Titanium alloy material crack opening force testing method based on DIC

Through the image processing method based on DIC technology, the opening-closing effect of fatigue cracks in titanium alloy materials is extracted and analyzed, and the problem of difficulty in measuring the opening force of fatigue cracks is solved, achieving high-precision real-time monitoring and expanding the scope of application.

CN119000669AInactive Publication Date: 2024-11-22ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411063481.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The classical flexibility method is difficult to accurately measure the expansion displacement of the fatigue crack surface of titanium alloy materials under constant combined fatigue loads with high and low circumference, and it is impossible to realize real-time monitoring of the fatigue crack expansion force of titanium alloy materials.

Method used

Using the fatigue crack opening force test method of titanium alloy materials based on digital image correlation (DIC) technology, the crack surface expansion displacement field affected by the crack opening-closing effect is extracted by collecting and processing digital image sequences, combining load-unloading feature extraction and mean Normalized calculations determine the crack opening force under high and low cycle random loads.

Benefits of technology

Real-time monitoring of fatigue crack opening force of high-precision titanium alloy materials, expand the applicable working range of crack opening force measurement by classical flexibility method, can quantitatively measure the change in the opening displacement of the fatigue crack surface, and make up for the flexibility method insufficient.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119000669A_ABST
    Figure CN119000669A_ABST
Patent Text Reader

Abstract

The invention relates to a method for testing fatigue crack opening force of a titanium alloy material based on DIC. The method comprises the following steps: acquiring a plurality of groups of digital image sequences for recording the change process of a fatigue crack propagation form of the titanium alloy material; carrying out mean value-based normalization calculation on the digital image sequence to obtain a crack propagation displacement field containing a closure effect influence; carrying out loading-unloading feature extraction on the crack propagation displacement field, and reducing the opening-closing propagation process of the fatigue crack surface of the titanium alloy material; data cleaning and feature processing are carried out on the crack surface in the opening-closing expansion process, and the method for determining the crack opening force under the high-low-cycle constant-amplitude load is innovatively provided. The problem that the high-precision fatigue crack opening force of the titanium alloy material is difficult to monitor in real time by using a flexibility method for measuring the crack opening force is solved, the variable quantity of the opening displacement of the fatigue crack surface of the titanium alloy material can be quantitatively measured, the high-precision real-time monitoring of the fatigue crack opening force of the titanium alloy material is realized, and the applicable working condition range is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an image processing and titanium alloy material fatigue crack measurement technology, and in particular to a titanium alloy material fatigue crack propagation opening force measurement method based on digital image correlation (DIC), which can be widely used in the fields involving fatigue crack propagation measurement of titanium alloy materials such as welding titanium alloy panels and titanium alloy components. Background Art

[0002] Titanium alloy, as a lightweight material with excellent mechanical properties, has been widely used in aerospace, shipbuilding, automotive industry and medical equipment. In actual use, these structures will be subjected to many cyclic loads, so it is crucial to understand the fatigue crack growth behavior in the welded area. Measuring the crack growth opening force can help evaluate the fatigue life of welded joints and ensure the safety and reliability of aircraft structures. The fatigue design method currently widely used is an evaluation method based on crack growth theory. Closure will occur during fatigue crack growth. The crack will only grow when the load reaches the crack opening force Fop. Therefore, the influence of crack closure needs to be considered to accurately estimate the fatigue residual life. In crack closure analysis, the determination of Fop is related to the judgment of the influence of crack closure on growth, so the study of Fop determination method is very important.

[0003] The classic compliance method for measuring crack opening force cannot quantitatively measure the change in the opening displacement of the fatigue crack surface of titanium alloy materials under high and low cycle constant combined fatigue loads, and cannot solve the problem of high-precision real-time monitoring of fatigue crack opening force of titanium alloy materials. Summary of the invention

[0004] In view of the fact that the compliance method for measuring crack opening force is difficult to solve the problem of high-precision real-time monitoring of fatigue crack opening force of titanium alloy materials, a fatigue crack opening force testing method of titanium alloy materials based on DIC is proposed. This method has clear principle, stable performance, good scalability, and can accurately determine the crack opening force under high and low cycle random loads.

