background Art

[0002] In today's world, science and technology are developing rapidly, and the demand for high-performance materials is increasing. Among many high-performance fiber materials, carbon fiber is widely used in national defense, aerospace, automobile manufacturing, wind turbine blades, gas cylinders, bridge construction, bicycles, golf clubs, fishing rods, rackets and other civilian products due to its low density, light weight, high strength, high modulus, good creep resistance, low thermal expansion coefficient, low friction coefficient, good conductivity, high and low temperature resistance and corrosion resistance. It has become one of the fastest-growing high-performance materials in recent years. Therefore, in-depth research and optimization of carbon fiber preparation technology and structural properties, so as to stably prepare high-performance carbon fiber, is the key to promoting the development of carbon fiber reinforced composite materials.

[0003] At present, carbon fiber can be divided into polyacrylonitrile (PAN) carbon fiber, viscose-based carbon fiber, asphalt-based carbon fiber, and phenolic-based carbon fiber according to the type of precursor. Among them, PAN fiber occupies more than 90% of the carbon fiber precursor market due to its high melting point, high carbon yield (greater than 50% of the original precursor mass) and fast pyrolysis rate. It is the most widely used carbon fiber and has become the most suitable precursor material for producing high-performance carbon fiber. The solution of high-performance PAN carbon fiber precursor mainly uses dimethyl sulfoxide as a solvent, which has the characteristics of low toxicity and high solubility of PAN copolymers. PAN fiber is mainly prepared by wet spinning and dry-jet wet spinning. The wet spinning process has a longer development history than the dry-jet wet spinning process and is more mature. The spinning process is stable and easy to control, the residual solvent in the fiber is easy to remove, and the obtained carbon fiber is easier to combine with composite materials. It is the main process method for preparing high-performance carbon fiber precursor.

[0004] The microstructure of a material determines its macroscopic properties. The strength of carbon fiber is subject to various defects, such as internal and external holes, cracks and contaminants. These defects make it impossible for carbon fiber to evenly distribute stress in the radial direction under the action of the force field, which greatly limits the improvement of the mechanical properties of carbon fiber. As the mother of carbon fiber, the structure and defects of carbon fiber precursor are hereditary, which is the key to determining the performance of carbon fiber. That is, only high-quality carbon fiber precursor can produce high-performance carbon fiber. Therefore, PAN carbon fiber precursor should have the characteristics of homogeneity, few internal and external defects, perfect crystallization, and regular orientation. In the wet spinning process of PAN fiber, the drying and densification process will have an important influence on the formation and regularity of the aggregated structure of the precursor, as well as the size of holes and defects. During the drying and densification process, the moisture inside the fiber escapes quickly, the radial structure becomes denser, and the hole defects inside and on the surface are greatly reduced. However, due to the rough groove structure on the surface of the wet fiber, the friction between the fibers and between the fibers and the guide rollers during the drying process will inevitably generate static electricity. Especially after leaving the drying area, the temperature of the fiber drops rapidly, the aggregated structure loses its mobility and shrinks and solidifies, and the surface charge inside and between the fibers is redistributed, making the fiber belt more positive / negatively charged than before, and the surface potential changes. In addition, the surface charge of the fiber is generated quickly, the conductivity is poor, and it is difficult to remove it through the guide roller, which will inevitably have an adverse effect on the closure of the hole defects inside and on the surface of the fiber, and will also cause the fiber to wear and increase the number of hairs, all of which will have an adverse effect on the performance of the final carbon fiber.

[0005] However, although there are many studies on the drying and densification process, the surface potential of the fiber during the spinning process has not been measured, nor has the electrostatic phenomenon of the fiber during the spinning process, especially the drying and densification stage, been mentioned. Patents TW202104694A and WO2020203531A1 disclose a method for manufacturing flame-retardant carbon fiber, in which a polyacrylonitrile fiber bundle is placed in an oxidizing environment for flame retardant treatment at a temperature of 200 to 300°C, and the surface potential of the fiber bundle is set to -1kV to +1kV to prepare flame-retardant carbon fiber, but the electrostatic problem in the preparation process of the raw silk is not disclosed. Patent CN111088540A discloses a scheme for controlling the air humidity in the first drying and densification interval, but does not mention the electrostatic phenomenon and the problems caused by it. Patent CN110685041A discloses a technical solution in which the polyacrylonitrile precursor after the first drying and densification is soaked in a water bath, the moisture content of the precursor is controlled to be 5% to 20%, and then the second oiling and drying and densification are performed, but it mainly solves the problems of low-carbon furnace exhaust coke and excessive silica residue. Due to the rough groove structure on the surface of the wet fiber, the friction between the fibers and between the fibers and the guide rollers during the drying process will inevitably generate static electricity, making the fiber surface carry more positive / negative charges than before, which will inevitably cause the fiber to wear and increase the number of hairy fibers, all of which will have an adverse effect on the performance of the final carbon fiber.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] In order to solve the problems of high ash content and poor mechanical properties of carbon fiber in the carbonization process in the prior art, the present invention provides a method for preparing high-performance polyacrylonitrile carbon fiber precursor, which better solves the problem and has the advantages of low ash content in the carbonization process, no need to frequently stop the equipment for cleaning, less carbon fiber fuzz, high carbon fiber strength, high modulus and high elongation.

