Silicon-doped carbon graphite negative electrode and active material selection method thereof, and lithium ion battery
By screening the volume distribution of silicon-carbon materials and graphite materials, ensuring the appropriate gap range, the problems of long periods and poor cycle performance in the prior art are solved, and the thickness expansion of silicon-doped graphite negative electrodes are reduced and the cycle performance improvement is improved.
Patent Information
- Application Number
- CN202411086742.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, verification, the evaluation of the mixed performance of graphite materials and silicon-carbon materials depends on the cycle test after the battery cell is made, resulting in a long evaluation cycle, and the rebound of the electrode sheet after the negative electrode is coated is too large, resulting in large expansion of the battery cell thickness and poor circulation performance. .
By screening the volume distribution of silicon-carbon materials and graphite materials, we ensure that the gap is suitable, the difference in the maximum volume density proportion is 0%≤b%-a%≤0.5%, and the maximum particle size difference is combined with the particle size distribution frequency. The value is 0um≤d-c≤5um, and the selected type is a silicon-doped carbon graphite negative electrode active material. The preliminary screening is conducted directly from the material level to evaluate the adaptability of graphite materials and silicon-carbon materials.
It effectively reduces the thickness expansion of the silicon-doped graphite negative electrode, shortens the evaluation cycle, reduces the cost, reduces the rebound of the electrode sheet after the negative electrode is coated, and improves the circulation performance.
Smart Images

Figure CN119001015A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion batteries, in particular to a silicon-carbon-doped graphite negative electrode and a method for selecting active materials thereof, and a lithium ion battery. Background Art
[0002] In lithium-ion battery systems, negative electrode materials have a decisive influence on energy density. Silicon negative electrode has a very high theoretical specific capacity (4200mAh / g) compared to the most widely used graphite negative electrode materials, and is considered to be a very promising next-generation high-energy-density lithium battery negative electrode material. However, due to its huge volume expansion (the volume change rate during lithium insertion / extraction process is as high as 280% to 400%), the large-scale application of silicon negative electrode is subject to certain restrictions.
[0003] In order to solve the above problems, the current solution is generally to mix the graphite negative electrode with some silicon-carbon materials. This can not only increase the specific capacity of the negative electrode, but also control the expansion within a reasonable range, avoiding significant deterioration of the cycle performance.
[0004] For hybrid negative electrode materials that add silicon-carbon materials to graphite materials, the main strategies for reducing cycle thickness expansion are: ① Optimizing the structure of silicon-carbon materials and their synthesis process; ② Optimizing the negative electrode formula, especially the type and proportion of binders; mainly using styrene-butadiene rubber SBR + polyacrylic acid PAA composite binder to increase the constraint on the volume change of silicon-carbon negative electrode particles after lithium is extracted and inserted. However, there are also many options for graphite materials with the same ratio, and the physical properties of graphite materials vary greatly, such as specific surface area, graphite material degree and particle size. At present, the verification of the mixed performance evaluation of graphite materials and silicon-carbon materials mainly relies on cycle testing and comparison after the battery cell is made, which leads to a long evaluation cycle. After the negative electrode is coated and rolled, the pole piece rebounds too much, resulting in a large expansion of the battery cell thickness and poor cycle performance. Summary of the invention
[0005] The embodiments of the present invention provide a silicon-carbon-doped graphite negative electrode and a method for selecting active materials thereof, and a lithium-ion battery, so as to solve the problem that in the prior art, the mixed performance evaluation of graphite materials and silicon-carbon materials mainly relies on cycle testing and comparison after the battery cells are made, resulting in a long evaluation cycle, and after the negative electrode is coated and rolled, the pole piece rebounds too much, resulting in a large expansion of the battery cell thickness and poor cycle performance.
[0006] The present invention discloses a method for selecting active materials for a silicon-doped carbon graphite negative electrode, comprising the steps of:
[0007] According to the cycle stability index and the thickness expansion index, the silicon-carbon material is screened, and the volume distribution of the silicon-carbon material is determined; wherein the volume distribution of the silicon-carbon material includes a% of the maximum volume density;
[0008] Screening graphite materials according to the rate cycle performance index and determining the volume distribution of the graphite materials; wherein the volume distribution of the graphite materials includes a maximum volume density accounting for b%;
[0009] If 0%≤b%-a%≤0.5%, it is determined that the silicon-carbon material and the graphite material are active materials of the silicon-carbon-doped graphite negative electrode.