[0005] The technical solution of the present invention is:

[0006] A method for testing the fatigue crack opening force of a titanium alloy material based on DIC, comprising the following steps: collecting multiple sets of digital image sequences recording the morphological change process of fatigue crack extension of the titanium alloy material; performing mean normalization calculation on the digital image sequence to measure the crack surface extension displacement field including the crack opening-closing effect; performing loading-unloading feature extraction on the crack extension displacement field, cleaning and feature transformation of the displacement field data during the crack opening-closing extension process, and using a method for determining the crack opening force under high and low cycle random loads;

[0007] Image acquisition captures the fatigue crack propagation process of titanium alloy materials and fully captures the dynamic changes of cracks; then enters the data processing process: first, select the quadrilateral speckle region QSR at the crack tip in the image, build a grid based on two deformation markers in the region, and generate a target data array to ensure that it is located near the crack tip; then, by contrast mapping each array number, find and record the numbers of adjacent points, and the adjacent points missing from the crack tip are recorded as negative numbers; DIC technology is used for point-to-point strain measurement to obtain the displacement field of each frame of the image, and its arrangement is consistent with the target data array; in the loading-unloading process and crack opening force analysis, data cleaning and feature transformation are first performed to calculate the correlation coefficient R of each point 12 , and set a threshold a to distinguish hysteresis points from non-hysteresis points, so as to define the obvious degree of crack opening force; if the opening force is obvious, the mean normalization method is used to process the displacement field, identify the crack boundary, obtain the displacement data in the opening-closing process, and map it to the loading-unloading process; if the opening force is not obvious, the unloading process feature extraction algorithm can be selected for analysis; finally, the crack extension displacement field of each frame image is summarized to form a complete fatigue crack opening-closing extension process in the time domain;

[0008] The digital image sequence is processed to obtain the crack propagation displacement field including the crack surface opening-closing effect, including:

[0009] S101, generating a target data array in a digital image;

[0010] A quadrilateral speckle region QSR containing a fatigue crack tip is determined in the digital image; two deformation structural landmarks of the QSR are found, and a patch mesh of the quadrilateral speckle region QSR is constructed based on the distance between the two deformation structural landmarks; in the patch mesh, a target data array is generated based on the accuracy and residual;

[0011] The process of generating the target data array is as follows: starting from a point near the crack tip of the patch mesh, generating the target data array in the order from left to right and from top to bottom according to the pixel spacing;

[0012] In the process of the target data array, the maximum principal strain method is used to determine whether the target data array is near the QSR crack tip in the target area. If so, the target data array is used, otherwise, the target data array is discarded;

[0013] S102, the target data array generates a crack surface extension displacement field;

[0014] According to the order in which the target data arrays are generated, starting from label 1, a seed label is assigned to each target data array in an accumulative manner; for each target data array, four adjacent target points with a distance of one pixel in the four directions of up, down, left and right are found in turn by using the comparison mapping and scanning method, and the labels of the four adjacent target data arrays are recorded; for the target data array at the crack tip, if the adjacent target data array is missing in a certain direction, the missing array label is recorded as a negative number;

[0015] S103, using DIC on the target point of the target data array to measure the displacement field of the fatigue crack of the titanium alloy, and obtaining the fatigue crack propagation displacement field including the influence of the opening-closing effect;

[0016] Point-to-point strain measurement is performed on each target array to obtain the deformation time domain curve of each target array in the time domain; the displacement field in each time node, i.e., each frame image, is obtained in the spatial domain. The arrangement of the displacement field in the spatial domain is derived from the target data array, and the displacement field has the same mapping rule as the target data array.

[0017] The crack extension loading-unloading process feature extraction algorithm is used for the crack extension displacement field to obtain the fatigue crack opening force of the titanium alloy material, which specifically includes the following steps:

[0018] S201, obtain the correlation R by data cleaning and feature transformation cross-correlation calculation 12 , defining fatigue crack opening force into obvious and inconspicuous categories;

[0019] Run the DIC algorithm for each target array in the target data array and calculate its correlation coefficient. The correlation calculation formula is:

[0020]

[0021] Where f(x,y) and g(x',y') are the reference image subset and matching image subset for cross-correlation operation, respectively. m =∑f(x,y) / M,g m =∑g(x',y') / M, M is the number of images in the reference image subset and the matching image subset;

