Porous fiber monofilament with electromagnetic shielding performance and preparation method thereof

By employing wet spinning technology and the directional distribution of modified MXene, the problem of unsatisfactory electromagnetic shielding performance of fiber monofilaments in existing technologies has been solved, enabling the preparation of porous fiber monofilaments with high electromagnetic shielding effect at low filler concentrations, which is suitable for industrial production.

CN118996667APending Publication Date: 2024-11-22ZANGBALA (YUYAO) NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411387550.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-04
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing technologies struggle to prepare fiber monofilaments with excellent electromagnetic shielding performance at low levels of functional filler content, and existing methods suffer from unsatisfactory shielding performance, a stiff and heavy feel, and poor wearability.

Method used

By employing wet spinning technology and utilizing the interaction between modified MXene and Pluronic F127, modified MXene is in situ assembled onto the pore walls of porous polymer fiber monofilaments. The porous structure and directional distribution enhance the reflection loss of electromagnetic waves, thereby preparing porous fiber monofilaments.

Benefits of technology

Achieving high electromagnetic shielding effect at low filler concentration, the porous fiber monofilament has a diameter of 0.05–1 mm, a porosity of 40%–80%, a breaking strength greater than 5.0 cN/dtex, and an electromagnetic shielding effectiveness of over 30 dB, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996667A_ABST
    Figure CN118996667A_ABST
Patent Text Reader

Abstract

The invention relates to a porous fiber monofilament with electromagnetic shielding performance and a preparation method thereof, and belongs to the technical field of functional fiber preparation. The preparation method of the porous fiber monofilament with the electromagnetic shielding performance comprises the following steps: preparing modified MXene, dispersing the modified MXene, a polymer and pluronic F127 in a solvent to obtain a spinning solution, introducing the spinning solution into an ethanol / water mixed coagulating bath through a spinneret orifice to form a nascent fiber, stretching the nascent fiber, and forming in a water coagulating bath to obtain the porous fiber monofilament with the electromagnetic shielding performance. And finally, drying. The amphiphilic pluronic F127 interacts with the polymer and the modified MXene at the same time, so that the modified MXene is distributed on the pore wall of the porous polymer fiber monofilament. The diameter of the prepared porous fiber monofilament is 0.05-1 mm, the porosity is 40%-80%, the breaking strength is larger than 5.0 cN / dtex, and the electromagnetic shielding effectiveness within the frequency range of 8.2-12.4 GHz is 30 dB or above. The preparation method disclosed by the invention is simple to operate, low in cost and suitable for industrial continuous and mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a porous fiber monofilament with electromagnetic shielding performance and a preparation method thereof, belonging to the technical field of functionalized fiber preparation. Background Art

[0002] With the development of science and technology, electronic equipment has brought great convenience to people's production and life, but the electromagnetic radiation and interference generated by electronic equipment during work have also continuously affected people's production and life, making electromagnetic waves another new source of pollution after water, air, and noise pollution. Electromagnetic waves not only affect normal communications, but also cause irreversible damage to the human central nervous system, sympathetic nervous system, and genetic sequences of the genome. Usually, the harm of electromagnetic waves to the body can be reduced by wearing clothes, but ordinary clothes have only a weak electromagnetic shielding effect. Therefore, it is urgent to develop nanofibers with electromagnetic shielding properties to achieve the effect of electromagnetic shielding, thereby effectively protecting human health.

[0003] The research on electromagnetic radiation protection has lasted for half a century at home and abroad. The earliest electromagnetic radiation protection fabric appeared in the 1960s. It was a fabric made of metal wire and textile fiber. It has a certain shielding effect on electromagnetic radiation, but it feels hard, thick and heavy, and has poor wearing performance. On this basis, fabrics blended with metal fibers and textile fibers have appeared, and their wearing performance has been greatly improved. However, since it is difficult to mix these two fibers evenly, the shielding performance is not ideal, and there are also phenomena of tip discharge and piercing.

[0004] Chinese invention patent applications No. 202210959912.6 and No. 202310752223.2 obtain electromagnetic shielding polyarylether composite fibers by electrospinning, but electrospinning produces non-woven fabrics, not fiber monofilaments. Chinese invention patent application No. 201310036607.0 prepares special pellets mainly composed of spinning-grade polyetheretherketone resin, heat stabilizer, functional powder material and organic polymer additives, which are melted, filtered and single-hole spun in a spinning extruder to form polyetheretherketone monofilaments; then the polyetheretherketone initial spinning monofilaments are obtained through an oiling device, a bundling device and a drawing disk; finally, a heat stretching and heat setting device is introduced to obtain polyetheretherketone monofilaments with electromagnetic shielding function. Although this melt spinning preparation method can achieve good dispersion of functional powder materials in organic polymers, it requires a higher filler concentration to obtain a high electromagnetic shielding effect. In summary, how to prepare fiber monofilaments with electromagnetic shielding effect at a lower functional filler content so as to prepare wearable clothing with excellent electromagnetic shielding performance and achieve effective electromagnetic shielding protection for the human body is a challenge that needs to be urgently solved by technicians in this field. Summary of the invention

[0005] In view of this, the purpose of the present invention is to prepare non-woven fabrics rather than fiber monofilaments by electrostatic spinning. Although the preparation method of melt spinning can achieve good dispersion of functional powder materials in organic polymers, it requires a higher filler concentration to obtain a high electromagnetic shielding effect. A porous fiber monofilament with electromagnetic shielding performance and a preparation method thereof are provided. The present invention utilizes amphiphilic Pluronic F127 to interact with polymers and modified MXene at the same time, and the modified MXene is assembled in situ and distributed on the pore walls of the porous polymer fiber monofilament during wet spinning. The porous structure and the directional distribution of the modified MXene improve the multiple reflection loss of electromagnetic waves, and achieve a high electromagnetic shielding effect at a lower filler concentration.