[0010] Optionally, the volume distribution of the silicon-carbon material further includes a particle size with the highest frequency in the particle size distribution c μm, and the volume distribution of the graphite material further includes a particle size with the highest frequency in the particle size distribution d μm;
[0011] The active material selection method further comprises the steps of:
[0012] If 0%≤b%-a%≤0.5%, and 0um≤dc≤5um, it is determined that the silicon-carbon material and the graphite material are active materials of the silicon-carbon-doped graphite negative electrode.
[0013] Optionally, the step of screening the graphite material according to the rate cycle performance index and determining the volume distribution of the graphite material is specifically as follows:
[0014] Screen multiple graphite materials based on rate cycle performance indicators and determine the volume distribution of each graphite material;
[0015] If 0%≤b%-a%≤0.5%, the steps of determining that the silicon-carbon material and the graphite material are active materials of the silicon-carbon-doped graphite negative electrode are specifically:
[0016] The difference between b% of each graphite material and a% of the silicon-carbon material is calculated. If 0%≤b%-a%≤0.5%, the silicon-carbon material and the graphite material are determined to be active materials for the silicon-carbon-doped graphite negative electrode.
[0017] Optionally, the step of screening the silicon-carbon material according to the cycle stability index and the thickness expansion index, and determining the volume distribution of the silicon-carbon material is specifically:
[0018] Screen multiple silicon-carbon materials based on cycle stability and thickness expansion indicators, and determine the volume distribution of silicon-carbon materials;
[0019] If 0%≤b%-a%≤0.5%, the steps of determining that the silicon-carbon material and the graphite material are active materials of the silicon-carbon-doped graphite negative electrode are specifically:
[0020] The difference between b% of the graphite material and a% of each silicon-carbon material is calculated. If 0%≤b%-a%≤0.5%, the silicon-carbon material and the graphite material are determined to be active materials for the silicon-carbon-doped graphite negative electrode.
[0021] Optionally, the volume distribution of the silicon-carbon material and the graphite material is determined by analyzing with a laser particle size analyzer.
[0022] The present invention also discloses a silicon-carbon-doped graphite negative electrode, comprising a current collector and an active material layer laid on the current collector; the active material layer comprises an active material, a conductive agent and a binder; the active material comprises a silicon-carbon material and a graphite material;
[0023] The maximum volume density of the silicon-carbon material accounts for a%, the maximum volume density of the graphite material accounts for b%, and 0%≤b%-a%≤0.5%.
[0024] Optionally, the particle size distribution with the highest frequency of the silicon-carbon material is c μm, the particle size distribution with the highest frequency of the graphite material is d μm, and 0um≤dc≤5um.
[0025] Optionally, the silicon-carbon material accounts for 5% to 10% of the mass of the graphite material.
[0026] Optionally, the silicon-carbon material is one of a coated silicon-carbon material, a doped silicon-carbon material, and a surface-modified silicon-carbon material.
[0027] The present invention also discloses a lithium ion battery, comprising the active material of the silicon-doped carbon graphite negative electrode determined by the above active material selection method, or comprising the above silicon-doped carbon graphite negative electrode.
[0028] Compared with the prior art, the method for selecting active materials for silicon-carbon-doped graphite negative electrodes provided by the embodiment of the present invention has the following beneficial effects: the method for selecting active materials for silicon-carbon-doped graphite negative electrodes of the present invention directly performs preliminary screening at the material level. Specifically, before the graphite material and the silicon-carbon material are mixed, different graphite materials and silicon-carbon materials of the same rate are tested for volume distribution, and the size compatibility of the graphite material and the silicon-carbon material is evaluated at the material level. By preferentially selecting graphite materials with a small difference in volume density from the silicon-carbon material among the graphite materials that meet the rate cycle performance requirements, the graphite material with a small difference in volume density from the silicon-carbon material is selected. The material meets the requirement of 0%≤b%-a%≤0.5%, can control the gap between the graphite material and the silicon-carbon material within a certain appropriate range, minimize the gap between the graphite material and the silicon particles, and the reserved gap can accommodate the thickness expansion caused by the deintercalation of lithium in the silicon negative electrode material during the battery charging and discharging process. At the same time, the gap will not be too large to cause a rapid increase in the thickness expansion of the pole piece, which can effectively reduce the thickness expansion of the silicon-doped graphite negative electrode, shorten the evaluation cycle, reduce costs, reduce the rebound of the pole piece after the negative electrode coating roller is pressed, reduce the thickness expansion of the battery cell, and improve the cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments, in which:
[0030] Figure 1 It is the volume distribution diagram of graphite material A, graphite material B, graphite material C and silicon material of the test example of the present invention;
[0031] Figure 2 It is a volume distribution diagram of the test examples of the present invention, graphite material B-1, graphite material B-2, graphite material B-3, and graphite material B-4;
[0032] Figure 3 This is a graph showing the cycle performance data of the battery cells of the test examples of the present invention, graphite group A, graphite group B, and graphite group C;
[0033] Figure 4 It is a data chart of battery cell cycle performance of graphite material group B-1, graphite material group B-2, graphite material group B-3, and graphite material group B-4 of the test examples of the present invention. DETAILED DESCRIPTION
[0034] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. Now, in conjunction with the accompanying drawings, the preferred embodiments of the present invention are described in detail.
