A method for improving the bonding strength of soft magnetic alloy sheets

By using specific ratio coarse liquid of HCL, HNO3 and deionized water to process the surface of the soft magnetic alloy sheet, the problem of insufficient bonding strength of the stator core of the micro special motor is solved, and efficient and environmentally friendly bonding strength is achieved Improves the stability of wire cutting processing, meeting the requirements of high bond strength, low cost and easy operation.

CN116065153BActive Publication Date: 2024-12-03AVIC SHAANXI HUAYAN AERO INSTR
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211440862.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-17
Publication Date
2024-12-03
Estimated Expiration
2042-11-17

AI Technical Summary

Technical Problem

The prior art cannot effectively improve the bonding strength of the stator core of the micro-special motor, resulting in easy cracking during online cutting and processing, and the traditional methods cannot meet the requirements of high bonding strength, low cost, easy operation and environmental protection at the same time.

Method used

The surface of the soft magnetic alloy sheet is roughened by a coarse liquid made of HCL, HNO3 and deionized water at a volume ratio of 36-38%: 65-68%: 20-25: 320-360: 600-650. To improve bonding strength, and to ensure uniformity of the glue layer by controlling the coarse time and spraying thickness, the stable processing of the stator core is achieved.

Benefits of technology

It significantly improves the bonding strength of soft magnetic alloy sheets, and the tensile strength is increased from 200N/cm2 to above 360N/cm2, ensuring the stability and process reliability of subsequent wire cutting processing, avoiding stator core cracking and wire cutting Problems with cutting the thread during the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116065153B_ABST
    Figure CN116065153B_ABST
Patent Text Reader

Abstract

In order to solve the technical problem that soft magnetic alloy sheet stacks are prone to cracking during wire cutting due to insufficient bonding strength, the present invention proposes a method for improving the bonding strength of soft magnetic alloy sheets from the perspective of engineering practicality. The soft magnetic alloy sheets are roughened by configuring an environmentally friendly roughening liquid that is easy to operate, easy to control the roughening effect and has high roughening efficiency, so as to obtain a microscopic rough surface that can effectively increase the bonding area, thereby greatly improving the bonding strength of parts with the same specifications. At the same time, by controlling process parameters such as roughening time, glue spraying time, glue layer thickness, and glue curing temperature, the final stator and rotor core blanks can meet the process requirements of wire cutting, thereby ensuring that they do not crack and the process stability of wire cutting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of micro-special motor manufacturing, and specifically relates to a method for improving the bonding strength of soft magnetic alloy sheets. The soft magnetic alloy involved in the invention has the following elements in mass percentage: Mn 0.3% to 0.6%, Si 0.15% to 0.3%, Ni 49.0% to 50.5%, and the balance is Fe. Background Art

[0002] The stator and rotor are the core components of micro special motors. At present, the stator and rotor cores of high-precision micro special motors are made by first processing the soft magnetic alloy sheets into circular ring sheets, and then bonding the circular ring sheets with X98-11 acetal drying glue to form a blank after heat treatment to obtain magnetic properties. The blank is then processed by wire cutting. Since wire cutting generates a lot of heat, the bonding strength of X98-11 acetal drying glue decreases rapidly with the increase of temperature. Therefore, the subsequent wire cutting is very destructive to the bonding strength of the stator and rotor cores, which can easily lead to cracking of the stator and rotor cores. Therefore, the bonding of the soft magnetic alloy sheets must reach a certain strength to ensure the stability of subsequent processing.

[0003] Traditional methods to improve bonding strength include mechanical grinding, surface sandblasting, chemical roughening with dichromate formula, etc. Mechanical grinding has limited improvement on bonding strength and cannot solve the problem of stator and rotor core cracking; surface sandblasting can effectively improve bonding strength, but it causes great damage to the punch die and has poor economic benefits; dichromate formula roughening takes about 10 minutes, has low roughening efficiency, and the roughening liquid contains heavy metal ions, which is not environmentally friendly.

[0004] In summary, traditional methods of improving bonding strength cannot simultaneously meet the requirements of high bonding strength, low cost, easy operation, and green environmental protection. It is urgent to develop a method for improving the bonding strength of soft magnetic alloy sheets with high bonding strength, low cost, easy operation, and green environmental protection. Summary of the invention

[0005] In order to solve the technical problem that soft magnetic alloy sheet stacks are prone to cracking during online cutting due to insufficient bonding strength, the present invention proposes a method for improving the bonding strength of soft magnetic alloy sheets from an engineering practical perspective. The method has a simple processing process, is fast and efficient, has high bonding strength, and is green and environmentally friendly.