[0006] Specifically, a modified MXene is first prepared, and then the modified MXene, polymer and Pluronic F127 are dispersed in a solvent to obtain a spinning solution. The spinning solution is introduced into an ethanol / water mixed coagulation bath through a spinneret to form a primary fiber. The primary fiber is stretched and formed in a water coagulation bath, and finally dried to prepare a porous fiber monofilament with electromagnetic shielding performance. The preparation method of the porous fiber monofilament with electromagnetic shielding performance is simple to operate and low in cost, and is suitable for industrial continuous and mass production. The prepared porous fiber monofilament with electromagnetic shielding performance has a diameter of 0.05 to 1 mm, a porosity of 40% to 80%, a breaking strength greater than 5.0 cN / dtex, and an electromagnetic shielding effectiveness of more than 30 dB in the frequency range of 8.2 to 12.4 GHz.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] The first technical purpose of the present invention is to provide a porous fiber monofilament with electromagnetic shielding performance, which is composed of 60-95 wt% of a polymer, 5-40 wt% of a modified MXene and 2-10 wt% of Pluronic F127, wherein the modified MXene is distributed on the pore wall of the porous polymer fiber monofilament through Pluronic F127 as a connector.

[0009] It should be noted that the diameter of the porous fiber monofilament with electromagnetic shielding performance is 0.05 to 1 mm, and the porosity is 40% to 80%.

[0010] Furthermore, the breaking strength of the porous fiber monofilament with electromagnetic shielding performance is greater than 5.0 cN / dtex, and the electromagnetic shielding effectiveness in the frequency range of 8.2 to 12.4 GHz is greater than 30 dB.

[0011] Furthermore, the polymer matrix of the porous fiber monofilament with electromagnetic shielding performance is one of polyarylether nitrile, polyarylether ketone, polyarylether sulfone, polyimide, polyetherimide, polyarylether nitrile-polyarylether ketone binary copolymer, polyarylether nitrile-polyarylether sulfone binary copolymer, polyarylether ketone-polyarylether sulfone binary copolymer, polyimide-polyetherimide binary copolymer, polyarylether nitrile-polyarylether ketone-polyarylether sulfone terpolymer.

[0012] Furthermore, the preparation method of the modified MXene is as follows:

[0013] Mix 1 part of lithium fluoride and 10-100 parts of 37% concentrated hydrochloric acid in a PTFE container and stir to obtain a uniform mixture, then add 0.5-1 part of titanium aluminum carbide, and etch at 30-60 ° C for 24-48 hours; the product is centrifuged at 1000-3000 rpm to remove the supernatant, and deionized water washing and centrifugation are repeated until the pH is neutral; 5-20 parts of deionized water are added again, ultrasonicated at 50-500 W for 1-2 hours, and further centrifuged at 1000-5000 rpm for 30-60 minutes to remove large pieces of unpeeled MAX products, and the supernatant is filtered to obtain MXene; MXene is dispersed in deionized water to prepare a dispersion with a mass concentration of 5-30 wt%, and 0.5-5 times the mass of MXene polyethyleneimine is added, and stirred at a speed of 100-500 rpm for 3-8 h, then centrifuged at 3000-10000 rpm, and finally dried in vacuum at room temperature for 24-48 h to obtain the modified MXene.

[0014] A further beneficial effect of the above method is that the MXene after etching and stripping is a nanomaterial with excellent conductive properties; and the surface of MXene is electronegative, and the electropositive polyethyleneimine can be coated on the surface of MXene through electrostatic action to achieve hydrophilic modification of MXene.

[0015] The second technical purpose of the present invention is to provide a method for preparing the porous fiber monofilament having electromagnetic shielding performance, the steps of which are as follows:

[0016] S1. Mixing the modified MXene and N-methylpyrrolidone A in a mass ratio of 1:20 to 100, and stirring to obtain a mixture;

[0017] S2, adding the polymer and Pluronic F127 to N-methylpyrrolidone B, stirring to obtain a uniform solution, wherein the mass ratio of the polymer to the modified MXene in S1 is 4:1-15:1, the mass ratio of Pluronic F127 to the modified MXene in S1 is 0.1:1-2:1, and the mass of N-methylpyrrolidone B is 1-3 times that of N-methylpyrrolidone A;

[0018] S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2 to obtain a spinning solution, then adding the solution to a spinning machine, and extruding the spinning solution from a spinneret hole to form a thin stream, wherein the spinneret hole has an aperture of 0.1 to 2 mm, and the speed at which the spinning solution is extruded from the spinneret hole to form a thin stream is 30 to 50 m / min;

[0019] S4, introducing the thin stream squeezed out from the spinneret in S3 into a coagulation bath 1 to form nascent fibers, wherein the coagulation bath 1 is a mixed coagulation bath of water and ethanol in a volume ratio of 1:1 to 4, and the residence time in the coagulation bath 1 is 2 to 5 min;

[0020] S5, the spun fiber is stretched and then formed in coagulation bath 2 to obtain a formed fiber, wherein the stretching temperature is room temperature, the stretching ratio is 3 to 10 times, the coagulation bath 2 is water, and the residence time in the coagulation bath 2 is 10 to 60 min;

[0021] S6. After winding the shaped fiber obtained in S5, dry it in a blast oven at 60-80° C. for 12-24 hours to obtain a porous fiber monofilament with electromagnetic shielding performance.