[0035] Mixing a certain proportion of silicon-carbon materials into graphite negative electrodes is the main measure to improve battery energy density. However, compared with pure graphite negative electrode systems, the presence of silicon components in this system of mixed graphite and silicon-carbon materials leads to a significant increase in the cell cycle expansion. Currently, the methods for improving the thickness expansion of mixed systems of graphite and silicon-carbon materials are mainly focused on silicon-carbon materials and cell manufacturing processes, such as batching and rolling. These methods are difficult, have a long evaluation cycle, are costly, and also bring other cycle performance risks.
[0036] Graphite materials are mainly divided into rate type and capacity type according to their functions. At present, the selection of negative electrode materials is mainly based on the rate requirements of the product to select the corresponding rate type graphite negative electrode, but there are also multiple choices of graphite materials with the same rate. The physical properties of graphite negative electrodes are quite different, such as specific surface area, graphite material degree and particle size. At present, the performance evaluation of the mixed system of graphite materials and silicon-carbon materials mainly relies on cycle testing and comparison after the battery cells are made. There is rarely a direct preliminary screening at the material level, resulting in a long evaluation cycle and high cost. It is very likely that the particle size of the graphite material and the particle size of the silicon material are poorly compatible. After the silicon-doped graphite material slurry is coated and rolled, the pole piece rebounds too much, resulting in a large expansion of the battery cell thickness and poor cycle performance.
[0037] The embodiment of the present invention provides a method for selecting active materials for a silicon-doped carbon graphite negative electrode, and the method is applied to selecting active materials for a silicon-doped carbon graphite negative electrode. The method for selecting active materials for a silicon-doped carbon graphite negative electrode comprises the following steps:
[0038] S100: screening silicon-carbon materials according to the cycle stability index and the thickness expansion index, and determining the volume distribution of the silicon-carbon materials; wherein the volume distribution of the silicon-carbon materials includes a maximum volume density accounting for a%;
[0039] S200: Screening graphite materials according to the rate cycle performance index and determining the volume distribution of the graphite materials; wherein the volume distribution of the graphite materials includes a maximum volume density accounting for b%;
[0040] S300: If 0%≤b%-a%≤0.5%, it is determined that the silicon-carbon material and the graphite material are active materials of the silicon-carbon-doped graphite negative electrode.
[0041] The applicant decomposed the thickness expansion of the mixed system of graphite material and silicon-carbon material and found that the thickness expansion of the silicon-carbon graphite negative electrode mainly comes from three aspects: first, the hard expansion of the silicon-carbon material and the graphite material itself. The lithium embedding of the graphite material is mainly an intercalation reaction without forming a structural change. The lithium embedding of the silicon-carbon material is an alloy reaction to form covalent bonds, and the volume expansion is large; second, the increase in internal gaps, including the increase in the gaps between silicon-carbon silicon-carbon materials and graphite materials, and the increase in the gaps between graphite materials; third, the accumulation of surface side reactants, among which the increase in the internal porosity of the electrode piece will lead to a rapid increase in cycle thickness.