[0022] Set the threshold a and set R 12 The target point greater than a is set as the non-hysteresis point, and R 12 The target point less than a is set as the hysteresis point; if there is a target point passing through R 12 If the target data array is judged as a hysteresis point by the threshold, it is considered that the target data array has obvious opening force, otherwise it is considered that the opening force is not obvious;

[0023] S202, if it is defined as obvious, use a loading process feature extraction algorithm to extract a fatigue crack growth process with obvious opening force;

[0024] A mean normalization-based calculation method is used to process the crack extension displacement field with opening-closing effect to obtain the crack extension strain field; the crack extension strain field is scanned and detected to obtain the peak stress area, and the target data array located at the boundary of the fatigue crack extension area is identified; after the target points at the boundary are sorted and combined according to the horizontal coordinates, two line segments composed of discrete points are obtained, each corresponding to the upper boundary and the lower boundary of the fatigue crack extension boundary, that is, the displacement data array in the crack opening-closing process is obtained; the displacement data array is mapped to the loading-unloading process;

[0025] S203, if it is defined as not obvious, using an unloading process feature extraction algorithm to extract a fatigue crack growth process with not obvious opening force;

[0026] S204, combining the crack extension displacement field changes obtained from each frame of the image to obtain the fatigue crack opening-closing extension change process including the opening force in the time city.

[0027] Preferably, the array image sequence is captured by an industrial camera at a certain acquisition frame rate of not less than 30fps, and the number of digital images included is not less than 240, so as to fully capture the dynamic changes of the cracks.

[0028] Preferably, the specific implementation steps include:

[0029] Based on the image processing algorithm, the target image in the image sequence generates a target data array, and DIC is used to measure the displacement of each target point in the target array, thereby obtaining the fatigue crack growth displacement field measurement results including the opening-closing effect.

[0030] Post-process the DIC crack displacement field to establish the obvious and unclear boundaries of fatigue crack opening force;

[0031] Firstly, based on the ZNCC birth-death boundary detection results after one cycle, the region with obvious opening force is determined, and the birth-death boundary of fine cracks is established by the peak region of strain field. After the birth-death boundary is established, the feature extraction of fatigue crack loading-unloading stage can be carried out.

[0032] The discrete boundaries are interpolated to obtain a discrete double chain with good agreement with the actual fatigue crack. The specific implementation process is as follows: read the target point i, find the 5 points adjacent to point i, perform curve fitting based on the interpolation of the adjacent points, calculate the displacement field of the unloading process, and interpolate the target point along the normal direction until all the target points are interpolated.

[0033] Fit the crack target data array to obtain the fatigue crack analytical solution, i.e., the fatigue crack opening-closing displacement field;

[0034] The fatigue crack static measurement results of all single-frame digital images in the image sequence are integrated to form the fatigue crack dynamic extension measurement results in the time domain.

[0035] The beneficial effects of the present invention are:

[0036] (1) The present invention adopts an image processing method and innovatively proposes a method for determining the crack opening force under high and low cyclic constant amplitude loads.

[0037] (2) Compared with the classical flexibility method for measuring crack opening force, the present invention can quantitatively measure the change in the opening displacement of the fatigue crack surface of the titanium alloy material, realize high-precision real-time monitoring of the fatigue crack opening force of the titanium alloy material, and expand the applicable working conditions of the classical flexibility method for measuring crack opening force.

[0038] (3) The present invention can be widely used in titanium alloy fatigue tests, making up for the many shortcomings of the compliance method, realizing high-precision real-time monitoring of fatigue crack opening force of titanium alloy materials, and expanding the applicable working conditions of the classic compliance method for measuring crack opening force. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The flowchart of the method for testing the crack opening force of titanium alloy material based on DIC of the present invention;

[0040] Figure 2 This is a diagram of actual fatigue crack extraction results of the present invention. DETAILED DESCRIPTION

[0041] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0042] The present invention provides an embodiment, a method for testing the fatigue crack opening force of a titanium alloy material based on DIC, comprising: collecting 5 groups of digital image sequences that record the morphological change process of fatigue crack expansion of the titanium alloy material; performing a mean normalization calculation method on the digital image sequence to measure the crack surface expansion displacement field including the influence of the crack opening-closing effect; performing loading-unloading feature extraction on the crack expansion displacement field, cleaning and feature transformation of the displacement field data during the crack opening-closing expansion process, and innovatively proposing a method for determining the crack opening force under high and low cycle random loads.