[0022] The beneficial effect of the preparation method is that in step S1, the polyethyleneimine on the surface of the modified MXene is a hydrophilic polymer, and the early dispersion helps the modified MXene to move to the polymer-poor phase during the phase inversion process; in step S2, the polymer matrix and Pluronic F127 are both hydrophobic polymers, and the interaction between the two is strong. The early mixing helps to anchor Pluronic F127 on the pore surface of the polymer porous membrane during the phase inversion process, and the interaction between the hydrophilic segment of Pluronic F127 and polyethyleneimine can make the modified MXene distributed on the pore wall of the porous fiber; in step S4, the mixed coagulation bath of ethanol and water helps to achieve the pore structure of the final porous fiber monofilament; in step S5, stretching helps to improve the breaking strength of the porous fiber monofilament, and the water coagulation bath helps to remove the solvent.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention uses wet spinning technology to prepare a porous fiber monofilament by controlling the coagulation bath, and uses amphiphilic Pluronic F127 to distribute the modified MXene on the pore walls of the porous fiber. The pore walls provide multiple interfaces, allowing reflection and absorption of electromagnetic radiation in the material. A small amount of conductive filler is used to achieve higher electromagnetic shielding performance. The porous fiber monofilament with electromagnetic shielding performance of the present invention has an electromagnetic shielding effectiveness of more than 30 dB in the frequency band of 8.2 to 12.4 GHz.

[0025] (2) The present invention controls the pore size of the wet spinning spinneret to achieve a porous fiber monofilament with a diameter of 0.05 to 1 mm and a porosity of 40% to 80%; and controls the stretching process of the spinning process to achieve a porous fiber monofilament with a breaking strength greater than 5.0 cN / dtex.

[0026] (3) The method for preparing the porous fiber monofilament with electromagnetic shielding performance of the present invention is simple to operate, environmentally friendly, has low equipment requirements and cost, and is suitable for practical application and large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0028] Figure 1 This is a scanning electron microscope image of the porous fiber prepared in Example 1 of the present invention.

[0029] Figure 2 This is the electromagnetic shielding performance of the porous fiber prepared in Example 1. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.

[0032] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.

[0033] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.

[0034] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.

[0035] The invention discloses a porous fiber monofilament with electromagnetic shielding performance and a preparation method thereof.

[0036] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.

[0037] Example 1

[0038] Preparation of modified MXene:

[0039] 16 g of lithium fluoride and 240 g of 37% concentrated hydrochloric acid were mixed in a PTFE container and stirred continuously for 15 min to obtain a uniform mixture, then 10 g of titanium aluminum carbide was added and stirred and etched at 40 °C for 48 h; the product was centrifuged at 2000 rpm to remove the supernatant, and deionized water washing and centrifugation were repeated until the pH was neutral; 300 g of deionized water was added again, ultrasonicated at 100 W for 1 h, and further centrifuged at 4000 rpm for 40 min to remove large pieces of unpeeled MAX products, and the supernatant was filtered to obtain MXene; MXene was dispersed in deionized water to prepare a dispersion with a mass concentration of 10 wt%, and polyethyleneimine with a mass of 1 times that of MXene was added, stirred at 400 rpm for 4 h, then centrifuged at 6000 rpm, and finally vacuum dried at room temperature for 30 h to obtain modified MXene.

[0040] Preparation of porous fiber monofilament with electromagnetic shielding performance:

[0041] S1, adding 0.1 g of modified MXene to 3 g of N-methylpyrrolidone A, and stirring the mixture at 500 rpm for 1 h;

[0042] S2, adding 0.86 g of poly(arylene ether nitrile) and 0.04 g of Pluronic F127 to 6 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;

[0043] S3, stirring and mixing the mixture obtained in S1 and the uniform solution obtained in S2 to obtain a spinning solution, then adding the solution to a spinning machine, and extruding the spinning solution from a spinneret with a pore size of 0.6 mm to form a thin stream of 50 m / min;

[0044] S4, introducing the thin stream squeezed out from the spinneret hole in S3 into a coagulation bath 1 containing water and ethanol in a volume ratio of 1:1, and leaving the thin stream in the coagulation bath 1 for 5 minutes to form primary fibers;

[0045] S5, the spun fiber is stretched at a stretching ratio of 5 times in a room temperature, and then placed in a water coagulation bath 2 for 30 minutes to obtain a molded fiber;

[0046] S6. After winding the shaped fiber obtained in S5, dry it in a 60° C. forced air oven for 12 h to obtain a porous fiber monofilament with electromagnetic shielding performance.