[0042] The active material selection method for the silicon-carbon doped graphite negative electrode of the present invention directly performs preliminary screening at the material level. Specifically, before the graphite material and the silicon-carbon material are mixed, different graphite materials and silicon-carbon materials of the same rate are tested for volume distribution, and the adaptability of the size of the graphite material and the silicon-carbon material is evaluated at the material level. By preferentially selecting a graphite material with a small volume density difference with the silicon-carbon material among the graphite materials that meet the rate cycle performance requirements and meet the requirement of 0%≤b%-a%≤0.5%, the gap between the graphite material and the silicon-carbon material can be controlled within a certain suitable range, and the gap between the graphite material and the silicon particles can be minimized. The reserved gap can accommodate the thickness expansion caused by the deintercalation of lithium by the silicon negative electrode material during the charge and discharge process of the battery, and at the same time, the gap will not be too large to cause a rapid increase in the thickness expansion of the pole piece, which can effectively reduce the thickness expansion of the silicon-doped graphite negative electrode, shorten the evaluation period, reduce costs, reduce the rebound of the pole piece after the negative electrode coating roller is pressed, reduce the thickness expansion of the battery cell, and improve the cycle performance.
[0043] In step S100, the cycle stability index is used to evaluate the stability of the battery material in multiple charge and discharge cycles. In this step, the index is used to screen silicon-carbon materials, that is, the active material selection method of the present invention takes into account the performance of silicon-carbon materials in long-term cycles. The thickness expansion index indicates the degree of expansion or contraction of the silicon-carbon material during the charge and discharge cycle. Through the thickness expansion index, a more stable silicon-carbon material can be selected for the negative electrode of the battery.
[0044] Step S100 screens silicon-carbon materials by combining the cycle stability index and the thickness expansion index, and determines the volume distribution of the silicon-carbon materials, so as to screen out silicon-carbon materials suitable as silicon-carbon-doped graphite negative electrode active materials.
[0045] Specifically, silicon-carbon materials with good cycle stability index and thickness expansion index can be screened through single-factor full-battery system evaluation. Single-factor full-battery system evaluation refers to the use of a single variable (factor) in battery research to evaluate the performance of battery components or the entire battery system. It is a commonly used experimental design method in battery research and will not be described in detail here.
[0046] In step S200, the rate cycle performance index evaluates the performance of the battery during high rate charging and discharging. In this step, the graphite material is screened according to the rate cycle performance index, and the stability of the graphite material in rapid charging and discharging cycles is particularly considered. This step determines the volume distribution of the graphite material, including the maximum volume density ratio. By determining the volume distribution of the graphite material, the distribution of the graphite material particles within a certain volume can be better understood, and then the graphite material suitable for use as the silicon-carbon graphite negative electrode active material can be screened.
[0047] Volume distribution refers to the distribution of particles or substances within a certain volume, which is the particle size distribution of the material particles themselves. The particle size distribution is divided into quantity and volume distribution according to the measurement method. Generally, the focus is on Dv0 (the minimum diameter in the cumulative volume distribution), Dv50 (the median diameter in the cumulative volume distribution), and Dv100 (the maximum diameter in the cumulative volume distribution). The maximum volume density ratio reflects the main concentration point in the particle size distribution. The maximum volume density ratio indicates the ratio of the particle size whose volume fraction reaches the peak or maximum value in the particle size distribution.
[0048] Similarly, graphite materials with good rate cycling performance indicators can be screened and verified through single-factor full-battery system evaluation.
[0049] In step S300, only when 0%≤b%-a%≤0.5% is satisfied, the silicon-carbon material and the graphite material are determined as active materials of the silicon-carbon graphite negative electrode. When the requirement of 0%≤b%-a%≤0.5% is satisfied, the gap between the graphite material and the silicon-carbon material can be controlled within a certain suitable range, and the gap between the graphite material and the silicon particles can be minimized. The reserved gap can accommodate the thickness expansion caused by the deintercalation of lithium by the silicon negative electrode material during the battery charging and discharging process. At the same time, the gap will not be too large to cause the thickness expansion of the pole piece to increase rapidly, which can effectively reduce the thickness expansion of the silicon-doped graphite negative electrode.
[0050] Specifically, the difference of b%-a% can be any one of 0%, 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, and 0.5%.
[0051] Furthermore, the volume distribution of the silicon-carbon material also includes the particle size cμm with the highest frequency in the particle size distribution, and the volume distribution of the graphite material also includes the particle size dμm with the highest frequency in the particle size distribution. The active material selection method also includes the step of: if 0%≤b%-a%≤0.5%, and 0um≤dc≤5um, then the silicon-carbon material and the graphite material are determined to be active materials for the silicon-carbon-doped graphite negative electrode. Specifically, the difference in dc can be any one of 0um, 0.5um, 1um, 1.5um, 2um, 2.5um, 3um, 3.5um, 4um, 4.5um, and 5um. The particle size with the highest frequency in the particle size distribution refers to the particle size of the particle with the largest particle size proportion in the granular material.
