Iron block standard substance for calibration of X-ray residual stress tester as well as preparation method and application of iron block standard substance

CN118999867APending Publication Date: 2024-11-22NATIONAL INSTITUTE OF METROLOGY CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411117555.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing X-ray residual stress sample preparation technology has problems such as poor density and uniformity of iron powder, large residual stress, poor uniformity and unscientific fixed value methods, resulting in inaccurate and unreliable measurement results.

Method used

Pure iron powder with particle size (1~8)μm is mixed with high transparency and high fluidity crystal glue, and standard iron block substances are obtained through natural settlement and curing and cutting treatment to ensure surface flatness and density, and high precision is adopted. The inclinometer is calibrated and traced, calculates residual stresses and provides standard values ​​and uncertainties.

Benefits of technology

The dense, uniform distribution and small residual stress of iron block standard substances are achieved, ensuring the accurate calibration and reliable value of the X-ray residual stress detector, and meeting the uniformity and traceability requirements of the standard substances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118999867A_ABST
    Figure CN118999867A_ABST
Patent Text Reader

Abstract

The invention discloses an iron block standard substance for calibration of an X-ray residual stress tester and a preparation method and application of the iron block standard substance, and belongs to the field of standard substances, the iron block standard substance comprises an iron block obtained by settling and curing iron powder in polyester resin and cutting the iron powder, and the iron powder adopts pure iron powder with the particle size of (1-8) mu m and the iron element content of more than or equal to 95%. Pure iron powder with a specific particle size of 1-8 [mu] m is selected to be mixed with polyester resin, and after curing molding, uneven parts at the upper part are cut off, so that iron powder particles in the obtained iron block body standard substance are compact and uniformly distributed, the iron block body standard substance is good in surface flatness and small in roughness, the residual stress of the standard substance is tiny and uniform, and the iron block body standard substance is suitable for industrial production. And the uniformity requirement of the standard substance is completely met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of standard substances, and in particular to an iron block standard substance for calibrating an X-ray residual stress measuring instrument, and a preparation method, a value determination method, a traceability method and an application thereof. Background Art

[0002] There are many methods for measuring residual stress in metal alloys or other crystalline materials, such as X-ray method, blind hole method, ultrasonic method, neutron diffraction method, etc. Among them, the X-ray stress measurement method is the most typical. The theoretical basis of this method is relatively rigorous, the experimental technology and hardware facilities are very complete, the measurement results are very reliable, and it is a non-destructive, online measurement method. Therefore, it has been widely used in aerospace, automobile, shipbuilding, machinery and other industrial fields. However, before measuring X-ray residual stress, it is necessary to use standard materials or standard samples with standard residual stress values ​​to calibrate the X-ray residual stress measuring instrument to check whether the measurement accuracy of the instrument system meets the requirements. Therefore, the selection and use of residual stress standard materials or standard samples to calibrate the instrument is crucial to the actual measurement work.

[0003] At present, there are two main sources of stress samples used for calibration of X-ray residual stress testers in the Chinese market: one is the residual stress samples prepared by X-ray residual stress tester manufacturers; the other is the residual stress samples prepared by users and third-party testing agencies, such as Figure 1 shown.

[0004] At present, my country does not have national certified standard materials and national certified standard samples for residual stress. my country currently has more than 2,000 X-ray residual stress testers, most of which are produced and sold by Proto of Canada and Stresstech of Finland. The residual stress samples prepared by these companies are sold with the instruments. The residual stress samples prepared by the equipment manufacturers do not disclose the preparation process and technical route of the residual stress samples, provide the residual stress reference value and error range of the sample, do not provide the reference value determination method and traceability path, and do not provide the uncertainty of the value.

[0005] Some X-ray residual stress measuring instrument users and third-party testing institutions in my country have prepared several residual stress specimens. The technical route for preparing residual stress specimens in China is: annealing and heat treating iron powder with a particle size of (1-45) μm in a vacuum furnace to reduce the residual stress in the iron powder as much as possible; diluting the nitrogen cellulose adhesive with acetone to a 10% solution as an adhesive solution; sprinkling the annealed iron powder on a microscope slide, and then evenly dripping the adhesive solution on the iron powder; sprinkling the annealed iron powder on the adhesive solution, and pressing it with another microscope slide; after the upper surface is flattened, taking off the upper display Continue to repeatedly sprinkle iron powder, drip adhesive solution and press the slide until the thickness of the sample reaches 15mm, then use a microscope slide to press the upper surface flat, and then dry the sample to obtain an X-ray residual stress sample. If the surface is uneven due to excessive adhesive, you can use acetone to wet the surface again, make it flat and then dry it; finally, place the dried residual stress sample under the probe of the X-ray residual stress measuring instrument, and repeat the measurement of the residual stress of the sample 5 times. If the average value of the 5 residual stresses is within the range of ±14MPa, it is determined that the residual stress value of the sample is close to zero.