[0047] The prepared porous fiber monofilament with electromagnetic shielding performance has a diameter of 0.2 mm, a porosity of 74%, a breaking strength of 5.6 cN / dtex, and an electromagnetic shielding of 32.6 dB at 8.2 GHz.

[0048] Example 2

[0049] Preparation of modified MXene:

[0050] The preparation of modified MXene is consistent with Example 1.

[0051] Preparation of porous fiber monofilament with electromagnetic shielding performance:

[0052] S1, adding 0.1 g of modified MXene to 3 g of N-methylpyrrolidone A, and stirring the mixture at 500 rpm for 1 h;

[0053] S2, adding 0.86 g of polyarylethersulfone and 0.04 g of Pluronic F127 to 6 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;

[0054] S3, stirring and mixing the mixture obtained in S1 and the uniform solution obtained in S2 to obtain a spinning solution, then adding the solution to a spinning machine, and extruding the spinning solution from a spinneret with a pore size of 0.6 mm to form a thin stream of 50 m / min;

[0055] S4, introducing the thin stream squeezed out from the spinneret hole in S3 into a coagulation bath 1 containing water and ethanol in a volume ratio of 1:1, and leaving the thin stream in the coagulation bath 1 for 5 minutes to form primary fibers;

[0056] S5, the spun fiber is stretched at a stretching ratio of 5 times in a room temperature, and then placed in a water coagulation bath 2 for 30 minutes to obtain a molded fiber;

[0057] S6. After winding the shaped fiber obtained in S5, dry it in a 60° C. forced air oven for 12 h to obtain a porous fiber monofilament with electromagnetic shielding performance.

[0058] The prepared porous fiber monofilament with electromagnetic shielding performance has a diameter of 0.2 mm, a porosity of 72%, a breaking strength of 5.8 cN / dtex, and an electromagnetic shielding of 32.4 dB at 8.2 GHz.

[0059] Example 3

[0060] Preparation of modified MXene:

[0061] The preparation of modified MXene is consistent with Example 1.

[0062] Preparation of porous fiber monofilament with electromagnetic shielding performance:

[0063] S1, adding 0.1 g of modified MXene to 3 g of N-methylpyrrolidone A, and stirring the mixture at 500 rpm for 1 h;

[0064] S2, adding 0.86 g of poly(arylether nitrile)-poly(arylether sulfone) binary copolymer and 0.04 g of Pluronic F127 to 6 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;

[0065] S3, stirring and mixing the mixture obtained in S1 and the uniform solution obtained in S2 to obtain a spinning solution, then adding the solution to a spinning machine, and extruding the spinning solution from a spinneret with a pore size of 0.6 mm to form a thin stream of 50 m / min;

[0066] S4, introducing the thin stream squeezed out from the spinneret hole in S3 into a coagulation bath 1 containing water and ethanol in a volume ratio of 1:1, and leaving the thin stream in the coagulation bath 1 for 5 minutes to form primary fibers;

[0067] S5, the spun fiber is stretched at a stretching ratio of 5 times in a room temperature, and then placed in a water coagulation bath 2 for 30 minutes to obtain a molded fiber;

[0068] S6. After winding the shaped fiber obtained in S5, dry it in a 60° C. forced air oven for 12 h to obtain a porous fiber monofilament with electromagnetic shielding performance.

[0069] The prepared porous fiber monofilament with electromagnetic shielding performance has a diameter of 0.2 mm, a porosity of 73%, a breaking strength of 5.7 cN / dtex, and an electromagnetic shielding of 32.5 dB at 8.2 GHz.

[0070] Example 4

[0071] Preparation of modified MXene:

[0072] The preparation of modified MXene is consistent with Example 1.

[0073] Preparation of porous fiber monofilament with electromagnetic shielding performance:

[0074] S1, adding 0.15 g of modified MXene to 3 g of N-methylpyrrolidone A, and stirring the mixture at 500 rpm for 1 h;

[0075] S2, adding 0.81 g of poly(arylene ether nitrile) and 0.04 g of Pluronic F127 to 6 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;

[0076] S3, stirring and mixing the mixture obtained in S1 and the uniform solution obtained in S2 to obtain a spinning solution, then adding the solution to a spinning machine, and extruding the spinning solution from a spinneret with a pore size of 0.6 mm to form a thin stream of 50 m / min;

[0077] S4, introducing the thin stream squeezed out from the spinneret hole in S3 into a coagulation bath 1 containing water and ethanol in a volume ratio of 1:1, and leaving the thin stream in the coagulation bath 1 for 5 minutes to form primary fibers;

[0078] S5, the spun fiber is stretched at a stretching ratio of 5 times in a room temperature, and then placed in a water coagulation bath 2 for 30 minutes to obtain a molded fiber;

[0079] S6. After winding the shaped fiber obtained in S5, dry it in a 60° C. forced air oven for 12 h to obtain a porous fiber monofilament with electromagnetic shielding performance.

[0080] The prepared porous fiber monofilament with electromagnetic shielding performance has a diameter of 0.2 mm, a porosity of 72%, a breaking strength of 5.3 cN / dtex, and an electromagnetic shielding of 35.2 dB at 8.2 GHz.