[0052] This solution limits b%-a% to greater than or equal to 0% and less than 5%, and 0um≤dc≤5um, so as to determine the selection of silicon-carbon materials and graphite materials. Further, by matching graphite materials and silicon-carbon materials with appropriate particle sizes (0um≤dc≤5um), the thickness expansion of the negative electrode side of the battery cell can be effectively reduced, and the volume expansion of the silicon negative electrode during the charge and discharge cycle can be effectively inhibited, thereby improving the cycle performance of the lithium-ion battery.
[0053] Regarding the screening and adaptation of graphite materials and silicon-carbon materials, in one embodiment, the step S200 of screening graphite materials according to the rate cycling performance index and determining the volume distribution of the graphite materials is specifically as follows: screening multiple graphite materials according to the rate cycling performance index and determining the volume distribution of each graphite material.
[0054] The step S300 of determining that the silicon-carbon material and the graphite material are active materials for the silicon-carbon graphite negative electrode if 0% ≤ b% - a% ≤ 0.5% is specifically: calculating the difference between b% of each graphite material and a% of the silicon-carbon material, and if 0% ≤ b% - a% ≤ 0.5%, determining that the silicon-carbon material and the graphite material are active materials for the silicon-carbon graphite negative electrode. More specifically, calculating the difference between b% - a% and dc of the silicon-carbon material and each graphite material, and if 0% ≤ b% - a% ≤ 0.5%, and 0um ≤ dc ≤ 5um, determining that the silicon-carbon material and the graphite material are active materials for the silicon-carbon graphite negative electrode, and used for the silicon-carbon graphite negative electrode.
[0055] In this embodiment, by screening suitable graphite materials from a variety of graphite materials and matching them with silicon-carbon materials, the selection range of the matching of graphite materials and silicon-carbon materials can be improved. This is because silicon materials are still in the development stage, the process is still not mature enough compared to graphite materials, and there are fewer material types to choose from. Therefore, by matching different graphite materials with silicon-carbon materials, there are more graphite materials to choose from, which can improve the selection range of the matching of graphite materials and silicon-carbon materials.
[0056] Regarding the screening and adaptation of graphite materials and silicon-carbon materials, in another embodiment, the step S100 of screening silicon-carbon materials according to the cycle stability index and the thickness expansion index, and determining the volume distribution of the silicon-carbon materials is specifically: screening multiple silicon-carbon materials according to the cycle stability index and the thickness expansion index, and determining the volume distribution of the silicon-carbon materials.
[0057] The step S300 of determining that the silicon-carbon material and the graphite material are active materials for the silicon-carbon graphite negative electrode if 0% ≤ b% - a% ≤ 0.5% is specifically: calculating the difference between the b% of the graphite material and the a% of each silicon-carbon material, if 0% ≤ b% - a% ≤ 0.5%, then determining that the silicon-carbon material and the graphite material are active materials for the silicon-carbon graphite negative electrode. More specifically, calculating the difference between b% - a% and dc of each silicon-carbon material and the graphite material, if 0% ≤ b% - a% ≤ 0.5%, and 0um ≤ dc ≤ 5um, then determining that the silicon-carbon material and the graphite material are active materials for the silicon-carbon graphite negative electrode, used for the silicon-carbon graphite negative electrode.
[0058] In this embodiment, a suitable silicon-carbon material is selected from a plurality of silicon-carbon materials and matched with the graphite material.
[0059] Specifically, the volume distribution of the silicon-carbon material and the graphite material is determined by laser particle size analyzer analysis. Laser particle size analyzer is an instrument used to measure the particle size distribution in a granular or powder sample. It uses a laser light source to irradiate the sample and analyzes the size and distribution of the particles by detecting the angle and intensity of the scattered light. The working principle of the laser particle size analyzer is that after the laser light source irradiates the surface of the particle sample, the particles will scatter light, and the scattered light will be captured by the detector. By analyzing the intensity and angular distribution of the scattered light, the size range and distribution of the particles can be inferred.