[0006] The current problems with the domestic residual stress specimen technology route include: heavy reliance on manual operations when sprinkling metal powder and dripping adhesive solution, a great influence of human factors, difficulty in obtaining a surface with good flatness and low roughness by manually pressing the specimen surface with a microscope slide, unscientific value determination methods, lack of a traceability chain, inaccurate and unreliable measurement results, and no assessment of uncertainty, which have hindered the successful preparation and widespread application of residual stress specimens.

[0007] At present, my country's third-party testing companies and research institutions mainly prepare low residual stress specimens through the powder mixing and curing method. After multiple measurements by a single device, the residual stress value of the specimen is determined to be close to zero, but no specific value is given. It is then used to test and evaluate the X-ray residual stress measuring instrument. The existing residual stress specimen preparation and determination methods have the following problems: (1) The residual stress value of the specimen after curing is generally large, and the residual stress uniformity in the specimen is poor. The error of the residual stress value is large, and the error range can reach (11-29) MPa; (2) When manually sprinkling iron powder and manually dripping adhesive solution on the glass sheet, it is heavily dependent on manual operation. The human factor has a great influence, resulting in some areas with dense iron powder and some areas with sparse iron powder. Some iron powder is completely covered and infiltrated by the adhesive solution, and some iron powder has no contact with the adhesive solution at all, resulting in poor uniformity of iron powder particle distribution in the final cured specimen, which in turn causes The residual stress uniformity of the finished sample is very poor; (3) It is difficult to obtain a surface with good flatness and low roughness by manually pressing the sample surface with a microscope slide. The final surface of the cured sample has poor flatness and large roughness, and the X-ray residual stress meter is very sensitive to them. Poor flatness and large roughness will seriously reduce the accuracy and reliability of the measurement results; (4) The X-ray residual stress meter is used to repeatedly measure the cured sample 5 times. If the average value of the 5 residual stresses is within the range of ±14MPa, the residual stress value of the sample is considered to be close to zero. This determination method does not calibrate and trace the instrument, and does not comply with the requirements of JJF 1343-2022 "Determination of the Value and Uniformity and Stability Evaluation of Standard Materials". The specific value of the residual stress of the sample and its uncertainty are not given. Therefore, the determination method is unscientific and incorrect, which hinders the development and widespread application of residual stress samples.

[0008] There is an urgent need to develop a residual stress specimen in order to solve the problems of poor density and uniformity of iron powder in existing residual stress specimens, large residual stress of the specimens, poor isotropy and uniformity, and unscientific and incorrect determination methods. Summary of the invention

[0009] Purpose of the Invention

[0010] In order to overcome the above-mentioned shortcomings, the purpose of the present invention is to provide an iron block residual stress standard material with dense and uniform distribution of iron powder particles, good surface flatness and small roughness, and small and uniform residual stress for use in calibrating X-ray residual stress measuring instruments, as well as its preparation method, determination method, traceability method and application.

[0011] Solution

[0012] To achieve the purpose of the present invention, the technical solution adopted by the present invention is as follows:

[0013] In the first aspect, the present invention provides an iron block standard material for calibrating an X-ray residual stress measuring instrument, which includes an iron block obtained by sedimentation and solidification of iron powder in crystal glue and then cutting, wherein the iron powder is pure iron powder with a particle size of (1 to 8) μm and an iron content of ≥95%.

[0014] Furthermore, the iron block standard material (also referred to as the iron block residual stress standard material) is an iron block obtained by cutting off the upper uneven part of an iron powder solidified iron block which is formed by mixing crystal glue and iron powder and then standing and settling to solidify; optionally, the cut-off upper uneven part is 1 / 3 to 2 / 3 of the height of the iron powder solidified iron block, optionally 1 / 3 to 1 / 2.

[0015] Furthermore, the iron block standard material has no bubbles and no depressions.

[0016] Furthermore, the back side of the iron block standard material is a polished surface.

[0017] Furthermore, the thickness difference between the front and back of the iron block standard material at different positions is less than 0.01 mm.

[0018] Furthermore, the size of the iron block standard material is (10-30) mm×(5-15) mm×(5-12) mm, and optionally the size is 20 mm×10 mm×8 mm.

[0019] Furthermore, the residual stress value of the iron block standard material is (3-7) MPa.

[0020] Furthermore, the standard deviation of the residual stress value of the iron block standard material is (0-3) MPa.

[0021] Furthermore, the error range of the residual stress value of the iron block standard material is ±3MPa.