[0081] Example 5

[0082] Preparation of modified MXene:

[0083] The preparation of modified MXene is consistent with Example 1.

[0084] Preparation of porous fiber monofilament with electromagnetic shielding performance:

[0085] S1, adding 0.2 g of modified MXene to 3 g of N-methylpyrrolidone A, and stirring the mixture at 500 rpm for 1 h;

[0086] S2, adding 0.76 g of poly(arylene ether nitrile) and 0.04 g of Pluronic F127 to 6 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;

[0087] S3, stirring and mixing the mixture obtained in S1 and the uniform solution obtained in S2 to obtain a spinning solution, then adding the solution to a spinning machine, and extruding the spinning solution from a spinneret with a pore size of 0.6 mm to form a thin stream of 50 m / min;

[0088] S4, introducing the thin stream squeezed out from the spinneret hole in S3 into a coagulation bath 1 containing water and ethanol in a volume ratio of 1:1, and leaving the thin stream in the coagulation bath 1 for 5 minutes to form primary fibers;

[0089] S5, the spun fiber is stretched at a stretching ratio of 5 times in a room temperature, and then placed in a water coagulation bath 2 for 30 minutes to obtain a molded fiber;

[0090] S6. After winding the shaped fiber obtained in S5, dry it in a 60° C. forced air oven for 12 h to obtain a porous fiber monofilament with electromagnetic shielding performance.

[0091] The prepared porous fiber monofilament with electromagnetic shielding performance has a diameter of 0.2 mm, a porosity of 70%, a breaking strength of 5.1 cN / dtex, and an electromagnetic shielding of 38.4 dB at 8.2 GHz.

[0092] Example 6

[0093] Preparation of modified MXene:

[0094] The preparation of modified MXene is consistent with Example 1.

[0095] Preparation of porous fiber monofilament with electromagnetic shielding performance:

[0096] S1, adding 0.1 g of modified MXene to 3 g of N-methylpyrrolidone A, and stirring the mixture at 500 rpm for 1 h;

[0097] S2, adding 0.86 g of poly(arylene ether nitrile) and 0.04 g of Pluronic F127 to 6 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;

[0098] S3, stirring and mixing the mixture obtained in S1 and the uniform solution obtained in S2 to obtain a spinning solution, then adding the solution to a spinning machine, and extruding the spinning solution from a spinneret with a pore size of 1.2 mm to form a thin stream of 50 m / min;

[0099] S4, introducing the thin stream squeezed out from the spinneret hole in S3 into a coagulation bath 1 containing water and ethanol in a volume ratio of 1:1, and leaving the thin stream in the coagulation bath 1 for 5 minutes to form primary fibers;

[0100] S5, the spun fiber is stretched at a stretching ratio of 5 times in a room temperature, and then placed in a water coagulation bath 2 for 30 minutes to obtain a molded fiber;

[0101] S6. After winding the shaped fiber obtained in S5, dry it in a 60° C. forced air oven for 12 h to obtain a porous fiber monofilament with electromagnetic shielding performance.

[0102] The prepared porous fiber monofilament with electromagnetic shielding performance has a diameter of 0.4 mm, a porosity of 70%, a breaking strength of 5.8 cN / dtex, and an electromagnetic shielding of 32.2 dB at 8.2 GHz.

[0103] Example 7

[0104] Preparation of modified MXene:

[0105] The preparation of modified MXene is consistent with Example 1.

[0106] Preparation of porous fiber monofilament with electromagnetic shielding performance:

[0107] S1, adding 0.1 g of modified MXene to 3 g of N-methylpyrrolidone A, and stirring the mixture at 500 rpm for 1 h;

[0108] S2, adding 0.86 g of poly(arylene ether nitrile) and 0.04 g of Pluronic F127 to 6 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;

[0109] S3, stirring and mixing the mixture obtained in S1 and the uniform solution obtained in S2 to obtain a spinning solution, then adding the solution to a spinning machine, and extruding the spinning solution from a spinneret with a pore size of 0.6 mm to form a thin stream of 50 m / min;

[0110] S4, introducing the thin stream squeezed out from the spinneret hole in S3 into a coagulation bath 1 containing water and ethanol in a volume ratio of 1:4, and leaving the thin stream in the coagulation bath 1 for 5 minutes to form primary fibers;

[0111] S5, the spun fiber is stretched at a stretching ratio of 5 times in a room temperature, and then placed in a water coagulation bath 2 for 30 minutes to obtain a molded fiber;

[0112] S6. After winding the shaped fiber obtained in S5, dry it in a 60° C. forced air oven for 12 h to obtain a porous fiber monofilament with electromagnetic shielding performance.

[0113] The prepared porous fiber monofilament with electromagnetic shielding performance has a diameter of 0.2 mm, a porosity of 80%, a breaking strength of 6.1 cN / dtex, and an electromagnetic shielding of 36.2 dB at 8.2 GHz.

[0114] Example 8

[0115] Preparation of modified MXene:

[0116] The preparation of modified MXene is consistent with Example 1.