[0006] The technical solution of the present invention is:

[0007] A roughening liquid is used for roughening the surface of a soft magnetic alloy sheet to improve the bonding strength; the special feature of the roughening liquid is that the roughening liquid is mixed with HCL with a mass concentration of 36-38%, HNO3 with a mass concentration of 65-68% and deionized water in a volume ratio of 20-25:320-360:600-650.

[0008] Furthermore, the volume ratio of HCL, HNO3 and deionized water is 1:13:25.

[0009] The present invention also provides a method for improving the bonding strength of soft magnetic alloy sheets, the special feature of which is that the surface of the soft magnetic alloy sheets is firstly roughened by using the above-mentioned roughening liquid, and then bonding is performed.

[0010] The present invention also provides a method for manufacturing a stator and rotor core blank, which is special in that it comprises the following steps:

[0011] Step 1: Prepare the roughening solution

[0012] Mixing HCL with a mass concentration of 36-38%, HNO3 with a mass concentration of 65-68%, and deionized water in a volume ratio of 20-25:320-360:600-650 to prepare a roughening solution;

[0013] Step 2: Surface roughening

[0014] Several soft magnetic alloy circular ring pieces with magnetic properties are used as test pieces, and are placed in the roughening solution prepared in step 1 for 1-4 seconds. During this period, the soft magnetic alloy circular ring pieces are taken out in real time and compared with the standard soft magnetic alloy pieces under a 10x magnifying glass. When the difference between the number of pits on a single surface and the average of the pit area on a single surface of the standard sample is less than 5%, it means that the roughening meets the requirements. The average total immersion time of the test piece in the roughening solution is taken as the roughening operation time, and the roughening is subsequently performed according to the roughening operation time;

[0015] Step 3: Make the stator and rotor core blanks

[0016] Spraying 0.007-0.012 mm thick X98-11 acetal drying glue onto the end surface of the soft magnetic alloy circular ring sheet roughened in step 2, and then stacking a corresponding number of soft magnetic alloy circular ring sheets according to the number of sheets required by the stator and rotor core design to form a laminated part, applying pressure to the laminated part and curing the glue at 155±5° C. to obtain a stator and rotor core blank;

[0017] Step 4, tensile strength test

[0018] The tensile strength of the stator and rotor core blanks is tested, and the tensile strength is ≥360N / cm 2 , indicating that the roughening effect is good, and the stator and rotor core blanks that meet the requirements of subsequent wire cutting processing are obtained.

[0019] Furthermore, in step 1, HCL, HNO3 and deionized water are mixed in a volume ratio of 1:13:25 to prepare a roughening solution.

[0020] Furthermore, in the step 2, the soft magnetic alloy sheet is placed in the roughening liquid for 2-3 seconds to complete the surface roughening.

[0021] Furthermore, in step 3, X98-11 acetal drying glue solution is sprayed within 24 hours after the roughening is completed.

[0022] Furthermore, in step 3, 49 N / cm is applied to the laminate. 2 pressure.

[0023] Furthermore, in step 2, a plurality of soft magnetic alloy sheets are placed in a series on a hanger at intervals, and the soft magnetic alloy circular ring sheets are placed in the roughening liquid by operating the hanger.

[0024] The present invention also provides a stator and rotor core, which is special in that it is made from a stator and rotor core blank through wire cutting; the stator and rotor core blank is made by the above-mentioned method for making a stator and rotor core blank.

[0025] The beneficial effects of the present invention are:

[0026] 1. The present invention is equipped with an environmentally friendly roughening liquid (without heavy metal ions) that is easy to operate, easy to control the roughening effect and has high roughening efficiency. The soft magnetic alloy sheet treated with the roughening liquid can obtain a microscopic rough surface that can effectively increase the bonding area, so that the bonding strength of parts of the same specification is greatly improved. The tensile strength test of the stator and rotor blanks (ferromagnetic alloy laminations) with the same structure obtained by bonding with the same thickness of X98-11 acetal drying glue is compared: when not roughened, the tensile strength is 200N / cm 2 After being roughened by the roughening liquid of the present invention, the tensile strength can reach at least 360N / cm 2 , up to 600N / cm 2 Therefore, the specially configured roughening liquid of the present invention can effectively improve the bonding strength between the soft magnetic alloy sheets, laying a foundation for the stability of subsequent wire cutting processing.