[0008] One of the purposes of the present invention is to provide a method for preparing high-performance polyacrylonitrile carbon fiber precursor, which adopts a wet spinning process, including a drying and densification step. During the drying and densification process, at least two adjacent temperature zones are cooled by gradient and the temperature difference is not higher than 28°C, and the temperature of the last temperature zone is not higher than 100°C.

[0009] According to some embodiments of the present invention, gradient cooling is adopted in some temperature zones during the drying and densification process. The preferred method is to first increase the temperature gradually and then decrease the temperature gradually. More preferably, the temperature difference of the gradient heating is not particularly limited, and is preferably not higher than 35°C; the temperature difference of the gradient cooling is not higher than 25°C, and the temperature of the last temperature zone is not higher than 95°C.

[0010] According to some embodiments of the present invention, the drying and densification process:

[0011] The drying and densification process includes at least 4 temperature zones;

[0012] The temperature of the drying and densification process is 80-150°C, and the residence time is 20-100s;

[0013] During the drying and densification process, the ratio of the length of the filament bundle between two adjacent drying rollers to the diameter of the drying roller is 0.3 to 1.8, preferably 0.4 to 1.7; the length of the filament bundle between two adjacent drying rollers refers to the filament bundle between two adjacent drying rollers that does not contact the drying rollers, and the total length of the filament bundle in this area is measured;

[0014] The maximum depth of the grooves on the fiber surface after drying and densification is 0.1 to 0.4 μm, preferably 0.12 to 0.35 μm; the maximum depth of the grooves on the fiber surface refers to the height difference between the highest groove peak and the lowest groove valley, which can be obtained by testing using a commonly used test method in the art;

[0015] The moisture content of the fiber after drying and densification is 0.3-2%, and the oil content is 0.5-2%; preferably, the moisture content of the fiber after drying and densification is 0.5-1.3%, and the oil content is 0.6-1.9%;

[0016] The surface potential of the fiber is -1.0 kV to +1.0 kV, preferably -800 V to +800 V.

[0017] According to some embodiments of the present invention, the preparation method specifically includes: wet coagulation molding of polyacrylonitrile stock solution, coagulation stretching, hot water stretching, water washing, oiling, drying densification, steam stretching, and steam heat setting to obtain the high-performance polyacrylonitrile carbon fiber precursor.

[0018] According to the present invention, the polyacrylonitrile stock solution is not particularly limited, and a polyacrylonitrile polymer solution commonly used in the art can be used. For example, but not limited to, the polyacrylonitrile comonomer is a vinyl-containing monomer, and the comonomer is preferably one or more of acrylates, vinyl esters, acrylamides, sulfonates, and ammonium salts. According to some embodiments of the present invention, the mass content of polyacrylonitrile in the polyacrylonitrile stock solution is 16.5-22.5%, preferably 17-22%; the intrinsic viscosity of the polyacrylonitrile stock solution is 2.8-5.5dL / g, preferably 3.0-5.1dL / g.

[0019] According to some embodiments of the present invention, the coagulation and stretching comprises at least three stages of coagulation and stretching; the temperature of the coagulation and stretching is 20-70° C.; and the total stretching ratio of the coagulation and stretching is 1-3.

[0020] According to some embodiments of the present invention, the hot water drawing includes at least four stages of hot water drawing; the temperature of the hot water drawing is 95-99° C.; the total drawing ratio of the hot water drawing is greater than or equal to 4 times, and the last stage of hot water drawing is greater than or equal to 1.5 times.

[0021] According to some embodiments of the present invention, the conditions for the steam stretching are: the steam pressure is 0.3-0.7 MPa, and the stretching ratio is greater than or equal to 3.

[0022] The second object of the present invention is to provide a high-performance polyacrylonitrile carbon fiber precursor prepared by the above preparation method.

[0023] The third object of the present invention is to provide a high-performance polyacrylonitrile carbon fiber prepared from the above-mentioned high-performance polyacrylonitrile carbon fiber precursor.