[0117] Preparation of porous fiber monofilament with electromagnetic shielding performance:

[0118] S1, adding 0.1 g of modified MXene to 3 g of N-methylpyrrolidone A, and stirring the mixture at 500 rpm for 1 h;

[0119] S2, adding 0.86 g of poly(arylene ether nitrile) and 0.04 g of Pluronic F127 to 6 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;

[0120] S3, stirring and mixing the mixture obtained in S1 and the uniform solution obtained in S2 to obtain a spinning solution, then adding the solution to a spinning machine, and extruding the spinning solution from a spinneret with a pore size of 0.6 mm to form a thin stream of 50 m / min;

[0121] S4, introducing the thin stream squeezed out from the spinneret hole in S3 into a coagulation bath 1 containing water and ethanol in a volume ratio of 1:1, and leaving the thin stream in the coagulation bath 1 for 5 minutes to form primary fibers;

[0122] S5, the spun fiber is stretched at a stretching ratio of 10 times in a room temperature, and then placed in a water coagulation bath 2 for 30 minutes to obtain a molded fiber;

[0123] S6. After winding the shaped fiber obtained in S5, dry it in a 60° C. forced air oven for 12 h to obtain a porous fiber monofilament with electromagnetic shielding performance.

[0124] The prepared porous fiber monofilament with electromagnetic shielding performance has a diameter of 0.1 mm, a porosity of 73%, a breaking strength of 5.9 cN / dtex, and an electromagnetic shielding of 33.4 dB at 8.2 GHz.

[0125] Comparative Example 1

[0126] Preparation of modified MXene:

[0127] 16 g of lithium fluoride and 240 g of 37% concentrated hydrochloric acid were mixed in a PTFE container and stirred continuously for 15 min to obtain a uniform mixture. Then 10 g of titanium aluminum carbide was added and stirred and etched at 40 °C for 48 h. The product was centrifuged at 2000 rpm to remove the supernatant, and deionized water washing and centrifugation were repeated until the pH was neutral. 300 g of deionized water was added again, and ultrasonic treatment was performed at 100 W for 1 h. The product was further centrifuged at 4000 rpm for 40 min to remove large pieces of unpeeled MAX products. The supernatant was then filtered to obtain MXene, which was defined as modified MXene.

[0128] Preparation of porous fiber monofilament with electromagnetic shielding performance:

[0129] S1, adding 0.1 g of modified MXene to 3 g of N-methylpyrrolidone A, and stirring the mixture at 500 rpm for 1 h;

[0130] S2, adding 0.86 g of poly(arylene ether nitrile) and 0.04 g of Pluronic F127 to 6 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;

[0131] S3, stirring and mixing the mixture obtained in S1 and the uniform solution obtained in S2 to obtain a spinning solution, then adding the solution to a spinning machine, and extruding the spinning solution from a spinneret with a pore size of 0.6 mm to form a thin stream of 50 m / min;

[0132] S4, introducing the thin stream squeezed out from the spinneret hole in S3 into a coagulation bath 1 containing water and ethanol in a volume ratio of 1:1, and leaving the thin stream in the coagulation bath 1 for 5 minutes to form primary fibers;

[0133] S5, the spun fiber is stretched at a stretching ratio of 5 times in a room temperature, and then placed in a water coagulation bath 2 for 30 minutes to obtain a molded fiber;

[0134] S6. After winding the shaped fiber obtained in S5, dry it in a 60° C. forced air oven for 12 h to obtain a porous fiber monofilament with electromagnetic shielding performance.

[0135] The prepared porous fiber monofilament with electromagnetic shielding performance has a diameter of 0.2 mm, a porosity of 73%, a breaking strength of 5.6 cN / dtex, and an electromagnetic shielding of 25.4 dB at 8.2 GHz.

[0136] Comparative Example 2

[0137] Preparation of modified MXene:

[0138] The preparation of modified MXene is consistent with Example 1.

[0139] Preparation of porous fiber monofilament with electromagnetic shielding performance:

[0140] S1, adding 0.1 g of modified MXene to 3 g of N-methylpyrrolidone A, and stirring the mixture at 500 rpm for 1 h;

[0141] S2, adding 0.9 g of poly(arylene ether nitrile) to 6 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;

[0142] S3, stirring and mixing the mixture obtained in S1 and the uniform solution obtained in S2 to obtain a spinning solution, then adding the solution to a spinning machine, and extruding the spinning solution from a spinneret with a pore size of 0.6 mm to form a thin stream of 50 m / min;

[0143] S4, introducing the thin stream squeezed out from the spinneret hole in S3 into a coagulation bath 1 containing water and ethanol in a volume ratio of 1:1, and leaving the thin stream in the coagulation bath 1 for 5 minutes to form primary fibers;

[0144] S5, the spun fiber is stretched at a stretching ratio of 5 times in a room temperature, and then placed in a water coagulation bath 2 for 30 minutes to obtain a molded fiber;

[0145] S6. After winding the shaped fiber obtained in S5, dry it in a 60° C. forced air oven for 12 h to obtain a porous fiber monofilament with electromagnetic shielding performance.

[0146] The prepared porous fiber monofilament with electromagnetic shielding performance has a diameter of 0.2 mm, a porosity of 73%, a breaking strength of 5.6 cN / dtex, and an electromagnetic shielding of 24.8 dB at 8.2 GHz.

[0147] Comparative Example 3

[0148] Preparation of modified MXene:

[0149] The preparation of modified MXene is consistent with Example 1.