[0043] The array image sequence is captured by an industrial camera at a certain acquisition frame rate (not less than 30fps), and the number of digital images included is not less than 240.

[0044] The image processing algorithm is used to process the digital image sequence that records the change process of fatigue crack propagation morphology of titanium alloy materials. The image processing algorithm can generate a target data array in the digital image, and use DIC (Digital Image Correlation) on the target points of the target data array to measure the displacement field of the fatigue crack of the titanium alloy, and obtain the fatigue crack propagation displacement field including the opening-closing effect. DIC is a relatively mature optical measurement mechanics technology, which obtains the deformation process of the object surface based on the random texture test of the object surface in the digital image.

[0045] In order to better restore the dynamic crack expansion process, the present invention provides a preferred embodiment. Figure 1 , is a method for testing crack opening force of titanium alloy material based on DIC according to an embodiment, comprising the following steps;

[0046] S100, reading a digital image sequence;

[0047] S200, generating the crack surface extension displacement field;

[0048] S300, loading-unloading feature extraction algorithm;

[0049] S400, generating a target data array with obvious hysteresis effect;

[0050] S500, generating a single-frame image of the fatigue crack static morphology to determine whether the image sequence has been read. If not, execute S100-S400; if yes, enter S600;

[0051] S600, calculate fatigue crack opening force.

[0052] Executing S200 causes the image processing algorithm to generate a target data array.

[0053] Specifically, a quadrilateral speckle region QSR containing the fatigue crack tip is determined in the digital image; two deformation structural landmarks of QSR are found, and the patch mesh of the quadrilateral speckle region QSR is constructed based on the distance between the two deformation structural landmarks, and the target data array is generated based on the accuracy and residual.

[0054] Based on the generated target data array, the present invention provides a preferred embodiment to execute S300 and S400, perform point-to-point strain measurement on each target data array, and obtain a deformation time domain curve of each target data array in the time domain; obtain a displacement field in each time node, i.e., each frame image in the spatial domain, having the same mapping rule as the target data array.

[0055] Specifically, the crack extension loading-unloading process feature extraction algorithm is used to obtain the fatigue crack opening force of titanium alloy materials, including the following processes;

[0056] The correlation is calculated by data cleaning and feature extraction, and the characteristic relationship between the opening force and the crack surface opening displacement is defined. The DIC algorithm is run on each target array in the target data array to calculate its correlation coefficient. The correlation calculation formula is:

[0057]

[0058] Set the threshold a and set R 12 The target point greater than a is set as the non-hysteresis point, and R 12 The target point less than a is set as the hysteresis point; if there is a target point passing through R 12 If it is judged as a hysteresis point, it is considered that the target data array has obvious opening force, otherwise it is considered that the opening force is not obvious.

[0059] S500 and S600 are executed, that is, the image processing algorithm and the crack extension loading-unloading process feature extraction algorithm are run on each frame image in the digital image sequence to obtain the fatigue crack opening force result in the time domain.

[0060] This embodiment can be widely used in laboratories and actual projects to meet the full coverage, refinement and intelligent measurement requirements of titanium alloy fatigue crack measurement, and further provide important protection for the safety of titanium alloy infrastructure.

[0061] In order to verify the feasibility of each embodiment of the DIC-based titanium alloy material fatigue crack opening force test method and the corresponding detection effect, the present invention provides a preferred specific embodiment. This specific embodiment provides the fatigue crack morphology measurement results of the test piece in the laboratory.

[0062] This specific embodiment includes the following works:

[0063] (1) Based on the image processing algorithm, the target image in the image sequence generates a target data array, and DIC is used to measure the displacement of each target point in the target array, thereby obtaining the fatigue crack propagation displacement field measurement results including the opening-closing effect.

[0064] (2) Post-process the DIC crack displacement field to establish the obvious and unclear boundaries of fatigue crack opening force.

[0065] First, based on the ZNCC birth-death boundary detection results after one cycle, the region with obvious opening force is determined, and the birth-death boundary of fine cracks is established by the strain field peak area. After the birth-death boundary is established, the fatigue crack loading-unloading stage feature extraction can be performed.