[0024] The present invention significantly affects the process of preparing high-performance carbon fiber from the precursor of high-performance polyacrylonitrile carbon fiber by adjusting the drying and densification process conditions, effectively reduces the generation of hair during the carbonization process, and the prepared carbon fiber has the characteristics of high strength, high modulus, and high toughness. The present invention firstly controls the drying and densification process by adopting a gradient cooling method, especially a method of first increasing the gradient and then decreasing the gradient, so as to avoid the static electricity generated by the friction between the fibers due to the sudden contraction of the fibers after leaving the drying temperature zone, resulting in the enlargement of the hole size in the fibers, the increase of defects, the generation of more hair during the carbonization process, and the adverse effect on the performance of the carbon fiber.

[0025] The drying and densification process conditions provided by the present invention can effectively improve the surface defects of carbon fiber precursors and improve the mechanical properties of carbon fiber. Moreover, the ash content is low during the carbonization process, and there is no need to frequently stop and clean the equipment, so as to realize the continuous industrial production of polyacrylonitrile carbon fiber precursors and improve production efficiency. Using the technical solution of the present invention, after continuous production for 3 months, the tensile strength of the prepared carbon fiber can reach 5.8GPa, the modulus can reach 388GPa, and the elongation can reach 1.6%, achieving good technical effects. DETAILED DESCRIPTION

[0026] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0027] The test instruments and test conditions used in the examples are as follows:

[0028] The groove depth on the fiber surface (the height difference between the highest groove peak and the lowest groove valley) was observed at room temperature using a scanning probe atomic force microscope (Nanoscope IV, AFM, Veeco Instruments, USA). The AFM mode was used to repeatedly scan along the single fiber surface within a range of 2×2 μm with a scanning frequency of 2 Hz to obtain a two-dimensional image and read the height difference between the groove peaks and valleys within the 2×2 μm image range.

[0029] The moisture / oil content of the fiber is measured according to the following method: take a certain amount of fiber sample, measure its mass and record it as W0, dry it at 105°C for 2 hours, measure its mass and record it as W1, place the sample in a Soxhlet extractor, add several or one of cyclohexane, acetone, ethanol (or an appropriate organic solvent in gas), heat it to 50°C, and extract it for 4 hours. Take out the sample, dry it at 105°C for 2 hours, measure its mass and record it as W2. The formula for calculating the moisture content of the fiber is: Moisture content (wt%) = (W1-W0) / W0. The formula for calculating the oil content of the fiber is: Oil content (wt%) = (W1-W2) / W1.

[0030] The surface potential of the fiber is measured using a SK-H050 series electrostatic measuring instrument. The vertical distance between the electrostatic measuring instrument and the fiber bundle surface is 25 mm. The measuring distance is based on the position where the linear laser and the point laser of the measuring instrument overlap.

[0031] The mechanical properties of carbon fiber precursor are measured using GB / T14337-2008; the mechanical properties of carbon fiber are measured using GB / T3362-2017. A lot of ash is generated during the carbonization process, and the furnace needs to be stopped and the ash needs to be cleaned every once in a while. If continuous production can be achieved for more than 3 months without affecting the performance of the carbon fiber, less ash is generated during the carbonization process.

[0032] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0033] [Example 1]

[0034] 1. Preparation of high-performance polyacrylonitrile carbon fiber precursor, using wet spinning method, the characteristic viscosity of the spinning solution used is 3.5dL / g, solid content is 18%, the spinning solution is accurately measured and filtered by a metering pump, extruded through a spinneret with 6000 holes and pore size of 60μm, and enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation, the coagulation temperature is 28℃, the concentration is 51.5%, and then undergoes three-stage coagulation and drawing, the temperature is 30℃, 40℃, 50℃, and the drawing ratio is 1.0, 1.1, 1.2 respectively; then undergoes four-stage hot water drawing, the temperature is 95℃, 96℃, 97℃, 99℃, and the drawing ratio is 1.35, 1.50, 1.70, 2.00 respectively; after oiling, four-stage drying and densification The fiber was treated by steam drawing with a drawing ratio of 3.0 times and a steam pressure of 0.35 MPa. The fiber was heat-set and collected to obtain high-performance polyacrylonitrile carbon fiber precursor with a linear density of 0.85 dtex, and a tensile strength, modulus and elongation of 7.5 cN / dtex, 125 cN / dtex and 12.0% respectively.