[0027] 2. Considering that the X98-11 acetal drying glue used for bonding soft magnetic alloy sheets not only plays a bonding role but also an insulating role, and the subsequent wire cutting of the stator and rotor blanks requires a thin and uniform glue layer between two adjacent soft magnetic alloy sheets. If the surface of the soft magnetic alloy sheet is too rough (over-roughening), the glue layer between the two adjacent soft magnetic alloy sheets will be uneven, resulting in the wire cutting of parts during the subsequent wire cutting process. Therefore, in addition to strictly controlling the thickness of the spray glue, the present invention also controls the surface state of the roughened soft magnetic alloy sheet through special roughening liquid ratio and roughening time control. After repeated tests and verifications, the final roughening effect can meet the uniformity requirement of the glue layer between sheets. A standard sample for comparative inspection of the roughening effect has been formulated to ensure the process stability and reliability of subsequent wire cutting.

[0028] 3. The roughening liquid formula of the present invention is preferably HCL (mass concentration of 36-38%): HNO3 (mass concentration of 65-68%): H2O = 1:13:25 (volume ratio). After repeated experiments and verification, it is found that the roughening liquid only needs to control the roughening time to 2-3 seconds to complete the surface roughening treatment of the soft magnetic alloy sheet to obtain a suitable micro-rough feature surface. Subsequently, it is only necessary to control the thickness of the spray glue to obtain the bonding strength and uniformity of the glue layer that meet the requirements of the wire cutting processing, thereby eliminating the problem of cracking of the stator and rotor core blanks during the wire cutting process and the problem of wire cutting causing the wire to damage parts.

[0029] 4. The experimental results show that the method of the present invention can be widely applied to soft magnetic alloy sheets such as 1J79 and 1JH3. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a schematic diagram of the state when the soft magnetic alloy ring sheet is roughened.

[0031] Figure 2 The following is a comparison diagram of the effects of the roughening liquid of the present invention on the soft magnetic alloy ring sheet after roughening and before roughening, wherein (a) is before roughening and (b) is after roughening.

[0032] Figure 3 This is a 16-fold magnification comparison of the image before and after coarsening, (a) is before coarsening, and (b) is after coarsening.

[0033] Figure 4 This is a physical picture of the soft magnetic alloy sheet stack made by the present invention. DETAILED DESCRIPTION

[0034] The present invention will be further described below in conjunction with the accompanying drawings.

[0035] One of the means of improving the bonding strength of the soft magnetic alloy sheet of the present invention is to configure a special roughening liquid, which has the characteristics of high roughening efficiency, controllability and environmental protection. The roughening liquid is prepared by mixing HCL with a mass concentration of 36% to 38%, HNO3 with a mass concentration of 65-68% and deionized water in a volume ratio of 20-25:320-360:600-650.

[0036] The formula design idea and mechanism of the roughening liquid provided by the present invention are:

[0037] Considering that the main components of soft magnetic alloy sheets are iron and nickel, which have high reactivity, the traditional "aqua regia" (hydrochloric acid: nitric acid = 3:1~5:1) strong oxidizing ratio (mainly used to dissolve inert metals) and single hydrochloric acid or nitric acid (single hydrochloric acid has a long coarsening time, and single nitric acid has extremely low utilization rate) were abandoned when designing the formula of the roughening liquid.