[0066] (3) The discrete boundaries are interpolated to obtain a discrete double chain that is consistent with the actual fatigue crack. Figure 2 As shown, specifically: read the target point i, find the 5 points adjacent to point i, perform curve fitting based on interpolation of adjacent points to calculate the displacement field of the unloading process, and push the target point inward along the normal until all target points are pushed inward.

[0067] (4) Fit the crack target data array to obtain the fatigue crack analytical solution, that is, the fatigue crack opening-closing displacement field.

[0068] (5) Integrate the static measurement results of fatigue cracks of all single-frame digital images in the image sequence to form the dynamic expansion measurement results of fatigue cracks in the time domain.

[0069] Figure 2 The dynamic expansion result of the fatigue crack morphology of the specimen measured by the present invention. It can be seen that as the crack continues to expand, the present invention can quantitatively measure the change in the opening displacement of the fatigue crack surface of the titanium alloy material, realize high-precision real-time monitoring of the fatigue crack opening force of the titanium alloy material, and expand the applicable working range of the classic compliance method for measuring the crack opening force.

[0070] The present invention does not make specific requirements on the digital images and the two digital image acquisition devices. Any images and acquisition devices that can be applied to the DIC technology can be applied to this algorithm.

[0071] The above-mentioned embodiment only expresses one implementation mode of the present invention, and its description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.

Claims

1. A method for testing fatigue crack opening force of titanium alloy material based on DIC, characterized in that: The following steps are involved: Collect multiple sets of digital image sequences that record the morphological changes of fatigue crack propagation in titanium alloy materials; perform mean normalization calculations on the digital image sequences to measure the crack surface propagation displacement field including the crack opening-closing effect; perform loading-unloading feature extraction on the crack propagation displacement field, perform data cleaning and feature transformation on the crack opening-closing propagation process displacement field, and use a method to determine the crack opening force under high and low cycle random loads; Image acquisition captures the fatigue crack propagation process of titanium alloy materials and fully captures the dynamic changes of cracks; then enters the data processing process: first, select the quadrilateral speckle region QSR at the crack tip in the image, build a grid based on the two deformation marker points in the region, and generate a target data array to ensure that it is located near the crack tip; then, by comparing and mapping each array number, find and record the numbers of adjacent points, and the adjacent points missing from the crack tip are recorded as negative numbers; DIC technology is used to perform point-to-point strain measurement to obtain the displacement field of each frame of the image, and its arrangement is consistent with the target data array; In the analysis of the loading-unloading process and crack opening force, data cleaning and feature transformation are first performed to calculate the correlation coefficient R of each point. 12 , and set a threshold a to distinguish hysteresis points from non-hysteresis points, thereby defining the degree of crack opening force; If the opening force is obvious, the mean normalization method is used to process the displacement field, identify the crack boundary, obtain the displacement data in the opening-closing process, and map it to the loading-unloading process; if the opening force is not obvious, the unloading process feature extraction algorithm can be selected for analysis; finally, the crack extension displacement field of each frame image is summarized to form a complete fatigue crack opening-closing extension process in the time domain; The digital image sequence is processed to obtain the crack propagation displacement field including the crack surface opening-closing effect, including: S101, generating a target data array in a digital image; A quadrilateral speckle region QSR containing a fatigue crack tip is determined in the digital image; two deformation structural landmarks of the QSR are found, and a patch mesh of the quadrilateral speckle region QSR is constructed based on the distance between the two deformation structural landmarks; in the patch mesh, a target data array is generated based on the accuracy and residual; The process of generating the target data array is as follows: starting from a point near the crack tip of the patch mesh, generating the target data array in the order from left to right and from top to bottom according to the pixel spacing; In the process of the target data array, the maximum principal strain method is used to determine whether the target data array is near the QSR crack tip in the target area. If so, the target data array is used, otherwise, the target data array is discarded; S102, the target data array generates a crack surface extension displacement field; According to the order in which the target data arrays are generated, starting from label 1, a seed label is assigned to each target data array in an accumulative manner; for each target data array, four adjacent target points with a distance of one pixel in the four directions of up, down, left and right are found in turn by using the comparison mapping and scanning method, and the labels of the four adjacent target data arrays are recorded; for the target data array at the crack tip, if the adjacent target data array is missing in a certain direction, the missing array label is recorded as a negative number; S103, using DIC on the target point of the target data array to measure the displacement field of the fatigue crack of the titanium alloy, and obtaining the fatigue crack propagation displacement field including the influence of the opening-closing effect; Point-to-point strain measurement is performed on each target array to obtain the deformation time domain curve of each target array in the time domain; the displacement field in each time node, i.e., each frame image, is obtained in the spatial domain. The arrangement of the displacement field in the spatial domain is derived from the target data array, and the displacement field has the same mapping rule as the target data array. The crack extension loading-unloading process feature extraction algorithm is used for the crack extension displacement field to obtain the fatigue crack opening force of the titanium alloy material, which specifically includes the following steps: S201, obtain the correlation R by data cleaning and feature transformation cross-correlation calculation 12 , defining fatigue crack opening force into obvious and inconspicuous categories; Run the DIC algorithm for each target array in the target data array and calculate its correlation coefficient. The correlation calculation formula is: Where f(x,y) and g(x',y') are the reference image subset and matching image subset for cross-correlation operation, respectively. m =∑f(x,y) / M,g m =∑g(x',y') / M, M is the number of images in the reference image subset and the matching image subset; Set the threshold a and set R 12 The target point greater than a is set as the non-hysteresis point, and R 12 The target point less than a is set as the hysteresis point; if there is a target point passing through R 12 If the target data array is judged as a hysteresis point by the threshold, it is considered that the target data array has obvious opening force, otherwise it is considered that the opening force is not obvious; S202, if it is defined as obvious, use a loading process feature extraction algorithm to extract a fatigue crack growth process with obvious opening force; A mean normalization-based calculation method is used to process the crack extension displacement field with opening-closing effect to obtain the crack extension strain field; the crack extension strain field is scanned and detected to obtain the peak stress area, and the target data array located at the boundary of the fatigue crack extension area is identified; after the target points at the boundary are sorted and combined according to the horizontal coordinates, two line segments composed of discrete points are obtained, each corresponding to the upper boundary and the lower boundary of the fatigue crack extension boundary, that is, the displacement data array in the crack opening-closing process is obtained; the displacement data array is mapped to the loading-unloading process; S203, if it is defined as not obvious, using an unloading process feature extraction algorithm to extract a fatigue crack growth process with not obvious opening force; S204, combining the crack extension displacement field changes obtained from each frame of the image to obtain the fatigue crack opening-closing extension change process including the opening force in the time city.