[0022] Furthermore, the crystal glue is highly transparent, highly fluid, and bubble-free after curing. Optionally, crystal glue containing components A and B may be used; optionally, the crystal glue is purchased from Wenzhou Anergu New Materials Co., Ltd.

[0023] In the second aspect, a method for preparing an iron block standard material for calibrating an X-ray residual stress measuring instrument is provided, comprising the following steps: evenly mixing iron powder and crystal glue, pouring the mixture into a mold, allowing the mixture to stand, settle naturally, and solidify to form an iron powder solidified block, cutting off the uneven portion of the upper iron powder, and polishing the back to obtain an iron block residual stress standard material.

[0024] Furthermore, the weight ratio of the iron powder to the crystal glue is 1:(1-5), optionally 1:(2-3).

[0025] Furthermore, the mixing method is stirring.

[0026] Furthermore, the upper uneven portion that is cut off is 1 / 3 to 2 / 3 of the height of the iron powder solidified block, and optionally 1 / 3 to 1 / 2.

[0027] Furthermore, the iron powder is pure iron powder with a particle size of (1-8) μm and an iron content of ≥95%.

[0028] Furthermore, the crystal glue is highly transparent, highly fluid, and bubble-free after curing. Optionally, crystal glue containing components A and B may be used; optionally, the crystal glue is purchased from Wenzhou Anergu New Materials Co., Ltd.

[0029] Furthermore, after cutting and grinding, the thickness difference between the front and back sides of the iron block residual stress standard material at different positions is less than 0.01 mm.

[0030] Furthermore, the residual stress value of the iron block residual stress standard material is (3-7) MPa.

[0031] Furthermore, the standard deviation of the residual stress value of the iron block residual stress standard material is (0-3) MPa.

[0032] And / or, the error range of the residual stress value of the iron block residual stress standard material is ±3 MPa.

[0033] In a third aspect, a method for determining the value of the iron block standard material according to the first aspect or the iron block standard material prepared by the preparation method according to the second aspect is provided, comprising:

[0034] 1) Calibrate the X-ray residual stress measuring instrument;

[0035] 2) The residual stress of the candidate iron block standard material is measured by a calibrated X-ray residual stress measuring instrument. The residual stress is calculated based on the data detected after calibration to obtain the standard value and uncertainty. The X-ray residual stress calculation formula is as follows:

[0036]

[0037]

[0038]

[0039] σ φ =K1M (4)

[0040] Where, E is the theoretical value of the elastic modulus of the material in a stress-free state, ν is the theoretical value of the Poisson's ratio of the material in a stress-free state, θ0 is the theoretical value of the Bragg diffraction angle of the material in a stress-free state, and θ is the Bragg diffraction angle of the material in a stress state; K is called the stress constant, which is a constant related only to the nature of the material and the selected diffraction surface hkl. When the measured samples are of the same material and the selected diffraction surface index is the same, K is a constant. M is the square root of 2θ with respect to sin 2 The slope of ψ is obtained by measuring the corresponding 2θ at at least 7 ψ angles using X-ray residual stress measurement. The slope is then calculated using the least squares fitting method. The residual stress σ can be calculated based on K and M. φ Since K<0, when M<0 it is tensile stress, when M>0 it is compressive stress, and when M=0 there is no stress.

[0041] Among them, the standard value is the average value, and the uncertainty is calculated according to the main principles.

[0042] Furthermore, the calibration includes: calibrating the residual stress measured by the high-precision digital inclinometer; and calibrating at least 7 ψ tilt angles of the X-ray residual stress measuring instrument by the calibrated high-precision digital inclinometer.

[0043] In a fourth aspect, a traceability method for the iron block standard material described in the first aspect or the iron block standard material prepared by the preparation method described in the second aspect is provided, comprising: tracing the residual stress of the iron block standard material to at least 7 ψ inclination angles through an X-ray residual stress measuring instrument, and then tracing at least 7 ψ inclination angles to the angle of the inclinometer through a calibrated inclinometer, and finally the angle of the inclinometer is traced back to the national angle reference device.

[0044] The seven ψ inclination angles of the X-ray residual stress measuring instrument are calibrated with the calibrated inclinometer, and then the residual stress of the iron block residual stress standard material is measured using the calibrated instrument. The residual stress is calculated based on the calibrated data to obtain the standard value of the standard material.

[0045] In the fifth aspect, there is provided an application of the iron block standard material described in the first aspect, or the iron block standard material prepared by the preparation method described in the second aspect, or the determination method described in the third aspect, or the traceability method described in the fourth aspect in inspecting and evaluating an X-ray residual stress measuring instrument.