[0150] Preparation of porous fiber monofilament with electromagnetic shielding performance:

[0151] S1, adding 0.1 g of modified MXene to 3 g of N-methylpyrrolidone A, and stirring the mixture at 500 rpm for 1 h;

[0152] S2, adding 0.9 g of poly(arylene ether nitrile) to 6 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;

[0153] S3, stirring and mixing the mixture obtained in S1 and the uniform solution obtained in S2 to obtain a spinning solution, then adding the solution to a spinning machine, and extruding the spinning solution from a spinneret with a pore size of 0.6 mm to form a thin stream of 50 m / min;

[0154] S4, introducing the thin stream squeezed out from the spinneret hole in S3 into a coagulation bath 1 containing water and ethanol in a volume ratio of 1:1, and leaving the thin stream in the coagulation bath 1 for 5 minutes to form primary fibers;

[0155] S5, the nascent fiber is placed in the water coagulation bath 2 for 30 min to be formed, thereby obtaining a formed fiber;

[0156] S6. After winding the shaped fiber obtained in S5, dry it in a 60° C. forced air oven for 12 h to obtain a porous fiber monofilament with electromagnetic shielding performance.

[0157] The prepared porous fiber monofilament with electromagnetic shielding performance has a diameter of 0.3 mm, a porosity of 76%, a breaking strength of 3.5 cN / dtex, and an electromagnetic shielding of 32.2 dB at 8.2 GHz.

[0158] Performance Testing:

[0159] The porous fiber monofilaments with electromagnetic shielding performance obtained in Examples 1-8 and Comparative Examples 1-3 were subjected to the following performance tests:

[0160] Diameter of porous fiber monofilament: The porous fiber monofilament was observed by scanning electron microscope, and then the diameter of the porous fiber monofilament was measured according to the test results, wherein the porous fiber monofilament was treated with gold spraying before the electron microscope test.

[0161] Porosity: The apparent density, particle density and skeleton density of the porous fiber monofilament were tested by the vibration method, mercury displacement method and helium displacement method respectively, and then the porosity was calculated.

[0162] Breaking strength: The breaking strength was tested using an XL-1A filament tensile tester. Each sample was tested more than 10 times and the test results were averaged.

[0163] Electromagnetic shielding: The porous fiber monofilaments of the embodiment and the comparative example were woven into fabrics using a textile machine, and the electromagnetic shielding effectiveness of the fabrics was tested using a vector network tester at a test frequency of 8.2 to 12.4 GHz.

[0164] The results are shown in Table 1.

[0165] Table 1: Performance test results of porous fiber monofilaments with electromagnetic shielding performance prepared in Examples and Comparative Examples.

[0166] Experiment number Diameter(mm) Porosity(%) Breaking strength (cN / dtex) Electromagnetic shielding at 8.2 GHz (dB) Example 1 0.2 74 5.6 32.6 Example 2 0.2 72 5.8 32.4 Example 3 0.2 73 5.7 32.5 Example 4 0.2 72 5.3 35.2 Example 5 0.2 70 5.1 38.4 Example 6 0.4 70 5.8 32.2 Example 7 0.2 80 6.1 36.2 Example 8 0.1 73 5.9 33.4 Comparative Example 1 0.2 74 5.6 25.4 Comparative Example 2 0.2 74 5.6 24.8 Comparative Example 3 0.3 76 4.5 32.2

[0167] It can be obtained from the above table that the porous fiber monofilaments with electromagnetic shielding performance prepared in Examples 1-8 have a diameter of 0.05-1 mm, a porosity of 40%-80%, a breaking strength greater than 5.0 cN / dtex, and an electromagnetic shielding effectiveness of more than 30 dB at 8.2 GHz. In Comparative Example 1, MXene was prepared without hydrophilic modification of polyethyleneimine. Compared with Example 1, the prepared porous fiber monofilaments with electromagnetic shielding performance have an electromagnetic shielding effectiveness of only 25.4 dB at 8.2 GHz, indicating that hydrophilic modification of MXene helps MXene to be oriented in the pore walls of porous fibers, thereby improving electromagnetic shielding effectiveness. In Comparative Example 2, Pluronic F127 was used, which also failed to effectively orient MXene in the pore walls of porous fibers. Therefore, its electromagnetic shielding effectiveness at 8.2 GHz was only 24.8 dB, indicating that the addition of Pluronic F127 is very necessary. Comparative Example 3 is a comparative test in which the primary fibers are not stretched after being formed. Since no stretching treatment is performed, the breaking strength of the prepared porous fibers is only 4.5 cN / dtex, which is lower than 5.0 cN / dtex. This indicates that stretching treatment after the primary fibers are formed is beneficial to improving the breaking strength of the porous fibers, that is, stretching treatment is necessary for the preparation of high-performance porous fibers.