[0060] The silicon-carbon material may be one of a coated silicon-carbon material, a doped silicon-carbon material, and a surface-modified silicon-carbon material. In terms of morphology, the silicon-carbon material may be one of a porous silicon-carbon material, a spherical silicon-carbon material, and a quasi-spherical silicon-carbon material.
[0061] The present invention also discloses a silicon-carbon-doped graphite negative electrode, comprising a current collector and an active material layer laid on the current collector; the active material layer comprises an active material, a conductive agent and a binder; the active material comprises a silicon-carbon material and a graphite material. The maximum volume density of the silicon-carbon material accounts for a%, and the maximum volume density of the graphite material accounts for b%, 0%≤b%-a%≤0.5%.
[0062] The active material of the silicon-carbon graphite negative electrode of the present invention is obtained by selecting the active material selection method mentioned above. The difference in volume density between the graphite material and the silicon-carbon material is small, and the maximum volume density meets the requirement of 0%≤b%-a%≤0.5%. The gap between the graphite material and the silicon-carbon material can be controlled within a certain suitable range, and the gap between the graphite material and the silicon particles can be minimized. The reserved gap can accommodate the thickness expansion caused by the deintercalation of lithium from the silicon negative electrode material during the battery charging and discharging process. At the same time, the gap is not too large to cause a rapid increase in the thickness expansion of the pole piece, which can effectively reduce the thickness expansion of the silicon-doped graphite negative electrode, shorten the evaluation cycle, reduce costs, reduce the pole piece rebound after the negative electrode coating roller is pressed, reduce the thickness expansion of the battery cell, and improve the cycle performance.
[0063] Specifically, the difference of b%-a% can be any one of 0%, 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, and 0.5%.
[0064] Furthermore, the particle size distribution frequency of the silicon-carbon material is cμm, and the particle size distribution frequency of the graphite material is dμm, and 0um≤dc≤5um. This solution limits b%-a% to greater than or equal to 0% and less than 5%, while 0um≤dc≤5um. Further, by matching graphite materials and silicon-carbon materials with suitable particle sizes (0um≤dc≤5um), the thickness expansion of the negative electrode side of the battery cell can be effectively reduced, and the volume expansion of the silicon negative electrode during the charge and discharge cycle can be effectively suppressed, thereby improving the cycle performance of the lithium-ion battery. Specifically, the difference in dc can be any one of 0um, 0.5um, 1um, 1.5um, 2um, 2.5um, 3um, 3.5um, 4um, 4.5um, and 5um.
[0065] Specifically, the silicon-carbon material accounts for 5% to 10% of the mass of the graphite material, and specifically can be 5%, 6%, 7%, 8%, 9%, 10%. The silicon-carbon material can be one of a coated silicon-carbon material, a doped silicon-carbon material, and a surface-modified silicon-carbon material. In terms of morphology, the silicon-carbon material can be one of a porous silicon-carbon material, a spherical silicon-carbon material, and a quasi-spherical silicon-carbon material.
[0066] The present invention also discloses a lithium ion battery, comprising the active material of the silicon-doped carbon graphite negative electrode determined by the above active material selection method, or comprising the above silicon-doped carbon graphite negative electrode.
[0067] The technical solution of the present invention is further illustrated by specific test examples below.
[0068] Test example
[0069] Silicon-carbon material verification: Silicon-carbon materials with good cycle stability and small thickness expansion (product model SiC-1) were screened out through single-factor full-battery system evaluation and verification, and their volume distribution was confirmed by laser particle size analyzer, including the maximum volume density ratio and the particle size with the highest frequency in particle size distribution, as shown in Tables 1 and 2, respectively. Figure 1 shown.
[0070] Graphite negative electrode verification: In the pure graphite material system, 7 rate-type graphite materials with good rate cycle performance were screened out through single-factor full battery system evaluation and verification (product models are Gr-A, Gr-B, Gr-C, Gr-B1, Gr-B2, Gr-B3, Gr-B4), and their volume distribution was confirmed by laser particle size analyzer, including the maximum volume density ratio and the particle size with the highest frequency in particle size distribution, as shown in Tables 1 and 2, respectively. Figure 1 shown.