[0046] Beneficial Effects

[0047] (1) The present invention selects pure iron powder with a specific particle size (1 to 8) μm and mixes it with crystal glue. After solidification and molding, the upper uneven part is cut off to obtain an iron block standard material in which the iron powder particles are dense and evenly distributed. The surface flatness of the iron block standard material is good and the roughness is small. The residual stress of the standard material is small and uniform, which fully meets the uniformity requirements of the standard material.

[0048] (2) The residual stress traceability and determination method of the iron block residual stress standard material of the present invention uses a calibrated high-precision inclinometer to calibrate the 7 ψ inclination angles of the X-ray residual stress measuring instrument, and then uses the calibrated X-ray residual stress measuring instrument to determine the value of the iron block residual stress standard material. The residual stress traceability and determination method is scientific and correct, and the determination result is accurate and reliable, which successfully solves the traceability and accuracy problems of residual stress sample determination. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] One or more embodiments are exemplarily described by the pictures in the accompanying drawings, and these exemplary descriptions do not constitute limitations on the embodiments. The special word "exemplary" here means "used as an example, embodiment or illustrative". Any embodiment described as "exemplary" here is not necessarily interpreted as being superior or better than other embodiments.

[0050] Figure 1 These are the existing X-ray residual stress standard samples at home and abroad: (a) from Proto Company in Canada; (b) from Proto Company in Canada, with a residual stress value of -457MPa; (c) from Stresstech Oy in Finland, with a residual stress value error range of ±35MPa; (d) from Shanghai Jiao Tong University, with a residual stress value error range of ±20MPa.

[0051] Figure 2 The X-ray residual stress diffraction spectra of pure iron powder with different particle sizes according to Example 1 and Comparative Example 1 of the present invention are as follows: (a) (1-8) μm particle size, the diffraction peak is narrow and sharp, the stress is small and the error is small; (b) (1-45) μm particle size, the diffraction peak is wide and blunt, the stress is large and the error is large.

[0052] Figure 3 This is an example of the structure diagram of an embodiment of the iron block standard material of the present invention before and after cutting (the dots do not represent the actual situation, but are only used to show the state of natural sedimentation of iron powder. For the actual object, see Figure 5 ), where A is the naturally settled iron block, and B is the iron powder that is evenly and densely cut and can be used as the iron block standard material.

[0053] Figure 4Scanning electron microscope test results of the pure iron powder used in the present invention: (a) and (b) are respectively the microscopic morphologies of two samples in the same package of iron powder; (c) and (d) are respectively the element types and contents measured by X-ray energy spectrometer of two samples in the same package of iron powder.

[0054] Figure 5 The process of preparing the iron block residual stress standard material of the present invention is as follows: (a) pure iron powder; (b) crystal glue; (c) plastic beaker and electronic balance; (d) soft glue mold; (e) solidified iron block; (f) wire cutting machine; (g) grinding and polishing machine; (h) prepared iron block standard material.

[0055] Figure 6 The iron block residual stress standard material prepared by the present invention: (a) the actual object, 20 mm long, 10 mm wide, and 8 mm high; (b) packaged with a dust-free cloth and a plastic box, the interior of the plastic box is 28 mm long, 21 mm wide, and 16 mm high.

[0056] Figure 7 The method for determining the value of the iron block residual stress standard material prepared by the present invention is as follows: (a) high-precision digital inclinometer; (b) X-ray residual stress measuring instrument; (c) the inclinometer calibrates the angle of the X-ray residual stress measuring instrument. That is, firstly, the high-precision digital inclinometer is calibrated with the national angle reference device, and then the calibrated inclinometer is used to calibrate the 7 ψ inclination angles of the X-ray residual stress measuring instrument, and then the calibrated X-ray residual stress measuring instrument is used to measure the residual stress of the iron block standard material to obtain the standard value and uncertainty. The determination method and process are scientific and rigorous, and fully comply with the requirements and regulations of the technical specification JJF 1343-2022 "Determination of Standard Materials and Uniformity and Stability Evaluation".

[0057] Figure 8 The traceability path of the residual stress standard material of the iron block prepared by the present invention. Traceability method: The residual stress of the iron block standard material is traced to 7 ψ tilt angles through an X-ray residual stress measuring instrument, and then the 7 ψ tilt angles are traced to the angle of the inclinometer through an inclinometer, and finally the angle of the inclinometer is traced to the national angle reference device, and the national angle reference device is directly related to the SI basic unit (meter). Therefore, the entire traceability chain is scientific and correct, and the residual stress is finally traced to the SI basic unit (meter).

[0058] Fig. 9 An example of the relationship between 2θ and sin2ψ under plane stress state when determining the value of the iron block residual stress standard material prepared by the present invention.