[0035] 2. Preparation of high-performance carbon fiber: pre-oxidize the raw silk obtained in step 1 at 180-260°C with a draft of 2% to obtain pre-oxidized fiber; then perform low-temperature carbonization and high-temperature carbonization at 300-750°C and 800-1500°C with a draft of 3% and -3%, respectively; then perform graphitization at 2800°C, and finally perform surface treatment, water washing, sizing, drying at 120°C and collecting to obtain high-performance carbon fiber.

[0036] After 4 months of continuous production, the carbon fiber had a tensile strength of 5.7 GPa, a modulus of 377 GPa, and an elongation of 1.5%.

[0037] [Example 2]

[0038] 1. The preparation of precursor for high-performance polyacrylonitrile carbon fiber adopts wet spinning method. The characteristic viscosity of the spinning solution used is 4.8dL / g and the solid content is 17%. The spinning solution is accurately measured and filtered by a metering pump, extruded through a spinneret with 6000 holes and a pore size of 60μm, and enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation. The coagulation temperature is 28℃ and the concentration is 51.5%. Then, it undergoes three-stage coagulation and drawing at temperatures of 40℃, 50℃, and 60℃, respectively, and the drawing ratios are 1.1, 1.2, and 1.25, respectively; then it undergoes four-stage hot water drawing at temperatures of 97℃, 98℃, 98℃, and 99℃, respectively, and the drawing ratios are 1.35, 1.50, 1.75, and 2.20, respectively; after oiling, it undergoes four-stage drying and densification The fiber was treated by steam drawing with a drawing ratio of 3.3 times and a steam pressure of 0.38 MPa. After heat setting and winding, high-performance polyacrylonitrile carbon fiber precursor was obtained. The linear density of the precursor was 0.70 dtex, and the tensile strength, modulus and elongation were 8.1 cN / dtex, 137 cN / dtex and 11.8%, respectively.

[0039] 2. Preparation of high-performance carbon fiber: pre-oxidize the raw silk obtained in step 1 at 180-260°C with a draft of 2% to obtain pre-oxidized fiber; then perform low-temperature carbonization and high-temperature carbonization at 300-750°C and 800-1500°C with a draft of 3% and -3%, respectively; then perform graphitization at 2800°C, and finally perform surface treatment, water washing, sizing, drying at 120°C and collecting to obtain high-performance carbon fiber.

[0040] After 4 months of continuous production, the carbon fiber had a tensile strength of 5.78 GPa, a modulus of 382 GPa, and an elongation of 1.34%.

[0041] [Example 3]

[0042] 1. The preparation of precursor for high-performance polyacrylonitrile carbon fiber adopts wet spinning method. The characteristic viscosity of the spinning solution used is 3.0dL / g and the solid content is 22%. The spinning solution is accurately measured and filtered by a metering pump, extruded through a spinneret with 6000 holes and a pore size of 60μm, and enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation. The coagulation temperature is 28°C and the concentration is 51.5%. Then, it undergoes three-stage coagulation and drawing at temperatures of 35°C, 45°C, and 55°C, respectively, and the drawing ratios are 1.01, 1.1, and 1.15, respectively; then it undergoes four-stage hot water drawing at temperatures of 96°C, 97°C, 97°C, and 99°C, respectively, and the drawing ratios are 1.25, 1.45, 1.75, and 2.00, respectively; after oiling, it undergoes four-stage drying and densification The fiber was treated by steam drawing with a drawing ratio of 3.1 times and a steam pressure of 0.30 MPa. The high-performance polyacrylonitrile carbon fiber precursor was obtained by heat setting and collecting. The linear density of the precursor was 0.88 dtex, and the tensile strength, modulus and elongation were 7.2 cN / dtex, 119 cN / dtex and 12.5%, respectively.

[0043] 2. Preparation of high-performance carbon fiber: pre-oxidize the raw silk obtained in step 1 at 180-260°C with a draft of 2% to obtain pre-oxidized fiber; then perform low-temperature carbonization and high-temperature carbonization at 300-750°C and 800-1500°C with a draft of 3% and -3%, respectively; then perform graphitization at 2800°C, and finally perform surface treatment, water washing, sizing, drying at 120°C and collecting to obtain high-performance carbon fiber.

[0044] After three months of continuous production, the carbon fiber had a tensile strength of 5.66 GPa, a modulus of 365 GPa, and an elongation of 1.6%.