2. The method for testing fatigue crack opening force of titanium alloy material based on DIC according to claim 1, characterized in that: The array image sequence is captured by an industrial camera at a certain acquisition frame rate of not less than 30fps, and the number of digital images included is not less than 240 to fully capture the dynamic changes of the crack.

3. The method for testing fatigue crack opening force of titanium alloy material based on DIC according to claim 1, characterized in that: The specific implementation steps include: Based on the image processing algorithm, the target image in the image sequence generates a target data array, and DIC is used to measure the displacement of each target point in the target array, thereby obtaining the fatigue crack growth displacement field measurement results including the opening-closing effect. Post-process the DIC crack displacement field to establish the obvious and unclear boundaries of fatigue crack opening force; Firstly, based on the ZNCC birth-death boundary detection results after one cycle, the region with obvious opening force is determined, and the birth-death boundary of fine cracks is established by the peak region of strain field. After the birth-death boundary is established, the feature extraction of fatigue crack loading-unloading stage can be carried out. The discrete boundaries are interpolated to obtain a discrete double chain with good agreement with the actual fatigue crack. The specific implementation process is as follows: read the target point i, find the 5 points adjacent to point i, perform curve fitting based on the interpolation of the adjacent points, calculate the displacement field of the unloading process, and interpolate the target point along the normal direction until all the target points are interpolated. Fit the crack target data array to obtain the fatigue crack analytical solution, i.e., the fatigue crack opening-closing displacement field; The fatigue crack static measurement results of all single-frame digital images in the image sequence are integrated to form the fatigue crack dynamic extension measurement results in the time domain.

Citation Information

Cited By

  • Characterization method of fatigue crack growth rate without digital image processing

    CN121431252A