[0059] Fig.10 The schematic diagram of the position of measuring the value of the iron block residual stress standard material of the present invention. A is a three-dimensional schematic diagram, and B shows the schematic diagram of the position (circle) of measuring the value. DETAILED DESCRIPTION

[0060] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0061] In addition, in order to better illustrate the present invention, numerous specific details are provided in the specific embodiments below. It should be understood by those skilled in the art that the present invention can also be implemented without certain specific details. In some embodiments, raw materials, elements, methods, means, etc. well known to those skilled in the art are not described in detail, so as to highlight the main purpose of the present invention.

[0062] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.

[0063] In a first aspect, the present invention provides an embodiment of an iron block standard material (also referred to as an iron block residual stress standard material) for calibrating an X-ray residual stress measuring instrument, such as Figure 3 As shown, it includes an iron block 1 obtained by settling and solidifying iron powder 10 in crystal glue and then cutting it. The iron powder 10 is pure iron powder with a particle size of (1-8) μm and an iron content of ≥95% (the iron powder identification result is shown in Figure 4 shown).

[0064] Furthermore, the iron block standard material is an iron block obtained by cutting off the upper uneven portion of an iron powder solidified iron block formed by mixing crystal glue and iron powder and then standing and settling to solidify; optionally, the cut-off upper uneven portion is 1 / 3 to 2 / 3 of the height of the iron powder solidified iron block, optionally 1 / 3 to 1 / 2.

[0065] Furthermore, the iron block standard material has no bubbles and no depressions.

[0066] Furthermore, the back side of the iron block standard material is a polished surface.

[0067] Furthermore, the thickness difference between the front and back of the iron block standard material at different positions is less than 0.01 mm.

[0068] Furthermore, the size of the iron block standard material is (10-30) mm×(5-15) mm×(5-12) mm, and optionally the size is 20 mm×10 mm×8 mm.

[0069] Furthermore, the residual stress value of the iron block standard material is (3-7) MPa.

[0070] Furthermore, the standard deviation of the residual stress value of the iron block standard material is (0-3) MPa.

[0071] Furthermore, the error range of the residual stress value of the iron block standard material is ±3MPa.

[0072] Furthermore, the crystal glue adopts a crystal glue with high transparency, high fluidity and no bubbles after curing. Optionally, a crystal glue containing components A and B can be used; optionally, the crystal glue is purchased from Wenzhou Anergu New Materials Co., Ltd.

[0073] Furthermore, the present invention provides a preferred preparation method, which is as follows:

[0074] Example 1

[0075] The method for manufacturing the iron block residual stress standard material for calibrating the X-ray residual stress measuring instrument in this embodiment is carried out according to the following steps:

[0076] 1) Purchasing pure iron powder from the metal powder material market, using scanning electron microscopy to screen the particle size and iron content of the pure iron powder, and finally determining a pure iron powder (purchased from Guangzhou Metallurgy (Group) Co., Ltd.): the pure iron powder particle size is (1-8) μm, and the iron content (mass fraction, %) is not less than 95% (the iron powder identification result is as follows Figure 4 shown);

[0077] 2) Use an electronic balance to weigh 400g of the above-screened pure iron powder and pour it into a plastic beaker, then use an electronic balance to weigh 600g of crystal glue A and 200g of crystal glue B (purchased from Wenzhou Anergu New Materials Co., Ltd., A-71) with high transparency, high fluidity and no bubbles after curing, pour them into the plastic beaker filled with pure iron powder, and use an electric stirrer to stir for 20 minutes to fully mix the pure iron powder and crystal glue;

[0078] 3) Use a dust-free cloth and alcohol to clean 10 rectangular silicone molds (internal dimensions: 80mm long, 20mm wide, 20mm high), use a red marker to make a dot mark at 3 / 4 of the depth inside each rectangular silicone mold, and then pour the evenly stirred iron powder solution into the rectangular silicone mold, so that the depth of the iron powder solution reaches 3 / 4 of the depth of the silicone mold;

[0079] 4) Place 10 rectangular silicone molds filled with iron powder solution on a vibration isolation test table, rely on gravity and high fluidity to allow the iron powder particles to settle naturally, and let it dry and solidify naturally for 48 hours. During the drying and solidification process, it is forbidden to move or vibrate; after the drying and solidification, take out the iron powder solidified block from the rectangular silicone mold, and then fix the iron powder solidified block on a molybdenum wire-plated diamond wire cutting machine, and cut along the width direction of the iron powder solidified block, so that the iron powder solidified block is cut every 10 mm in the length direction. After the iron powder solidified block is cut, 7 iron powder solidified small blocks with a length of 20 mm, a width of 10 mm, and a height of about 15 mm are obtained (due to cutting loss, the width of the 8th iron powder solidified block is slightly smaller and is discarded), and 10 iron powder solidified blocks are cut in the same way, and finally 70 iron powder solidified small blocks are obtained;

