Preparation method of anhydrous stemming sample for blast furnace
By employing baking at 60–80℃, molding pressure of 35kN–45kN, and carbonization treatment at 500℃ in the preparation of anhydrous taphole clay samples for blast furnaces, the problem of unclear molding in existing methods has been solved, the molding effect of the samples has been improved, and the samples are suitable for blast furnace performance testing.
Patent Information
- Application Number
- CN202411339367.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-22
AI Technical Summary
The existing methods for preparing anhydrous taphole clay samples for blast furnaces lack clear operational procedures, especially regarding molding temperature and pressure, resulting in poor molding effects that fail to meet the requirements for performance research.
The preparation method adopts a baking temperature of 60-80℃, a molding pressure of 35kN (5.47MPa)-45kN (7.03MPa) and a carbonization treatment temperature of 500℃ for 5h. The method includes steps such as crushing the clay, electric heating drying, molding and pressing, and carbonization treatment to ensure that the sample meets the dimensional requirements.
It achieves simple operation, determines suitable temperature and pressure, improves the molding effect of anhydrous taphole clay samples, and is suitable for blast furnace performance testing.
Smart Images

Figure CN119000219A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anhydrous taphole clay, and particularly relates to a method for preparing anhydrous taphole clay samples for blast furnaces. Background Art
[0002] After the blast furnace has finished tapping molten iron and slag, taphole is filled with mud. Since the mud is squeezed in with a mud cannon, this kind of mud is called taphole mud. Anhydrous taphole mud generally uses high-quality and high-purity raw materials such as brown corundum, silicon carbide, coke powder, high-quality bonding clay, etc. as the main raw materials, and is added with different carbon materials such as coal tar, anthracene oil or phenolic resin as a binder. It has the advantages of high high-temperature strength and good resistance to slag erosion. The use of anhydrous taphole mud can extend the tapping time of the taphole, reduce the number of tapping times, and is not prone to damp taphole. Therefore, in order to improve the performance of the taphole mud product, it is very necessary to conduct a performance study on it; preparing anhydrous taphole mud samples is the first step in conducting a performance study on it, and it is also an important part of the test method. However, the existing standard method for preparing anhydrous taphole mud samples for blast furnaces stipulates that: the 50°C dried For uniform cannon clay, first use a hammer to tamp the sample in a 160mm×40mm×40mm mold. It is required to be non-stratified, with a flat surface and dense edges and corners. Then it can be demoulded directly or dried and demoulded. When preparing samples in the laboratory according to this standard, some specific operation regulations are vague. For example, the binders used in cannon clay mainly include organic substances such as tar, anthracene oil, asphalt and resin, which exist as hard solids at room temperature and are not conducive to molding. Therefore, they need to be baked at a certain temperature to obtain plasticity. This standard only stipulates baking at 50°C, and does not specify the baking time and method; the molding method described in this standard is tamping sample preparation, and the molding pressure is not specified; therefore, it is very necessary to provide a preparation method for anhydrous cannon clay samples for blast furnaces that is simple to operate, determines the appropriate temperature and pressure, and has good sample preparation effect. Summary of the invention
[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and to provide a method for preparing anhydrous taphole mud samples for blast furnaces which has the advantages of simple operation, determination of suitable temperature and pressure, and good sample preparation effect.
[0004] The object of the present invention is achieved in this way: a method for preparing anhydrous taphole mud sample for blast furnace, the preparation method comprising the following steps:
[0005] Step 1: Sample preparation: Chisel the anhydrous taphole mud to be tested into small pieces, evenly take a certain amount of the small pieces and put them into an electric drying oven for baking;
[0006] Step 2: Sample preparation: Weigh an appropriate amount of small pieces of taphole clay baked in the above steps, quickly and evenly put them into the mold, and press them into shape under the pressure of the molding press;
[0007] Step 3: After demoulding, move the sample to a rigid flat plate, keep the molding surface facing up, and measure the size of the sample with a vernier caliper. The size should meet the requirements, otherwise redo it;
[0008] Step 4: Carbonization treatment: Place the qualified sample in a sagger and perform carbonization treatment in a carbonization furnace under the condition of burying carbon (graphite powder);
[0009] Step 5: Record: including: sample name, brand, batch number, production date, sampling, sample preparation date and tester information.