[0038] The roughening solution of the present invention is prepared by mixing HCL with a mass concentration of 36-38%, nitric acid with a mass concentration of 65-68% and deionized water in a specific volume ratio; because the iron and nickel in the soft magnetic alloy sheet will be passivated when encountering concentrated nitric acid, and the reaction rate is low, a large amount of deionized water is introduced when preparing the roughening solution in order to reduce the concentration of nitric acid and improve its reaction activity; in addition, when the single nitric acid reacts chemically with the soft magnetic alloy sheet, the iron element in the soft magnetic alloy sheet will preferentially react with the nitric acid to quickly form trivalent iron ions, and the trivalent iron ions will precipitate in a strongly acidic environment with a pH value of 2.7, resulting in an extremely low utilization rate of the roughening solution; combined with actual experience and through a large amount of research and experimental verification, it is found that: appropriately introducing chloride ions into the nitric acid , which can balance the reaction rates of iron, nickel and nitric acid to obtain a uniform micro-rough surface, reduce the oxidizing property of nitric acid, and prevent Fe(OH)3 precipitation from being produced during the use of the roughening solution, thereby improving the utilization rate of the roughening solution; the present invention introduces chloride ions by adding hydrochloric acid to nitric acid, but in practice it is found that: as the concentration of hydrochloric acid increases, the reaction rate is too fast and the roughening effect becomes uncontrollable, and the reduction in the concentration of hydrochloric acid causes the reaction rate to become too slow and the roughening efficiency is low; as the amount of hydrochloric acid added increases, the roughening reaction time becomes shorter, but if the amount of hydrochloric acid added exceeds a certain proportion, the micro-pits on the surface of the soft magnetic alloy sheet after roughening become larger, making it impossible to ensure the uniformity of the glue layer after spraying, thereby affecting the stability of the subsequent wire cutting process.

[0039] Therefore, taking into account the bonding strength, uniformity of the adhesive layer and controllability of the roughening, the present invention configures the above-mentioned roughening liquid. Especially when the formula of the above-mentioned roughening liquid is HCL (mass concentration is 36-38%): HNO3 (mass concentration is 65-68%): H2O = 1:13:25 (volume ratio), after a large number of practical verifications, it is only necessary to place the soft magnetic alloy sheet in the roughening liquid for 2-3s to achieve the required roughening effect, and only the thickness of the adhesive layer needs to be strictly controlled later, making the operation simpler, more convenient and controllable.

[0040] In addition to using the above-mentioned roughening liquid to roughen the steel to improve the bonding strength between the soft magnetic alloy sheets, the present invention also controls the process parameters such as the roughening time, the glue spraying time, the glue layer thickness, and the glue curing temperature to ensure that the stator and rotor core blanks finally manufactured meet the process requirements of wire cutting processing, thereby ensuring that they do not crack and the process stability of wire cutting processing.

[0041] The specific method for manufacturing the stator and rotor core of the present invention is as follows:

[0042] Step S1: preparing the above-mentioned roughening liquid;

[0043] Step S2: Roughening

[0044] A plurality of soft magnetic alloy circular ring sheets with magnetic properties are placed in the roughening liquid configured in step S1 for 1-4 seconds respectively. During this period, the soft magnetic alloy circular ring sheets are taken out in real time (for example, at intervals of 1 second) and compared with the standard soft magnetic alloy sheets (pre-made soft magnetic alloy sheets with a roughening degree that meets the requirements, and the standard soft magnetic alloy sheets can be made into laminated parts that pass the tensile strength test requirements according to the design requirements) under a 10x magnifying glass for inspection. If the state of its single surface is basically consistent with the state of the single surface of the standard sample, there is no obvious difference (it can be determined based on the number of pits on a single surface and the average value of the pit area size, and if the difference is less than 5%, it is considered that there is no obvious difference; Figure 2 , 3 is a comparison chart before and after roughening), indicating that the roughening meets the requirements. At this time, the average total immersion time of these specimens in the roughening liquid can be used as the roughening operation time, and the remaining soft magnetic alloy discs can be roughened according to the roughening operation time. In order to further improve the roughening efficiency and facilitate the control of the roughening time, multiple soft magnetic alloy circular rings can be placed on the hanger at intervals (such as Figure 1As shown), take good protection, operate the hanger in a ventilated place, and place the soft magnetic alloy ring piece in the roughening liquid, or remove it from the roughening liquid by operating the hanger; after repeated verification, when the roughening liquid is configured according to HCL (mass concentration is 36-38%): HNO3 (mass concentration is 65-68%): H2O = 1:13:25 (volume ratio), the soft magnetic alloy ring piece can achieve the roughening effect that meets the wire cutting requirements in the roughening liquid for 2-3s. In actual operation, there is no need for real-time comparison, and the roughening effect can be controlled by controlling the roughening time, which is convenient to operate.

[0045] Step S3: Making stator and rotor core blanks

[0046] Spray 0.007-0.012 mm thick X98-11 acetal drying glue onto the end surface of the soft magnetic alloy circular ring piece roughened in step 2, and then stack the soft magnetic alloy circular ring pieces according to the specified number of pieces to form a Figure 4 As shown in the figure, pressure is applied to the laminated parts according to the area (a pressure of 5Kg*9.8N / Kg=49N is applied per square centimeter) and the glue is solidified at 155±5℃ to obtain the stator and rotor core blanks; when spraying the glue in this step, it is best to spray the glue within the specified time and carry out the bonding process.