[0080] 5) Use 800-mesh silicon carbide sandpaper to grind the line-cut surface of each iron powder solidified block on a metallographic grinder until the cutting marks disappear; then use 180-mesh and 800-mesh silicon carbide sandpaper in turn to thin and grind the back of each iron powder solidified block (the surface that does not contact the silicone mold during drying and solidification) to reduce the thickness of the iron powder solidified block from 15mm to 8mm, and make the thickness difference of the left, middle and right positions of the iron powder solidified block less than 0.01mm; after all the iron powder solidified blocks are ground, clean and wipe them with tap water and a dust-free cloth, and then blow dry them with a hair dryer;

[0081] 6) Check the front side of 70 iron powder solidified blocks (the side in contact with the bottom of the silicone mold during drying and solidification), remove the iron powder solidified blocks with bubbles, depressions or impurities on the surface, and finally leave 60 iron powder solidified blocks as candidates for iron block residual stress standard materials. The length of the standard material is 20 mm, the width is 10 mm, and the height is 8 mm. The preparation process of the iron block residual stress standard material is as follows: Figure 5 As shown;

[0082] 7) Use a blue marker and ruler to draw bisectors on the length and width of each iron powder solidified block to form a cross. The intersection is the midpoint of the iron powder solidified block. Then wrap it with a dust-free cloth with a length of 50 mm and a width of 50 mm and put it into a transparent plastic box with a length of 28 mm, a width of 21 mm and a height of 16 mm. Figure 6 As shown;

[0083] 8) First, send the high-precision digital inclinometer (DMI820) to the metrology technical organization for calibration. The X-ray residual stress tester generally needs to measure at least 7 ψ inclination angles to measure the residual stress. Therefore, the calibrated high-precision digital inclinometer is used to calibrate the 7 ψ inclination angles of the X-ray residual stress tester. Then, the calibrated X-ray residual stress tester is used to measure and determine the value of the iron block residual stress standard material candidate. The determination method and process are as follows: Figure 7As shown, specifically: first, the high-precision digital inclinometer is calibrated with the national angle reference device, and then the calibrated inclinometer is used to calibrate the 7 ψ inclination angles of the X-ray residual stress meter. Then, the calibrated X-ray residual stress meter is used to measure the residual stress of the iron block standard material, and the residual stress is calculated according to the calibrated data to obtain the standard value and uncertainty. The determination method and process are scientific and rigorous, and fully comply with the requirements and provisions of the technical specification JJF 1343-2022 "Determination of Value and Uniformity and Stability Evaluation of Standard Materials".

[0084] The traceability path of the X-ray residual stress tester to the value of the iron block residual stress standard material is as follows: Figure 8 As shown, specifically: the residual stress of the iron block standard material is traced back to 7 ψ inclination angles through the X-ray residual stress measuring instrument, and then the 7 ψ inclination angles are traced back to the angle of the inclinometer through the inclinometer, and finally the angle of the inclinometer is traced back to the national angle reference device, and the national angle reference device is directly related to the SI basic unit (meter). Therefore, the entire traceability chain is scientific and correct, and the residual stress is finally traced back to the SI basic unit (meter).

[0085] The calculation formula for X-ray residual stress measurement is as follows:

[0086]

[0087]

[0088]

[0089] σ φ =K1M (4)

[0090] Where, E is the theoretical value of the elastic modulus of the material in a stress-free state, ν is the theoretical value of the Poisson's ratio of the material in a stress-free state, θ0 is the theoretical value of the Bragg diffraction angle of the material in a stress-free state, and θ is the Bragg diffraction angle of the material in a stress state; K is called the stress constant, which is a constant related only to the nature of the material and the selected diffraction surface hkl. When the measured samples are of the same material and the selected diffraction surface index is the same, K is a constant. M is the square root of 2θ with respect to sin 2 The slope of ψ is measured by X-ray residual stress measurement at least 7 ψ angles to obtain the corresponding 2θ, and then the slope is calculated by least squares fitting (the relationship between 2θ and sin2ψ under plane stress state when the residual stress standard material of iron block is determined as follows Fig. 9 ), the residual stress σ can be calculated based on K and M φ Since K<0, when M<0 it is tensile stress, when M>0 it is compressive stress, and when M=0 there is no stress.