[0071] The screened 7 graphite materials were divided into 7 groups, namely graphite group A (graphite material product model Gr-A), graphite group B (graphite material product model Gr-B), graphite group C (graphite material product model Gr-C), graphite group B-1 (graphite material product model Gr-B1), graphite group B-2 (graphite material product model Gr-B2), graphite group B-3 (graphite material product model Gr-B3) and graphite group B-4 (graphite material product model Gr-B4). 10% by mass of silicon-carbon material was added to the same mass of graphite material A, graphite material B, graphite material C, graphite material B-1, graphite material B-2, graphite material B-3 and graphite material B-4 respectively to obtain negative electrode active materials for use.
[0072] The negative electrode active material, carbon black, polyacrylic acid (PAA) and solvent water were mixed in a mass ratio of 90:2:8 to form negative electrode slurry. The 7 groups of negative electrode slurries were coated with intermittent extrusion coating equipment. The single-layer slurry coating surface density was 150g / m 2 , coating speed 8m / s, coated on copper foil to form an active material layer, after drying, slitting, cutting, welding positive electrode ears, 7 groups of silicon-doped carbon graphite negative electrodes were obtained.
[0073] Lithium cobalt oxide, carbon black, binder polyvinylidene fluoride (PVDF) and solvent NMP are used to make positive electrode slurry in a mass ratio of 98:1.2:0.8. The positive electrode slurry is coated with intermittent extrusion coating equipment, and the coating surface density is 54g / m 2 The coating speed is 8m / s, and it is applied to 12um aluminum foil to form an active material layer. After drying, slitting, cutting, and welding the positive electrode ears, the positive electrode is obtained.
[0074] The 7 groups of silicon-carbon-doped graphite negative electrodes were respectively wound with the positive electrodes to form a core, which was then packaged, injected with liquid and then formed into 7 groups of battery cells.
[0075] Cycle performance test: 7 groups of batteries were cycled for 600 cycles using the same test method. At a constant temperature of 25°C, they were charged to 4.45V at a constant current of 1C, then charged at a constant voltage of 4.45V until the current dropped to 0.05C, and then discharged to 2.8V at a constant current of 1C to obtain the first-cycle discharge capacity (C0); this was repeated until the 600th cycle, and the discharge capacity after 600 cycles was obtained, recorded as Cn. Capacity retention rate = discharge capacity after 500 cycles (Cn) / first-cycle discharge capacity (C0) capacity retention rate.
[0076] like Figure 3 Comparing the cycle performance data of graphite group A, graphite group B, and graphite group C battery cells, the graphite material group B and graphite material group C, where the maximum volume density ratio difference (%) between silicon-carbon material and graphite material is ≤0.5%, have a thickness expansion of <10% and a capacity retention rate of >80% after 600 cycles at 25°C. Among them, graphite material group B has the highest particle size distribution frequency between silicon-carbon material and graphite material and the smallest particle size difference (≤5um), so it exhibits better cycle performance. The maximum volume density ratio difference (%) between silicon-carbon material and graphite material in graphite material group A is as large as 3.98%, resulting in large thickness expansion during the cycle, rapid growth of particle gaps, poor contact of the conductive network between particles, and large cycle attenuation.
[0077] like Figure 4 , comparing the cycle performance data of graphite B-1 group, graphite B-2 group, graphite B-3 group, and graphite B-4 group battery cells, the graphite B-1 group, where the difference in particle size distribution frequency between silicon-carbon material and graphite material is 5μm, has a thickness expansion of <10% and a capacity retention rate of >80% after 600 cycles at 25°C, compared with the graphite B-1 group, where the difference in particle size distribution frequency between silicon-carbon material and graphite material is 5.1μm, and shows better cycle performance. The graphite B-3 group, where the difference in the maximum volume density between silicon-carbon material and graphite is 0.5%, has a smaller thickness expansion and a better capacity retention rate after 600 cycles at 25°C, compared with the graphite B-4 group, where the difference in the maximum volume density between silicon-carbon material and graphite is 0.51%.
[0078] In summary, in order to improve the cycle performance of silicon-doped graphite negative electrode, the particle volume distribution of graphite material and silicon-carbon material is determined. First, it is evaluated to determine whether the difference (%) between the maximum volume density of silicon-carbon material and graphite material is ≤0.5%, so that the cycle retention rate and thickness expansion of the battery cell have advantages; secondly, it is determined whether the difference in the highest frequency particle size between silicon-carbon material and graphite material is ≤5um. When both are met, the gap between graphite material and silicon-carbon material is small after mixing, and the cycle retention rate and thickness expansion of the battery cell are more advantageous.