[0168] The above test shows that the present invention uses wet spinning technology to prepare a porous fiber monofilament by controlling the coagulation bath, and uses amphiphilic Pluronic F127 to make the modified MXene distributed on the pore wall of the porous fiber. The pore wall provides multiple interfaces, allowing the reflection and absorption of electromagnetic radiation in the material, and using a small amount of conductive filler to achieve higher electromagnetic shielding performance; at the same time, by controlling the stretching process of the spinning process, the fracture strength of the porous fiber monofilament is controlled. The porous fiber monofilament with electromagnetic shielding performance of the present invention has a diameter of 0.05 to 1 mm, a porosity of 40% to 80%, a fracture strength greater than 5.0 cN / dtex, and an electromagnetic shielding effectiveness of more than 30 dB in the frequency range of 8.2 to 12.4 GHz. The preparation method of the porous fiber monofilament with electromagnetic shielding performance of the present invention is simple to operate, environmentally friendly, has low equipment requirements and cost, and is suitable for practical application and large-scale production.

[0169] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A porous fiber monofilament with electromagnetic shielding performance, characterized in that: The porous fiber monofilament with electromagnetic shielding performance has a diameter of 0.05 to 1 mm and a porosity of 40% to 80%; The porous fiber monofilament with electromagnetic shielding performance is composed of 60-95 wt% of polymer, 5-40 wt% of modified MXene and 2-10 wt% of Pluronic F127, wherein the modified MXene is distributed on the pore wall of the porous polymer fiber monofilament through Pluronic F127 as a connector; The breaking strength of the porous fiber monofilament with electromagnetic shielding performance is greater than 5.0 cN / dtex, and the electromagnetic shielding effectiveness in the frequency range of 8.2 to 12.4 GHz is greater than 30 dB.

2. The porous fiber monofilament with electromagnetic shielding performance according to claim 1, characterized in that: The polymer is one of polyarylether nitrile, polyarylether ketone, polyarylether sulfone, polyimide, polyetherimide, polyarylether nitrile-polyarylether ketone binary copolymer, polyarylether nitrile-polyarylether sulfone binary copolymer, polyarylether ketone-polyarylether sulfone binary copolymer, polyimide-polyetherimide binary copolymer, polyarylether nitrile-polyarylether ketone-polyarylether sulfone terpolymer.

3. The porous fiber monofilament with electromagnetic shielding performance according to claim 1, characterized in that: The steps of the preparation method of the modified MXene are as follows: Mix 1 part of lithium fluoride and 10-100 parts of 37% concentrated hydrochloric acid in a PTFE container and stir to obtain a uniform mixture, then add 0.5-1 part of titanium aluminum carbide, and etch at 30-60 ° C for 24-48 hours; the product is centrifuged at 1000-3000 rpm to remove the supernatant, and deionized water washing and centrifugation are repeated until the pH is neutral; 5-20 parts of deionized water are added again, ultrasonicated at 50-500 W for 1-2 hours, and further centrifuged at 1000-5000 rpm for 30-60 minutes to remove large pieces of unpeeled MAX products, and the supernatant is filtered to obtain MXene; MXene is dispersed in deionized water to prepare a dispersion with a mass concentration of 5-30 wt%, and 0.5-5 times the mass of MXene polyethyleneimine is added, and stirred at a speed of 100-500 rpm for 3-8 h, then centrifuged at 3000-10000 rpm, and finally dried in vacuum at room temperature for 24-48 h to obtain the modified MXene.

4. A method for preparing a porous fiber monofilament with electromagnetic shielding performance as claimed in claim 1, characterized in that: The preparation method comprises the following steps: S1. Mixing the modified MXene and N-methylpyrrolidone A in a mass ratio of 1:20 to 100, and stirring to obtain a mixture; S2, adding the polymer and Pluronic F127 into N-methylpyrrolidone B, stirring to obtain a uniform solution; S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2 to obtain a spinning solution, then adding the solution to a spinning machine, and squeezing the spinning solution out of a spinneret hole to form a thin stream; S4, introducing the thin stream squeezed out from the spinneret hole in S3 into the coagulation bath 1 to form primary fibers; S5, the spun fiber is stretched and then formed in coagulation bath 2 to obtain a formed fiber; S6. After winding the formed fiber obtained in S5, dry it in a forced air oven at 60-80° C. for 12-24 h to obtain a porous fiber monofilament with electromagnetic shielding performance.

5. The method for preparing a porous fiber monofilament with electromagnetic shielding performance according to claim 4, characterized in that: In step S2, the mass ratio of the polymer to the modified MXene is 4:1-15:1, the mass ratio of Pluronic F127 to the modified MXene is 0.1:1-2:1, and the mass of N-methylpyrrolidone B is 1-3 times that of N-methylpyrrolidone A.

6. The method for preparing a porous fiber monofilament with electromagnetic shielding performance according to claim 4, characterized in that: In step S3, the diameter of the spinneret hole is 0.1-2 mm, and the speed at which the spinning solution is pressed out of the spinneret hole to form a thin stream is 30-50 m / min.

7. The method for preparing a porous fiber monofilament with electromagnetic shielding performance according to claim 4, characterized in that: In step S4, the coagulation bath 1 is a mixed coagulation bath of water and ethanol in a volume ratio of 1:1 to 4, and the residence time in the coagulation bath 1 is 2 to 5 minutes.

8. The method for preparing a porous fiber monofilament with electromagnetic shielding performance according to claim 4, characterized in that: In step S5, the stretching temperature is room temperature, the stretching ratio is 3 to 10 times, the coagulation bath 2 is water, and the residence time in the coagulation bath 2 is 10 to 60 min.