[0091] Randomly select 20 from 60 standard substances, according to Fig.10 9 points are selected at the schematic positions in the figure to measure and determine the residual stress (determination method: when the X-ray residual stress measuring instrument is used for detection, after the parameters are set, the instrument starts automatic testing, and then the instrument records the data and spectrum. The software of the instrument automatically calculates the residual stress results based on the data and the above formulas (1) to (3). After the test, the instrument automatically displays the residual stress results.), the determination results of the iron block residual stress standard material used for calibration of the X-ray residual stress measuring instrument are shown in Table 1. Table 1 shows that the iron block residual stress standard material prepared and determined in this proposal gives a specific residual stress value (3-7) MPa) and its standard deviation that is very close to zero, and the standard deviation is only (0-3) MPa, which is much lower than the error range of residual stress specimens at home and abroad.

[0092] Table 1. Results of calibration of residual stress reference materials of iron blocks for calibration of X-ray residual stress tester

[0093]

[0094] The results in Table 1 show that the determination results of the iron block residual stress standard material prepared by the present invention are accurate, reliable and have a good repetition rate.

[0095] The X-ray residual stress diffraction spectrum of the iron block residual stress standard material obtained by the X-ray residual stress measuring instrument during the determination process is as follows Figure 2 a. The results show that the diffraction peak of the iron block residual stress standard material prepared using (1-8) μm pure iron powder is narrow and sharp, with small stress and small error, and the error range is only ±3 MPa.

[0096] Comparative Example 1

[0097] The difference from Example 1 is that step 1) uses pure iron powder with a particle size of (1-45) μm (iron content (mass fraction, %) is not less than 95%), and the other steps are the same as Example 1.

[0098] The X-ray residual stress diffraction spectrum of the iron block residual stress standard material prepared in this comparative example is as follows: Figure 2 b. The results show that the diffraction peak of the iron block residual stress standard material prepared using (1-45) μm pure iron powder is broad and blunt, the stress is large and the error is large. The error range of the residual stress value is (11-29) MPa.

[0099] The present invention selects pure iron powder with a particle size of (1-8) μm and an iron content of not less than 95%, adopts highly transparent, highly fluid, and bubble-free crystal glue after solidification to mix the pure iron powder, and adopts an electric stirrer to fully stir and mix evenly, which can improve the density and uniformity of the iron powder in the solidified block. The residual stress of the iron block residual stress standard material obtained by selecting pure iron powder with a specific particle size ((1-8) μm) is small (as shown in Table 1), which solves the problems of poor density and uniformity of iron powder in the residual stress sample after solidification in the prior art, large residual stress of the sample, poor isotropy and poor uniformity.

[0100] The invention fully stirs and mixes pure iron powder and crystal glue evenly, pours them into a silica gel mold, dries and solidifies them in one go, relies on natural sedimentation by gravity and high fluidity, greatly improves the density and uniformity of the pure iron powder in the solidified block, reduces surface roughness and improves surface flatness; solves the problems of uneven and non-dense distribution of metal powder caused by manual sprinkling of pure iron powder and dripping of adhesive solution during the solidification process of pure iron powder, and it is difficult to obtain a surface with good flatness and low roughness by manually pressing the sample surface with a microscope slide.

[0101] The present invention adopts a calibrated high-precision inclinometer to calibrate the 7 ψ inclination angles of the X-ray residual stress measuring instrument, and then uses the calibrated X-ray residual stress measuring instrument to determine the value of the iron block residual stress standard material. The determination method is scientific, the traceability path of the residual stress value is clear, and the determination result is accurate and reliable, which solves the traceability and accuracy problems of the residual stress sample determination method in the prior art.

[0102] The preparation and determination method of the iron block residual stress standard material for calibration of the X-ray residual stress measuring instrument described in the present invention has very good reproducibility and repeatability of the preparation method, greatly reduces the influence of human factors on the value in the preparation process, and improves the density, uniformity and isotropy of residual stress in the standard material after solidification; the determination method is scientific, the traceability path of the residual stress value is clear, and the determination result is accurate and reliable, which can fully meet the calibration requirements of the X-ray residual stress measuring instrument and support the accurate measurement of residual stress in industrial fields such as aerospace, automobiles, ships, and machinery.

[0103] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An iron block standard material for calibrating an X-ray residual stress measuring instrument, characterized in that: The invention comprises an iron block obtained by settling and solidifying iron powder in crystal glue and then cutting the iron powder, wherein the iron powder is pure iron powder with a particle size of (1-8) μm and an iron content of ≥95%.