[0010] In the step 1, the anhydrous taphole mud to be tested is broken into small pieces of 30-20 mm.
[0011] In step 1, the baking temperature of the electric drying oven is between 60-80° C., the heating rate is 5° C. / min, and the baking time is 20 min.
[0012] The pressure range of the molding press in step 2 is 35KN-45KN.
[0013] The sample size standard in step 3 is: length 160±2.00mm, width 40±2.00mm, height 40±2.00mm.
[0014] The minimum scale of the vernier caliper in step 3 is 0.02 mm.
[0015] The carbonization treatment temperature in step 4 is 500° C., the treatment time is 5 h, and the heating rate is 3-5° C. / min.
[0016] When the graphite powder is buried in the carbonization treatment in step 4, the graphite thickness is 45-50 mm more than the sample, which is thick enough to ensure that the sample is not oxidized and the graphite powder covers densely.
[0017] The carbonization treatment in step 4 is for soft taphole clay that is easily deformed after molding. In order to prevent deformation after molding, it should be fixed with a mold of corresponding size, and then carbonization treatment is carried out.
[0018] The carbonization furnace in step 4 is an electric furnace with a temperature control device and a smoke exhaust device.
[0019] The beneficial effects of the invention are as follows: the invention is a method for preparing a sample of anhydrous cannon clay for a blast furnace. During use, the invention studies the method for preparing a sample of anhydrous cannon clay for a blast furnace. Before the sample of anhydrous cannon clay for a blast furnace is prepared, the sample should be baked at a suitable baking temperature of 60 to 80°C. For easy operation, the anhydrous cannon clay should be broken into small pieces of 20 to 30 mm, and the baking time is about 20 minutes. When the sample of anhydrous cannon clay for a blast furnace is prepared, the optimal molding pressure is 35 kN (5.47 MPa) to 45 kN (7.03 MPa). The sample of anhydrous cannon clay for a blast furnace needs to be carbonized before high-temperature performance testing. The optimal carbonization treatment temperature is 500°C, the insulation time is 5 hours, and the atmosphere is carbon buried or other reducing atmospheres. The invention has the advantages of simple operation, determination of suitable temperature and pressure, and good sample preparation effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a relationship diagram between the sample volume density and the molding pressure of the present invention.
[0021] Figure 2 This is a graph showing the mass loss rate of anhydrous taphole mud after heat treatment at different temperatures of the present invention.
[0022] Figure 3 It is a schematic diagram of the room-temperature flexural strength of anhydrous taphole clay after heat treatment at different temperatures of the present invention.
[0023] Figure 4 It is a schematic diagram of the volume density of the sample after heat treatment at different temperatures of the present invention.
[0024] Figure 5 It is a schematic diagram of the apparent porosity of the sample after heat treatment at different temperatures of the present invention. DETAILED DESCRIPTION
[0025] The experimental raw materials come from the anhydrous taphole clay currently used in different large blast furnaces of 5 steel mills. The main chemical composition is shown in Table 1.
[0026] Table 1 Chemical composition of anhydrous taphole mud %
[0027]
[0028] The present invention will be further described below in conjunction with the accompanying drawings.
[0029] Example 1
[0030] like Figure 1-5 As shown, a method for preparing anhydrous taphole mud sample for blast furnace comprises the following steps:
[0031] Step 1: Preparation before sample preparation: Chisel the anhydrous taphole mud to be tested into small pieces of 30 mm, evenly take a certain amount of the small pieces and put them into the electric drying oven for baking. The baking temperature is between 60 ° C, the heating rate is 5 ° C / min, and the baking time is 20 min;
[0032] Step 2: Sample preparation: Weigh an appropriate amount of small pieces of taphole clay baked in the above steps, quickly and evenly put them into the mold, and press them into shape under a pressure of 35KN on a molding press;
[0033] Step 3: After demoulding, move the sample to a rigid flat plate, keep the molding surface facing up, and measure the size of the sample with a vernier caliper. The size should meet the requirements, otherwise redo it;
[0034] Step 4: Carbonization treatment: Place the qualified sample in a sagger and perform carbonization treatment in a carbonization treatment furnace under the condition of burying carbon (graphite powder). The carbonization treatment temperature is 500℃, the treatment time is 5h, and the heating rate is 3℃ / min. When burying graphite powder, the graphite thickness is 45mm more than the sample, which has enough thickness to ensure that the sample is not oxidized, and at the same time, the graphite powder must be densely covered.