[0045] [Example 4]

[0046] 1. The preparation of precursor for high-performance polyacrylonitrile carbon fiber adopts wet spinning method. The characteristic viscosity of the spinning solution used is 4.0dL / g and the solid content is 20%. The spinning solution is accurately measured and filtered by a metering pump, extruded through a spinneret with 6000 holes and a pore size of 60μm, and enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation. The coagulation temperature is 28°C and the concentration is 51.5%. Then, it undergoes three-stage coagulation and drawing, and the temperatures are 32°C, 42°C, and 52°C, respectively, and the drawing ratios are 1.05, 1.15, and 1.21, respectively; then it undergoes four-stage hot water drawing, and the temperatures are 95°C, 96°C, 98°C, and 99°C, respectively, and the drawing ratios are 1.35, 1.45, 1.80, and 2.20, respectively; after oiling, it is dried in four stages Densification treatment, the ratio of the length of the filament bundle leaving the drying roller between two adjacent drying rollers to the diameter of the drying roller is 0.4-1, the temperature is 115℃, 140℃, 117℃ and 95℃ respectively, the residence time is 20s, the fiber surface potential is -600V, the maximum height difference between adjacent protrusions and grooves of the fiber surface grooves after drying is 0.3μm, and the fiber water content and oil content are 0.9% and 1.3% respectively; then it is steam drawn with a drawing ratio of 3.2 times and a steam pressure of 0.35MPa; finally, after heat setting and winding, high-performance polyacrylonitrile carbon fiber precursor is obtained, the linear density of the precursor is 0.72dtex, and the tensile strength, modulus and elongation are 7.6cN / dtex, 128cN / dtex and 11.2% respectively.

[0047] 2. Preparation of high-performance carbon fiber: pre-oxidize the raw silk obtained in step 1 at 180-260°C with a draft of 2% to obtain pre-oxidized fiber; then perform low-temperature carbonization and high-temperature carbonization at 300-750°C and 800-1500°C with a draft of 3% and -3%, respectively; then perform graphitization at 2800°C, and finally perform surface treatment, water washing, sizing, drying at 120°C and collecting to obtain high-performance carbon fiber.

[0048] After three months of continuous production, the carbon fiber had a tensile strength of 5.75 GPa, a modulus of 374 GPa, and an elongation of 1.55%.

[0049] [Example 5]

[0050] 1. The preparation of precursor for high-performance polyacrylonitrile carbon fiber adopts wet spinning method. The characteristic viscosity of the spinning solution used is 3.6dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, extruded through a spinneret with 6000 holes and a pore size of 60μm, and enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation. The coagulation temperature is 28°C and the concentration is 51.5%. Then, it undergoes three-stage coagulation and drawing at temperatures of 37°C, 47°C, and 57°C, respectively, and the drawing ratios are 1.02, 1.15, and 1.20, respectively; then it undergoes four-stage hot water drawing at temperatures of 96°C, 97°C, 97°C, and 99°C, respectively, and the drawing ratios are 1.30, 1.45, 1.75, and 2.20, respectively; after oiling, it undergoes four-stage drying and densification The fiber was subjected to chemical treatment, the ratio of the length of the filament bundle leaving the drying roller between two adjacent drying rollers to the diameter of the drying roller was 0.7-1.5, the temperatures were 90°C, 120°C, 115°C and 90°C, the residence time was 80s, the fiber surface potential was +280V, the maximum height difference between adjacent protrusions and grooves of the fiber surface grooves after drying was 0.2μm, and the fiber water content and oil content were 1.13% and 0.96%, respectively; then it was steam drawn with a drawing ratio of 3.1 times and a steam pressure of 0.35MPa; finally, after heat setting and winding, high-performance polyacrylonitrile carbon fiber precursor was obtained, the linear density of the precursor was 0.78dtex, and the tensile strength, modulus and elongation were 7.4cN / dtex, 126cN / dtex and 11.5%, respectively.

[0051] 2. Preparation of high-performance carbon fiber: pre-oxidize the raw silk obtained in step 1 at 180-260°C with a draft of 2% to obtain pre-oxidized fiber; then perform low-temperature carbonization and high-temperature carbonization at 300-750°C and 800-1500°C with a draft of 3% and -3%, respectively; then perform graphitization at 2800°C, and finally perform surface treatment, water washing, sizing, drying at 120°C and collecting to obtain high-performance carbon fiber.

[0052] After 5 months of continuous production, the carbon fiber had a tensile strength of 5.72 GPa, a modulus of 372 GPa, and an elongation of 1.54%.