[0079] Table 1 Particle size distribution data of different graphite materials and silicon carbon materials
[0080]
[0081]
[0082] It should be understood that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. For those skilled in the art, the technical solutions described in the above embodiments can be modified, or some of the technical features therein can be replaced by equivalents; and all these modifications and replacements should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for selecting silicon-doped carbon graphite negative electrode active material, characterized in that: Includes steps: According to the cycle stability index and the thickness expansion index, the silicon-carbon material is screened, and the volume distribution of the silicon-carbon material is determined; wherein the volume distribution of the silicon-carbon material includes a% of the maximum volume density; Screening graphite materials according to the rate cycle performance index and determining the volume distribution of the graphite materials; wherein the volume distribution of the graphite materials includes a maximum volume density accounting for b%; If 0%≤b%-a%≤0.5%, it is determined that the silicon-carbon material and the graphite material are active materials of the silicon-carbon-doped graphite negative electrode.
2. The active material selection method according to claim 1, characterized in that: The volume distribution of the silicon-carbon material also includes a particle size with the highest frequency in the particle size distribution c μm, and the volume distribution of the graphite material also includes a particle size with the highest frequency in the particle size distribution d μm; The active material selection method further comprises the steps of: If 0%≤b%-a%≤0.5%, and 0um≤dc≤5um, it is determined that the silicon-carbon material and the graphite material are active materials of the silicon-carbon-doped graphite negative electrode.
3. The method for selecting active materials according to claim 1, characterized in that: The steps of screening the graphite material according to the rate cycle performance index and determining the volume distribution of the graphite material are specifically as follows: Screen multiple graphite materials based on rate cycle performance indicators and determine the volume distribution of each graphite material; If 0%≤b%-a%≤0.5%, the steps of determining that the silicon-carbon material and the graphite material are active materials of the silicon-carbon-doped graphite negative electrode are specifically: The difference between b% of each graphite material and a% of the silicon-carbon material is calculated. If 0%≤b%-a%≤0.5%, the silicon-carbon material and the graphite material are determined to be active materials for the silicon-carbon-doped graphite negative electrode.
4. The method for selecting active materials according to claim 1, characterized in that: The steps of screening the silicon-carbon material according to the cycle stability index and the thickness expansion index and determining the volume distribution of the silicon-carbon material are specifically as follows: Screen multiple silicon-carbon materials based on cycle stability and thickness expansion indicators, and determine the volume distribution of silicon-carbon materials; If 0%≤b%-a%≤0.5%, the steps of determining that the silicon-carbon material and the graphite material are active materials of the silicon-carbon-doped graphite negative electrode are specifically: The difference between b% of the graphite material and a% of each silicon-carbon material is calculated. If 0%≤b%-a%≤0.5%, the silicon-carbon material and the graphite material are determined to be active materials for the silicon-carbon-doped graphite negative electrode.
5. The method for selecting active materials according to claim 1, characterized in that: The volume distribution of the silicon-carbon material and the graphite material is determined by laser particle size analyzer analysis.
6. A silicon-doped carbon graphite negative electrode, characterized in that: It includes a current collector and an active material layer laid on the current collector; the active material layer includes an active material, a conductive agent and a binder; the active material includes a silicon-carbon material and a graphite material; The maximum volume density of the silicon-carbon material accounts for a%, the maximum volume density of the graphite material accounts for b%, and 0%≤b%-a%≤0.5%.
7. The silicon-doped carbon graphite negative electrode according to claim 6, characterized in that: The particle size distribution frequency of the silicon-carbon material has a maximum particle size of c μm, the particle size distribution frequency of the graphite material has a maximum particle size of d μm, and 0um≤dc≤5um.
8. The silicon-doped carbon graphite negative electrode according to claim 6 or 7, characterized in that: The silicon-carbon material accounts for 5% to 10% of the mass of the graphite material.
9. The silicon-doped carbon graphite negative electrode according to claim 6 or 7, characterized in that: The silicon-carbon material is one of a coated silicon-carbon material, a doped silicon-carbon material, and a surface-modified silicon-carbon material.
10. A lithium ion battery, characterized in that: An active material of a silicon-doped carbon graphite negative electrode determined by the active material selection method described in any one of claims 1 to 4, or a silicon-doped carbon graphite negative electrode described in any one of claims 5 to 9.