[0035] Step 5: Record: including: sample name, brand, batch number, production date, sampling, sample preparation date and tester information.
[0036] The sample size standard in step 3 is: length 160±2.00mm, width 40±2.00mm, height 40±2.00mm.
[0037] The minimum scale of the vernier caliper in step 3 is 0.02 mm.
[0038] The carbonization treatment in step 4 is for soft taphole clay that is easily deformed after molding. In order to prevent deformation after molding, it should be fixed with a mold of corresponding size, and then carbonization treatment is carried out.
[0039] The carbonization furnace in step 4 is an electric furnace with a temperature control device and a smoke exhaust device.
[0040] In this embodiment, the baking temperature and baking time before the anhydrous cannon mud sample preparation are determined as follows: at room temperature, the binder (such as tar) in the anhydrous cannon mud has a large viscosity and poor fluidity, so the anhydrous cannon mud at room temperature is very hard. The greater the viscosity of the tar, the greater the extrusion pressure of the cannon mud. The kinematic viscosity of the tar can be determined by the following formula: lglg (v+0.8) = 13.80-5.33lgT, where v is the kinematic viscosity, cm 2 / s; T is temperature, K; Engler viscosity is often used in practical applications, that is, at a certain temperature, the ratio of the time (s) required for liquid tar to flow out of 200 mL from the Engler viscometer to the time (s) required for water to flow out of 200 mL at 20°C, expressed as Et Indicates that the Engler viscosity of general tar is 20-30E at 40°C t ; 80℃ is 3-5E t ; 150℃ is 1-2E t ; From the above formula, we can know that the viscosity of tar is related to temperature. The higher the temperature, the smaller the viscosity and the better the fluidity. Therefore, in order to make the hard taphole clay have a certain plasticity and be easy to press into the required shape, it must be baked at a certain temperature.
[0041] ① Test process: Weigh 500g of each of the 1#-5# anhydrous taphole mud test samples, put them into a constant temperature drying oven and bake them at 50℃, 60℃, 70℃, 80℃, 90℃ and 100℃ respectively, and the heating system is 5℃ / min. Observe the appearance of the taphole mud until it becomes soft, and record the baking time; after baking and softening, press them into 40mm×40mm×160mm test samples;
[0042] ②Analysis of test results: Through the test, it was found that when the baking temperature was below 60℃, the appearance of the five kinds of cannon clay had no metallic luster and poor softness. When pressed into shape, the samples were not dense and had many cracks and delaminations. When the baking temperature was 60-80℃, the cannon clay had a metallic luster, soft texture and good plasticity. This was because the fluidity of the organic binder in the cannon clay increased with increasing temperature. When the baking temperature was 90℃ and 100℃, the cannon clay had a more metallic luster, but during molding, it was too thin and mud appeared and stuck to the mold wall. After demoulding, the sample was easily deformed, affecting the later performance test. Therefore, the suitable baking temperature before the anhydrous cannon clay was molded was 60-80℃. In order to facilitate laboratory operation, the cannon clay was broken into small pieces of 20-30mm. It was found through observation that when baked at 60-80℃ for about 20min, the inside and outside of the small pieces of cannon clay softened evenly, and the plasticity was good, so the next test could be carried out.
[0043] In summary, the suitable baking temperature range for anhydrous cannon clay before molding is 60-80℃, and the suitable baking time when the cannon clay is broken into small pieces of 20-30mm is about 20min.
[0044] The invention discloses a method for preparing a sample of anhydrous taphole clay for a blast furnace. In use, the invention studies the method for preparing a sample of anhydrous taphole clay for a blast furnace. Before the sample of anhydrous taphole clay for a blast furnace is prepared, baking is performed, and the suitable baking temperature is 60-80 DEG C. For convenient operation, the anhydrous taphole clay should be broken into small pieces of 20-30 mm, and the baking time is about 20 minutes. When the sample of anhydrous taphole clay for a blast furnace is prepared, the optimal molding pressure is 35 kN (5.47 MPa)-45 kN (7.03 MPa). The sample of anhydrous taphole clay for a blast furnace needs to be carbonized before high-temperature performance testing is performed, the optimal carbonization treatment temperature is 500 DEG C, the heat preservation time is 5 hours, and the atmosphere is carbon buried or other reducing atmospheres. The invention has the advantages of simple operation, determination of suitable temperature and pressure, and good sample preparation effect.