2. The iron block standard material according to claim 1, characterized in that: The iron block standard material is an iron block obtained by cutting off the upper uneven portion of an iron powder solidified iron block formed by mixing crystal glue and iron powder and then standing and settling to solidify; optionally, the cut upper uneven portion is 1 / 3 to 2 / 3 of the height of the iron powder solidified iron block, and optionally 1 / 3 to 1 / 2; And / or, the iron block standard material has no bubbles and no depressions; And / or, the back side of the iron block standard material is a polished surface; and / or; the thickness difference between the front and back of the iron block standard material at different positions is less than 0.01 mm; And / or, the size of the iron block standard material is (10-30) mm×(5-15) mm×(5-12) mm, and optionally the size is 20 mm×10 mm×8 mm.

3. The iron block standard material according to claim 1 or 2, characterized in that: The residual stress value of the iron block standard material is (3-7) MPa; And / or, the standard deviation of the residual stress value of the iron block standard material is (0-3) MPa; And / or, the error range of the residual stress value of the iron block standard material is ±3MPa; And / or, the crystal glue is highly transparent, highly fluid, and bubble-free after curing. Optionally, crystal glue containing components A and B may be used; optionally, the crystal glue is purchased from Wenzhou Anergu New Materials Co., Ltd.

4. A method for preparing an iron block standard material for calibrating an X-ray residual stress measuring instrument, characterized in that: The method comprises the following steps: mixing iron powder and crystal glue evenly, pouring the mixture into a mold, letting the mixture stand, settling naturally, and solidifying to form an iron powder solidified block, cutting off the uneven part of the upper iron powder, grinding the back, and obtaining an iron block residual stress standard material.

5. The preparation method according to claim 4, characterized in that: The weight ratio of the iron powder to the crystal glue is 1:(1-5), optionally 1:(2-3); Optionally, the mixing method is stirring; and / or, the upper uneven portion cut off is 1 / 3 to 2 / 3 of the height of the iron powder solidified block, and optionally 1 / 3 to 1 / 2; And / or, the iron powder is pure iron powder with a particle size of (1-8) μm and an iron content of ≥95%; And / or, the crystal glue is highly transparent, highly fluid, and bubble-free after curing. Optionally, a crystal glue containing components A and B may be used.

6. The preparation method according to claim 4 or 5, characterized in that: After cutting and grinding, the thickness difference between the front and back of the iron block residual stress standard material at different positions is less than 0.01 mm; And / or, the residual stress value of the iron block residual stress standard material is (3-7) MPa; And / or, the standard deviation of the residual stress value of the iron block residual stress standard material is (0-3) MPa; And / or, the error range of the residual stress value of the iron block residual stress standard material is ±3 MPa.

7. A method for determining the value of an iron block standard material according to any one of claims 1 to 3 or an iron block standard material prepared by the preparation method according to any one of claims 4 to 6, characterized in that: include: 1) Calibrate the X-ray residual stress measuring instrument; 2) The residual stress of the candidate iron block residual stress standard material is measured by a calibrated X-ray residual stress measuring instrument. The residual stress is calculated based on the data detected after calibration to obtain the standard value and uncertainty. The X-ray residual stress calculation formula is as follows: σ φ =K1M (4) Where, E is the theoretical value of the elastic modulus of the material in a stress-free state, ν is the theoretical value of the Poisson's ratio of the material in a stress-free state, θ0 is the theoretical value of the Bragg diffraction angle of the material in a stress-free state, and θ is the Bragg diffraction angle of the material in a stress state; K is called the stress constant, which is a constant only related to the nature of the material and the selected diffraction surface hkl. When the measured samples are of the same material and the selected diffraction surface index is the same, K is a constant; M is the square root of 2θ with respect to sin 2 The slope of ψ is obtained by measuring the corresponding 2θ at at least 7 ψ angles using X-ray residual stress measurement. The slope is then calculated using the least squares fitting method. The residual stress σ is calculated based on K and M. φ .

8. The value determination method according to claim 7, characterized in that: Calibration includes: The high-precision digital inclinometer is used to measure and calibrate the residual stress; the calibrated high-precision digital inclinometer is used to calibrate at least 7 ψ tilt angles of the X-ray residual stress measuring instrument.

9. A method for tracing the source of the iron block standard material according to any one of claims 1 to 3 or the iron block standard material prepared by the preparation method according to any one of claims 4 to 6, characterized in that: include: The residual stress of the iron block standard material is traced back to at least 7 ψ inclination angles through an X-ray residual stress measuring instrument, and then at least 7 ψ inclination angles are traced back to the angle of the inclinometer through a calibrated inclinometer, and finally the angle of the inclinometer is traced back to the national angle reference device.

10. Use of the iron block standard material described in any one of claims 1 to 3, or the iron block standard material prepared by the preparation method described in any one of claims 4 to 6, or the determination method described in claim 7 or 8, or the traceability method described in claim 9 in inspecting and evaluating an X-ray residual stress measuring instrument.