[0047] Step S4: Tensile strength test

[0048] The tensile strength test of the stator and rotor core blanks obtained in step S3 is used to determine the results. If the tensile strength of the first piece is ≥360N / cm 2 It means that it meets the requirements of subsequent wire cutting processing; if the tensile strength is less than 360N / cm 2 It means that the roughening is unqualified and there is a risk in using it. You can return and roughen it again.

[0049] After repeated practical verification, the tensile strength of the stator and rotor core blanks produced by the method of the present invention is greater than or equal to 360N / cm 2 , in line with the subsequent wire cutting processing requirements.

Claims

1. A roughening liquid for roughening the surface of a soft magnetic alloy sheet to improve bonding strength; characterized in that: The roughening liquid is prepared by mixing HCL with a mass concentration of 36-38%, HNO3 with a mass concentration of 65-68%, and deionized water in a volume ratio of 20-25:320-360:600-650.

2. The roughening liquid according to claim 1, characterized in that: The volume ratio of the HCL, HNO3 and deionized water is 1:13:

25.

3. A method for improving the bonding strength of soft magnetic alloy sheets, characterized in that: The surface of the soft magnetic alloy sheet is first roughened using the roughening liquid described in claim 1 or 2, and then bonded.

4. A method for manufacturing a stator and rotor core blank, characterized in that: The following steps are involved: Step 1: Prepare the roughening solution Mixing HCL with a mass concentration of 36-38%, HNO3 with a mass concentration of 65-68%, and deionized water in a volume ratio of 20-25:320-360:600-650 to prepare a roughening solution; Step 2: Surface roughening Several soft magnetic alloy circular rings with magnetic properties are used as test pieces, and are placed in the roughening solution prepared in step 1 for 1-4 seconds. During this period, the soft magnetic alloy circular rings are taken out in real time and compared with the standard soft magnetic alloy sheets under a 10x magnifying glass. When the difference between the number of pits on a single surface and the average of the pit area on a single surface of the standard sample is less than 5%, it means that the roughening meets the requirements. The average total immersion time of the test piece in the roughening solution is taken as the roughening operation time, and the roughening is subsequently performed according to the roughening operation time; Step 3: Make the stator and rotor core blanks Spraying 0.007-0.012 mm thick X98-11 acetal drying glue onto the end surface of the soft magnetic alloy circular ring sheet roughened in step 2, and then stacking a corresponding number of soft magnetic alloy circular ring sheets according to the number of sheets required by the stator and rotor core design to form a laminated part, applying pressure to the laminated part and curing the glue at 155±5° C. to obtain a stator and rotor core blank; Step 4, tensile strength test The tensile strength of the stator and rotor core blanks is tested, and the tensile strength is ≥360N / cm 2 , indicating that the roughening effect is good, and the stator and rotor core blanks that meet the requirements of subsequent wire cutting processing are obtained.

5. The method for manufacturing a stator and rotor core blank according to claim 4, characterized in that: In the step 1, HCL, HNO3 and deionized water are mixed in a volume ratio of 1:13:25 to prepare a roughening solution.

6. The method for manufacturing a stator and rotor core blank according to claim 5, characterized in that: In the step 2, the soft magnetic alloy sheet is placed in the roughening solution for 2-3 seconds to complete the surface roughening.

7. The method for manufacturing a stator and rotor core blank according to claim 6, characterized in that: In step 3, X98-11 acetal drying glue solution is sprayed within 24 hours after the roughening is completed.

8. The method for manufacturing a stator and rotor core blank according to claim 7, characterized in that: In step 3, 49 N / cm is applied to the laminate. 2 pressure.

9. The method for manufacturing a stator and rotor core blank according to any one of claims 4 to 8, characterized in that: In the step 2, a plurality of soft magnetic alloy sheets are placed in a series on a hanger at intervals, and the soft magnetic alloy circular ring sheets are placed in the roughening liquid by operating the hanger.

10. A stator and rotor core, characterized in that: The stator and rotor core blank is made by wire cutting; the stator and rotor core blank is made by the method for making the stator and rotor core blank according to any one of claims 4-9.