[0045] Example 2
[0046] like Figure 1-5 As shown, a method for preparing anhydrous taphole mud sample for blast furnace comprises the following steps:
[0047] Step 1: Preparation before sample preparation: Chisel the anhydrous taphole mud to be tested into small pieces of 25 mm, evenly take a certain amount of the small pieces and put them into the electric drying oven for baking. The baking temperature is between 70 ° C, the heating rate is 5 ° C / min, and the baking time is 20 min;
[0048] Step 2: Sample preparation: Weigh an appropriate amount of small pieces of taphole clay baked in the above steps, quickly and evenly put them into the mold, and press them into shape under a pressure of 40KN on a molding press;
[0049] Step 3: After demoulding, move the sample to a rigid flat plate, keep the molding surface facing up, and measure the size of the sample with a vernier caliper. The size should meet the requirements, otherwise redo it;
[0050] Step 4: Carbonization treatment: Place the qualified sample in a sagger and perform carbonization treatment in a carbonization treatment furnace under the condition of burying carbon (graphite powder). The carbonization treatment temperature is 500℃, the treatment time is 5h, and the heating rate is 4℃ / min. When burying graphite powder, the graphite thickness is 50mm more than the sample, which has sufficient thickness to ensure that the sample is not oxidized, and at the same time, the graphite powder must be densely covered.
[0051] Step 5: Record: including: sample name, brand, batch number, production date, sampling, sample preparation date and tester information.
[0052] The sample size standard in step 3 is: length 160±2.00mm, width 40±2.00mm, height 40±2.00mm.
[0053] The minimum scale of the vernier caliper in step 3 is 0.02 mm.
[0054] The carbonization treatment in step 4 is for soft taphole clay that is easily deformed after molding. In order to prevent deformation after molding, it should be fixed with a mold of corresponding size, and then carbonization treatment is carried out.
[0055] The carbonization furnace in step 4 is an electric furnace with a temperature control device and a smoke exhaust device.
[0056] In this embodiment, the determination of the molding pressure of anhydrous cannon clay sample preparation: ① Test process: First, the crushed 1#-5# cannon clay sample pieces (20-30mm) are baked according to the above baking system, and then 160mm×40mm×40mm strip samples are made under 15kN (2.34MPa), 25kN (3.91MPa), 35kN (5.47MPa), 45kN (7.03MPa), and 50kN (7.81MPa) pressures, respectively. After demoulding, the size and mass of each sample are measured, and its apparent bulk density is calculated;
[0057] ②Test results and analysis: From Table 2 and Figure 1 It can be seen that when the molding pressure is less than 35 kN, the volume density of the five samples increases with the increase of molding pressure; when the molding pressure is greater than 45 kN, the volume density of the sample tends to decrease with the increase of molding pressure; for example, for sample 3#, when the molding pressure is 45 kN (7.03 MPa), the volume density of the sample reaches a maximum value of 2.57 g / cm 3 However, when the molding pressure increased to 50 kN (7.81 MPa), the volume density of the sample decreased to 2.54 g / cm 3 The reason is that when the molding pressure is greater than 45kN, the sample rebounds after demolding, the volume increases, and the volume density decreases. Therefore, the higher the molding pressure is, the better it is. At the same time, the samples with a molding pressure less than 35kN have more surface cracks and layer cracks than other samples, and the density of the samples is not high, which affects the later performance testing of the samples. Therefore, the appropriate range of molding pressure for anhydrous cannon clay sampling is between 35kN (5.47MPa) and 45kN (7.03MPa).
[0058] Table 2 Bulk density of samples formed at different pressures g / cm 3
[0059]
[0060] The invention discloses a method for preparing a sample of anhydrous taphole clay for a blast furnace. In use, the invention studies the method for preparing a sample of anhydrous taphole clay for a blast furnace. Before the sample of anhydrous taphole clay for a blast furnace is prepared, baking is performed, and the suitable baking temperature is 60-80 DEG C. For convenient operation, the anhydrous taphole clay should be broken into small pieces of 20-30 mm, and the baking time is about 20 minutes. When the sample of anhydrous taphole clay for a blast furnace is prepared, the optimal molding pressure is 35 kN (5.47 MPa)-45 kN (7.03 MPa). The sample of anhydrous taphole clay for a blast furnace needs to be carbonized before high-temperature performance testing is performed, the optimal carbonization treatment temperature is 500 DEG C, the heat preservation time is 5 hours, and the atmosphere is carbon buried or other reducing atmospheres. The invention has the advantages of simple operation, determination of suitable temperature and pressure, and good sample preparation effect.