[0053] [Example 6]

[0054] 1. The preparation of precursor for high-performance polyacrylonitrile carbon fiber adopts wet spinning method. The intrinsic viscosity of the spinning solution used is 5.1dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, extruded through a spinneret with 6000 holes and a pore size of 60μm, and enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation. The coagulation temperature is 28℃ and the concentration is 51.5%. Then, it undergoes three-stage coagulation and drawing at temperatures of 40℃, 50℃, and 60℃, respectively, and the drawing ratios are 1, 1.1, and 1.2, respectively; then it undergoes four-stage hot water drawing at temperatures of 97℃, 98℃, 98℃, and 99℃, respectively, and the drawing ratios are 1.35, 1.5, 1.7, and 2, respectively; after oiling, it undergoes four-stage drying and densification treatment. The ratio of the length of the filament bundle leaving the drying roller between two adjacent drying rollers to the diameter of the drying roller is 0.8-1.7, the temperatures are 85°C, 105°C, 100°C and 85°C, respectively, the residence time is 100s, the fiber surface potential is +800V, and the maximum height difference between adjacent protrusions and grooves of the fiber surface grooves after drying is 0.12μm, and the fiber water content and oil content are 1.21% and 1.5%, respectively; then it is steam drawn, the drawing ratio is 3.1 times, and the steam pressure is 0.35MPa; finally, after heat setting and winding, high-performance polyacrylonitrile carbon fiber precursor is obtained, the linear density of the precursor is 0.86dtex, and the tensile strength, modulus and elongation are 8.5cN / dtex, 139cN / dtex and 12%, respectively.

[0055] 2. Preparation of high-performance carbon fiber: pre-oxidize the raw silk obtained in step 1 at 180-260°C with a draft of 2% to obtain pre-oxidized fiber; then perform low-temperature carbonization and high-temperature carbonization at 300-750°C and 800-1500°C with a draft of 3% and -3%, respectively; then perform graphitization at 2800°C, and finally perform surface treatment, water washing, sizing, drying at 120°C and collecting to obtain high-performance carbon fiber.

[0056] After three months of continuous production, the carbon fiber had a tensile strength of 5.81 GPa, a modulus of 388 GPa, and an elongation of 1.31%.

[0057] [Comparative Example 1]

[0058] 1. The preparation of precursor for high-performance polyacrylonitrile carbon fiber adopts wet spinning method. The characteristic viscosity of the spinning solution used is 3.5dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, extruded through a spinneret with 6000 holes and a pore size of 60μm, and enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation. The coagulation temperature is 28℃ and the concentration is 51.5%. Then, it undergoes three-stage coagulation and drawing at temperatures of 30℃, 40℃, and 50℃, respectively, and the drawing ratios are 1.0, 1.1, and 1.2, respectively; then it undergoes four-stage hot water drawing at temperatures of 95℃, 96℃, 97℃, and 99℃, respectively, and the drawing ratios are 1.35, 1.50, 1.70, and 2.00, respectively; after oiling, it undergoes four-stage drying and densification treatment The ratio of the length of the filament bundle leaving the drying roller between two adjacent drying rollers to the diameter of the drying roller is 0.5-1.1, the temperatures are 105°C, 135°C, 120°C and 105°C, respectively, the residence time is 50s, the fiber surface potential is -2.0kV, the maximum height difference between adjacent protrusions and grooves of the fiber surface grooves after drying is 0.4μm, and the fiber water content and oil content are 1.05% and 2.2%, respectively; then it is steam drawn with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, after heat setting and winding, high-performance polyacrylonitrile carbon fiber precursor is obtained, the linear density of the precursor is 0.85dtex, and the tensile strength, modulus and elongation are 7.4cN / dtex, 128cN / dtex and 11.7%, respectively.

[0059] 2. Preparation of high-performance carbon fiber: pre-oxidize the raw silk obtained in step 1 at 180-260°C with a draft of 2% to obtain pre-oxidized fiber; then perform low-temperature carbonization and high-temperature carbonization at 300-750°C and 800-1500°C with a draft of 3% and -3%, respectively; then perform graphitization at 2800°C, and finally perform surface treatment, water washing, sizing, drying at 120°C and collecting to obtain high-performance carbon fiber.

[0060] After 1.5 months of continuous production, the carbon fiber had a tensile strength of 4.8 GPa, a modulus of 347 GPa, and an elongation of 1.30%.