[0061] Example 3
[0062] like Figure 1-5 As shown, a method for preparing anhydrous taphole mud sample for blast furnace comprises the following steps:
[0063] Step 1: Preparation before sample preparation: Chisel the anhydrous taphole mud to be tested into small pieces of 20 mm, evenly take a certain amount of the small pieces and put them into the electric drying oven for baking. The baking temperature is between 80 ° C, the heating rate is 5 ° C / min, and the baking time is 20 min;
[0064] Step 2: Sample preparation: Weigh an appropriate amount of small pieces of taphole clay baked in the above steps, quickly and evenly put them into the mold, and press them into shape under a pressure of 45KN on a molding press;
[0065] Step 3: After demoulding, move the sample to a rigid flat plate, keep the molding surface facing up, and measure the size of the sample with a vernier caliper. The size should meet the requirements, otherwise redo it;
[0066] Step 4: Carbonization treatment: Place the qualified sample in a sagger and perform carbonization treatment in a carbonization treatment furnace under the condition of burying carbon (graphite powder). The carbonization treatment temperature is 500℃, the treatment time is 5h, and the heating rate is 5℃ / min. When burying graphite powder, the graphite thickness is 50mm more than the sample, which has enough thickness to ensure that the sample is not oxidized, and at the same time, the graphite powder must be densely covered.
[0067] Step 5: Record: including: sample name, brand, batch number, production date, sampling, sample preparation date and tester information.
[0068] The sample size standard in step 3 is: length 160±2.00mm, width 40±2.00mm, height 40±2.00mm.
[0069] The minimum scale of the vernier caliper in step 3 is 0.02 mm.
[0070] The carbonization treatment in step 4 is for soft taphole clay that is easily deformed after molding. In order to prevent deformation after molding, it should be fixed with a mold of corresponding size, and then carbonization treatment is carried out.
[0071] The carbonization furnace in step 4 is an electric furnace with a temperature control device and a smoke exhaust device.
[0072] In this embodiment, the temperature, time and atmosphere of the carbonization treatment of anhydrous taphole mud are determined: organic binders such as tar, asphalt, anthracene oil, resin and other components in anhydrous taphole mud will undergo carbonization reaction within a certain temperature range, volatilizing harmful substances such as phenol, formaldehyde, xylenol, etc., and organic aromatic compounds will partially decompose at about 400°C when heated under normal pressure to form low-molecular compounds that escape from the carbonization system; in order to prevent the laboratory from being polluted by toxic gases and causing personal harm, and also for the anhydrous taphole mud to obtain a certain early strength, the sample should be carbonized before testing various high-temperature physical and chemical performance indicators;
[0073] ① Determination of carbonization temperature: 1) Experimental process: 1#-5# anhydrous cannon clay is made into 5 strips of 160mm×40mm×40mm as required, and one strip is taken for heat treatment in the modified electric furnace. The temperatures are 200℃, 300℃, 400℃, 500℃ and 600℃ respectively, and the heating rate is 5℃ / min; since the cannon clay contains easily oxidized substances such as carbon, in order to prevent carbon from being oxidized during heat treatment, the sample should be placed in a sagger in a carbon-buried (graphite) atmosphere; heat treatment is carried out until the sample does not smoke, and then the mass loss rate, room temperature flexural strength, bulk density and apparent porosity of the sample are measured;
[0074] 2) Test results and analysis: 2.1) Mass loss rate: Record the mass of the sample before and after heat treatment at different temperatures, and calculate the mass loss according to the following formula: η = m 后 -m 前 ×100%; Figure 2 Based on laboratory data
[0075] m 前
[0076] The figure shows the variation of the mass loss rate of each anhydrous cannon mud sample at different heat treatment temperatures. As shown in the figure, when the heat treatment temperature rises from 200℃ to 500℃, the mass loss rate of 1#-5# cannon mud all shows a significant upward trend, especially in the temperature range of 300-400℃, the mass loss rate increases the most, while at 500-600℃, the mass loss rate growth rate slows down or tends to be stable; when the heat treatment temperature is 200℃, the mass loss rate of each sample is 1%-1.5%, accounting for about 10% of the total volatile matter; when the heat treatment temperature is 300 ℃, the mass loss rate is 2.5%-3.5%, accounting for about 30% of the total volatiles; when the treatment temperature is 400℃, the mass loss increases sharply to 6.5%-8.5%, accounting for about 80% of the total volatiles; when the temperature continues to rise to 500℃, the mass loss rate is 8.3%-10%, accounting for more than 95% of the total volatiles; when the treatment temperature reaches 600℃, the mass loss rate does not change significantly compared with the data at 500℃; it can be seen that after the anhydrous cannon mud is heat treated at 500℃, the mass loss rate tends to be stable and the volatiles are basically consumed.
[0077] 2.2) Room temperature flexural strength: The room temperature flexural strength change trend of each sample after heat treatment at different temperatures is as follows Figure 3 As shown in the figure, after the samples were heat treated at 200℃ and 300℃, when the room temperature flexural strength test was carried out, the samples were not directly destroyed by the force, but first underwent obvious plastic deformation, indicating that no sufficient curing reaction occurred during the heat treatment; when the heat treatment temperature was 300-400℃, the room temperature flexural strength of each sample increased rapidly, which was due to the violent curing reaction inside the anhydrous taphole mud, which was consistent with the Figure 2 The reasons for the substantial increase in mass loss rate when the heat treatment temperature increases from 300°C to 400°C are consistent; when the temperature is 400-500°C, the room temperature flexural strength of each sample increases slowly or does not change significantly; when the heat treatment temperature is 500-600°C, the room temperature flexural strength of the sample decreases slightly or does not change significantly, which is due to the fact that the curing reaction is basically completed and the apparent porosity increases slightly (such as Figure 5 shown);
[0078] 2.3) Bulk density and apparent porosity: The changes in bulk density and apparent porosity of anhydrous taphole mud samples at different heat treatment temperatures are as follows: Figure 4 , Figure 5 As shown in the figure; when the heat treatment temperature is 200-400℃, the carbon binder in the anhydrous taphole mud undergoes more and more intense decomposition, bridging, dehydrogenation and polycondensation reactions, and the volatile matter discharge rate gradually accelerates, resulting in a decrease in the volume density of each sample and a rapid increase in the apparent porosity; when the heat treatment temperature is 500-600℃, the volatile matter is discharged slowly, the apparent porosity of the sample increases slightly, and the volume density decreases slightly;
[0079] From the above analysis, it can be seen that after the anhydrous cannon mud is treated at 500℃, the volatiles are basically discharged, and sufficient curing strength is also obtained; at the same time, the samples after heat treatment at different temperatures are treated again at high temperature in a carbon-buried atmosphere. It is found that the samples after carbonization treatment at 200℃ and 300℃ begin to emit thick smoke at about 400℃, and the samples after carbonization treatment at 400℃ emit a small amount of smoke. Only when the carbonization treatment temperature is ≥500℃, the sample will not smoke when subjected to high temperature treatment again; therefore, the optimal carbonization treatment temperature for anhydrous cannon mud is 500℃.
[0080] ② Determination of carbonization treatment time and atmosphere: After obtaining the optimal carbonization treatment temperature, the following test was carried out to determine the optimal carbonization treatment time: 1#-5# anhydrous cannon mud was made into 160mm×40mm×40mm long strip samples according to the above requirements, and placed in carbon buried kilns respectively, and carbonized at 500℃ with a heating rate of 5℃ / min. The smoke situation was recorded every 30 minutes, and the test was terminated when there was no smoke. The test results are listed in Table 3.
[0081] Table 3 Smoking of each anhydrous taphole mud sample during heat treatment at 500℃
[0082]
[0083] It can be seen from Table 3 that samples 1# and 4# stopped emitting smoke after being kept at 500℃ for 4.5h, and the test was ended; samples 2#, 3# and 5# began to emit thin smoke after being kept at 4-4.5h, and stopped emitting smoke after being kept at 5h; therefore, the optimal holding time for carbonization treatment should be 5h.