[0061] [Comparative Example 2]

[0062] 1. The preparation of precursor for high-performance polyacrylonitrile carbon fiber adopts wet spinning method. The characteristic viscosity of the spinning solution used is 3.8dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, extruded through a spinneret with 6000 holes and a pore size of 60μm, and enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation. The coagulation temperature is 28℃ and the concentration is 51.5%. Then, it undergoes three-stage coagulation and drawing at temperatures of 40℃, 50℃, and 60℃, respectively, and the drawing ratios are 1.05, 1.15, and 1.25, respectively; then it undergoes four-stage hot water drawing at temperatures of 97℃, 98℃, 98℃, and 99℃, respectively, and the drawing ratios are 1.30, 1.50, 1.80, and 2.30, respectively; after oiling, it undergoes four-stage drying and densification The fiber was treated by steam drawing with a drawing ratio of 3.3 times and a steam pressure of 0.38 MPa. Finally, the fiber was heat-set and collected to obtain high-performance polyacrylonitrile carbon fiber precursor with a linear density of 0.70 dtex, a tensile strength, a modulus and an elongation of 7.9 cN / dtex, 136 cN / dtex and 11.3%.

[0063] 2. Preparation of high-performance carbon fiber: pre-oxidize the raw silk obtained in step 1 at 180-260°C with a draft of 2% to obtain pre-oxidized fiber; then perform low-temperature carbonization and high-temperature carbonization at 300-750°C and 800-1500°C with a draft of 3% and -3%, respectively; then perform graphitization at 2800°C, and finally perform surface treatment, water washing, sizing, drying at 120°C and collecting to obtain high-performance carbon fiber.

[0064] After 2 months of continuous production, the carbon fiber had a tensile strength of 5.1 GPa, a modulus of 351 GPa, and an elongation of 1.2%.

[0065] [Comparative Example 3]

[0066] 1. The preparation of precursor for high-performance polyacrylonitrile carbon fiber adopts wet spinning method. The characteristic viscosity of the spinning solution used is 3.6dL / g and the solid content is 19%. The spinning solution is accurately measured and filtered by a metering pump, extruded through a spinneret with 6000 holes and a pore size of 60μm, and enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation. The coagulation temperature is 28°C and the concentration is 51.5%. Then, it undergoes three-stage coagulation and drawing at temperatures of 35°C, 45°C, and 55°C, respectively, and the drawing ratios are 1.00, 1.10, and 1.20, respectively; then it undergoes four-stage hot water drawing at temperatures of 96°C, 97°C, 97°C, and 99°C, respectively, and the drawing ratios are 1.20, 1.60, 1.75, and 2.10, respectively; after oiling, it undergoes four-stage drying and densification The fiber was treated by a steam drawing method with a drawing ratio of 3.0 times and a steam pressure of 0.30 MPa. The fiber was then heat-set and collected to obtain high-performance polyacrylonitrile carbon fiber precursor with a linear density of 0.86 dtex, and a tensile strength, modulus and elongation of 7.7 cN / dtex, 130 cN / dtex and 11.5% respectively.

[0067] 2. Preparation of high-performance carbon fiber: pre-oxidize the raw silk obtained in step 1 at 180-260°C with a draft of 2% to obtain pre-oxidized fiber; then perform low-temperature carbonization and high-temperature carbonization at 300-750°C and 800-1500°C with a draft of 3% and -3%, respectively; then perform graphitization at 2800°C, and finally perform surface treatment, water washing, sizing, drying at 120°C and collecting to obtain high-performance carbon fiber.

[0068] After 1.5 months of continuous production, the carbon fiber had a tensile strength of 4.6 GPa, a modulus of 340 GPa, and an elongation of 1.35%.

[0069] [Comparative Example 4]

[0070] 1. The preparation of precursor for high-performance polyacrylonitrile carbon fiber adopts wet spinning method. The characteristic viscosity of the spinning solution used is 3.7dL / g and the solid content is 19%. The spinning solution is accurately measured and filtered by a metering pump, extruded through a spinneret with 6000 holes and a pore size of 60μm, and enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation. The coagulation temperature is 28°C and the concentration is 51.5%. Then, it undergoes three-stage coagulation and drawing at temperatures of 37°C, 47°C, and 57°C, respectively, and the drawing ratios are 1.01, 1.05, and 1.15, respectively; then it undergoes four-stage hot water drawing at temperatures of 95°C, 96°C, 97°C, and 99°C, respectively, and the drawing ratios are 1.30, 1.60, 1.80, and 2.10, respectively; after oiling, it undergoes four-stage drying and densification The fiber was treated by a steam drawing method with a ratio of the length of the filament bundle leaving the drying roller between two adjacent drying rollers to the diameter of the drying roller being 1.3-1.9, the temperatures being 100°C, 130°C, 125°C and 95°C, respectively, the residence time being 20s, the fiber surface potential being -1.8kV, the maximum height difference between adjacent protrusions and grooves of the fiber surface grooves after drying being 0.37μm, and the fiber water content and oil content being 1.1% and 1.95%, respectively; then the fiber was subjected to steam drawing with a drawing ratio of 3.2 times and a steam pressure of 0.35MPa; finally, the fiber was subjected to heat setting and winding to obtain high-performance polyacrylonitrile carbon fiber precursor with a linear density of 0.85dtex, and a tensile strength, modulus and elongation of 7.5cN / dtex, 126cN / dtex and 11.7%, respectively.