[0084] The above sample preparation method was used to make 1#-5# anhydrous cannon clay into 160mm×40mm×40mm long strip samples, which were directly heat treated at 500℃ for 5h in air atmosphere. After the test, it was found that decarburization reaction occurred in each sample to varying degrees, and the surface particles were loose, making high-temperature detection no longer possible. Therefore, the carbonization treatment of anhydrous cannon clay must be carried out under carbon burial or other reducing atmospheres.
[0085] The invention discloses a method for preparing anhydrous taphole clay samples for blast furnaces. Before the preparation of the anhydrous taphole clay samples for blast furnaces, baking should be carried out, and the suitable baking temperature is 60-80 DEG C. For the convenience of operation, the anhydrous taphole clay should be broken into small pieces of 20-30 mm, and the baking time is about 20 minutes. When the anhydrous taphole clay samples for blast furnaces are prepared, the optimal molding pressure is 35 kN (5.47 MPa)-45 kN (7.03 MPa). The anhydrous taphole clay samples for blast furnaces need to be carbonized before high-temperature performance testing, and the optimal carbonization treatment temperature is 500 DEG C. The heat preservation time is 5 hours, and the atmosphere is carbon buried or other reducing atmospheres. The invention has the advantages of simple operation, determination of suitable temperature and pressure, and good sample preparation effect.
Claims
1. A method for preparing anhydrous taphole mud samples for blast furnaces, characterized in that: The preparation method comprises the following steps: Step 1: Sample preparation: Chisel the anhydrous taphole mud to be tested into small pieces, evenly take a certain amount of the small pieces and put them into an electric drying oven for baking; Step 2: Sample preparation: Weigh an appropriate amount of small pieces of taphole clay baked in the above steps, quickly and evenly put them into the mold, and press them into shape under the pressure of the molding press; Step 3: After demoulding, move the sample to a rigid flat plate, keep the molding surface facing up, and measure the size of the sample with a vernier caliper. The size should meet the requirements, otherwise redo it; Step 4: Carbonization treatment: Place the qualified sample in a sagger and perform carbonization treatment in a carbonization furnace under the condition of burying carbon (graphite powder); Step 5: Record: including: sample name, brand, batch number, production date, sampling, sample preparation date and tester information.
2. The method for preparing anhydrous taphole clay sample for blast furnace according to claim 1, characterized in that: In the step 1, the anhydrous taphole mud to be tested is broken into small pieces of 30-20 mm.
3. The method for preparing anhydrous taphole clay sample for blast furnace according to claim 2, characterized in that: In step 1, the baking temperature of the electric drying oven is between 60-80° C., the heating rate is 5° C. / min, and the baking time is 20 min.
4. The method for preparing anhydrous taphole clay sample for blast furnace according to claim 1, characterized in that: The pressure range of the molding press in step 2 is 35KN-45KN.
5. The method for preparing anhydrous taphole clay sample for blast furnace according to claim 1, characterized in that: The sample size standard in step 3 is: length 160±2.00mm, width 40±2.00mm, height 40±2.00mm.
6. The method for preparing anhydrous taphole clay sample for blast furnace according to claim 5, characterized in that: The minimum scale of the vernier caliper in step 3 is 0.02 mm.
7. The method for preparing anhydrous taphole clay sample for blast furnace according to claim 1, characterized in that: The carbonization treatment temperature in step 4 is 500° C., the treatment time is 5 h, and the heating rate is 3-5° C. / min.
8. The method for preparing anhydrous taphole clay sample for blast furnace according to claim 7, characterized in that: When the graphite powder is buried in the carbonization treatment in step 4, the thickness of the graphite is 45-50 mm more than the sample to ensure that the sample is not oxidized and at the same time ensure that the graphite powder covers densely.
9. The method for preparing anhydrous taphole clay sample for blast furnace according to claim 8, characterized in that: The carbonization treatment in step 4 is for soft taphole clay that is easily deformed after molding. In order to prevent deformation after molding, it should be fixed with a mold of corresponding size, and then carbonization treatment is carried out.
10. The method for preparing anhydrous taphole clay sample for blast furnace according to claim 9, characterized in that: The carbonization furnace in step 4 is an electric furnace with a temperature control device and a smoke exhaust device.