[0071] 2. Preparation of high-performance carbon fiber: pre-oxidize the raw silk obtained in step 1 at 180-260°C with a draft of 2% to obtain pre-oxidized fiber; then perform low-temperature carbonization and high-temperature carbonization at 300-750°C and 800-1500°C with a draft of 3% and -3%, respectively; then perform graphitization at 2800°C, and finally perform surface treatment, water washing, sizing, drying at 120°C and collecting to obtain high-performance carbon fiber.

[0072] After 2 months of continuous production, the carbon fiber had a tensile strength of 4.7 GPa, a modulus of 344 GPa, and an elongation of 1.25%.

Claims

1. A method for preparing high-performance polyacrylonitrile carbon fiber precursor, using a wet spinning process, which includes a drying and densification step. During the drying and densification process, at least two adjacent temperature zones are cooled by gradient and the temperature difference is not higher than 28°C, and the temperature of the last temperature zone is not higher than 100°C.

2. The preparation method according to claim 1, It is characterized in that The temperature difference of the gradient cooling is not higher than 25°C; and / or, The temperature of the last temperature zone is not higher than 95°C.

3. The preparation method according to claim 1, It is characterized in that The drying and densification process includes at least 4 temperature zones; and / or, The temperature of the drying and densification process is 80-150° C., and the residence time is 20-100 seconds.

4. The preparation method according to claim 1, It is characterized in that During the drying and densification process, the ratio of the length of the filament bundle between two adjacent drying rollers to the diameter of the drying rollers is 0.3 to 1.8, preferably 0.4 to 1.7; and / or, The maximum depth of the grooves on the fiber surface after drying and densification is 0.1 to 0.4 μm, preferably 0.12 to 0.35 μm; and / or, The moisture content of the fiber after drying and densification is 0.3-2%, and the oil content is 0.5-2%; preferably, the moisture content of the fiber after drying and densification is 0.5-1.3%, and the oil content is 0.6-1.9%; and / or, The surface potential of the fiber is -1.0 kV to +1.0 kV, preferably -800 V to +800 V.

5. The preparation method according to any one of claims 1 to 4, It is characterized in that The preparation method specifically comprises the steps of wet coagulation molding of polyacrylonitrile stock solution, coagulation drawing, hot water drawing, water washing, oiling, drying and densification, steam drawing and steam heat setting to obtain the high-performance polyacrylonitrile carbon fiber precursor.

6. The preparation method according to claim 5, It is characterized in that The mass content of polyacrylonitrile in the polyacrylonitrile stock solution is 16.5-22.5%, preferably 17-22%; and / or, The intrinsic viscosity of the polyacrylonitrile stock solution is 2.8 to 5.5 dL / g, preferably 3.0 to 5.1 dL / g.

7. The preparation method according to claim 5, It is characterized in that The coagulation and stretching comprises at least three stages of coagulation and stretching; and / or, The coagulation and stretching temperature is 20 to 70° C.; and / or, The total drawing ratio of the coagulation drawing is 1-3.

8. The preparation method according to claim 5, It is characterized in that The hot water drawing comprises at least four levels of hot water drawing; and / or, The temperature of the hot water drawing is 95-99° C.; and / or, The total drawing ratio of the hot water drawing is greater than or equal to 4 times, and the last stage of hot water drawing is greater than or equal to 1.5 times.

9. The preparation method according to claim 5, It is characterized in that The conditions for the steam drawing are: the steam pressure is 0.3-0.7 MPa, and the drawing ratio is greater than or equal to 3.

10. A high-performance polyacrylonitrile carbon fiber precursor prepared by the preparation method according to any one of claims 1 to 9.

11. A high-performance polyacrylonitrile carbon fiber prepared from the high-performance polyacrylonitrile carbon fiber precursor according to claim 10.

Citation Information

Patent Citations

  • Preparation method of polyacrylonitrile-based carbon fiber

    CN110685041A

  • Preparation method of high-performance polyacrylonitrile fibers

    CN111088540A

  • Method for producing flame-proof fiber bundle, and method for producing carbon fiber bundle

    TW202104694A

  • Method for producing flame-proof fiber bundle, and method for producing carbon fiber bundle

    WO2020203531A1

Cited By

  • Polyacrylonitrile precursor fiber and carbon fiber, and preparation methods therefor

    WO2026041107A1