Transparent conductive film

By forming a high surface roughness easy-to-adhesive layer on a transparent substrate and forming a transparent conductive layer with high energy rare gas sputtering, the problem of insufficient adhesion of the transparent conductive layer to the substrate is solved, and the application in folding display panels is improved Stability and durability in the

CN119008084APending Publication Date: 2024-11-22NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410571718.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-10
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the application of the existing transparent conductive films, the transparent conductive layer has insufficient adhesion to the transparent substrate, resulting in easy peeling during folding and reusing, affecting the stability and life of the equipment.

Method used

By forming an easy-to-adhesive layer with a surface roughness of 1.50 nm or more on the transparent substrate, and using rare gas atoms with atomic number greater than argon, such as krypton, as sputtering gas, a transparent conductive layer is formed during the sputtering film formation process. Improve the anchoring effect and adhesion between the conductive layer and the substrate.

Benefits of technology

It significantly improves the adhesion of the transparent conductive layer to the transparent substrate, enhances the stability and durability in the folding and multiplexing process, and is suitable for high-demand applications such as foldable display panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008084A_ABST
    Figure CN119008084A_ABST
Patent Text Reader

Abstract

The invention relates to a transparent conductive film. This transparent conductive film (X) is provided with a transparent substrate (10) and a transparent conductive layer (20). The transparent substrate (10) has a first surface (10a) and a second surface (10b) facing the first surface (10a). The transparent conductive layer (20) is located on a first surface (10a) of the transparent substrate (10). The first surface (10a) has a surface roughness (Ra) of 1.50 nm or more. The transparent conductive layer (20) contains a rare gas atom having a larger atomic number than argon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a transparent conductive film. Background Art

[0002] In the past, it is known that a transparent conductive film has a transparent substrate made of resin and a transparent conductive layer (transparent conductive layer) in sequence in the thickness direction. The transparent conductive layer is used, for example, as a conductor film for forming transparent electrodes in various devices such as display panels, touch panels, and solar cells. The transparent conductive layer is formed, for example, by forming a film of a transparent conductive material on a transparent substrate using a sputtering method (sputtering film formation). In sputtering film formation, argon is used as a sputtering gas (inert gas) in the past. Regarding the technology related to such a transparent conductive film, for example, it is recorded in the following patent document 1.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2004-213990

[0006] For transparent conductive films, it is required that the transparent conductive layer has good adhesion to the transparent substrate to prevent the transparent conductive layer from peeling off from the transparent substrate. On the other hand, in the use of smartphones or tablet terminals, the development of display panels that can be repeatedly bent (foldable) is being promoted. For example, for transparent conductive films used in foldable display panels, it is strongly required that the transparent conductive layer has high adhesion to the transparent substrate. Summary of the invention

[0007] The present invention provides a transparent conductive film suitable for achieving high adhesion of a transparent conductive layer to a transparent substrate.

[0008] The present invention [1] includes a transparent conductive film, which comprises: a transparent substrate having a first surface and a second surface opposite to the first surface; and a transparent conductive layer on the first surface, wherein the first surface has a surface roughness Ra of 1.50 nm or more, and the transparent conductive layer contains rare gas atoms with an atomic number greater than argon.

[0009] The present invention [2] includes the transparent conductive film described in the above [1], wherein the rare gas atom is krypton.

[0010] The present invention [3] includes the transparent conductive film described in [1] or [2] above, wherein the transparent conductive layer is a crystalline film.

[0011] The present invention [4] includes the transparent conductive film according to any one of [1] to [3] above, wherein the surface roughness Ra is 2.50 nm or less.

[0012] The present invention [5] includes the transparent conductive film according to any one of [1] to [4] above, wherein the transparent substrate has an easy adhesive layer forming the first surface, and the easy adhesive layer has an average thickness of 50 nm or less.

[0013] Effects of the Invention

[0014] In the transparent conductive film of the present invention, as described above, the surface roughness Ra of the first surface of the transparent substrate is greater than 1.50 nm, and a transparent conductive layer is formed on the first surface. Such a structure is suitable for ensuring a high anchoring effect of the first surface on the transparent conductive layer, and helps to improve the adhesion of the transparent conductive layer to the transparent substrate. In addition, in the transparent conductive film of the present invention, as described above, the transparent conductive layer contains rare gas atoms with an atomic number greater than argon. Such a transparent conductive layer can be formed by sputtering film forming of a transparent conductive material on the first surface. In the sputtering film forming, rare gas atoms with an atomic number greater than argon are used as sputtering gas. In such sputtering film forming, compared with sputtering film forming using argon as sputtering gas, the transparent conductive material can collide with the transparent substrate with high energy and be deposited on the substrate. This situation helps to improve the adhesion of the transparent conductive layer to the transparent substrate. Therefore, the transparent conductive film of the present invention is suitable for achieving high adhesion of the transparent conductive layer to the transparent substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 It is a schematic cross-sectional view of one embodiment of the transparent conductive film of the present invention.

[0016] FIG. 2A to FIG. 2C express Figure 1 An example of a method for producing a transparent conductive film is shown. Figure 2A It shows the process of preparing the resin film. Figure 2B It indicates the process of forming an easy-adhesion layer on a resin film. Figure 2C This shows the step of forming a transparent conductive layer on the easy-adhesion layer.

[0017] Figure 3 Indicated in Figure 1 In the transparent conductive film shown, the transparent conductive layer is patterned.

[0018] Description of Reference Numerals

[0019] X: transparent conductive film; D: thickness direction; 10: transparent substrate; 10a: first surface; 10b: second surface; 11: resin film; 12: easy-adhesion layer; 20: transparent conductive layer; 21: surface. DETAILED DESCRIPTION

[0020] The transparent conductive film X as one embodiment of the present invention has a transparent substrate 10 and a transparent conductive layer 20 in the thickness direction D in sequence. The transparent substrate 10 has a first surface 10a and a second surface 10b opposite to the first surface 10a. The transparent conductive layer 20 is arranged on the first surface 10a. That is, the transparent conductive layer 20 is in contact with the first surface 10a. In addition, the transparent conductive film X has a sheet shape extending in a direction (surface direction) orthogonal to the thickness direction D. Such a transparent conductive film X is an element provided in a touch sensor device, a dimming element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, and an image display device (display panel).

[0021] In the present embodiment, the transparent base material 10 includes a resin film 11 and an easily adhesive layer 12 in this order in the thickness direction D. The easily adhesive layer 12 is in contact with the resin film 11. The easily adhesive layer 12 forms the first surface 10a.

[0022] From the viewpoint of ensuring a high anchoring effect of the first surface 10a on the transparent conductive layer 20, the surface roughness Ra of the first surface 10a is 1.50 nm or more, preferably 1.60 nm or more, and more preferably 1.65 nm or more. From the viewpoint of the ease of forming a crystalline transparent conductive layer 20, the surface roughness Ra is preferably 2.50 nm or less, more preferably 2.20 nm or less, and more preferably 2.00 nm or less. The surface roughness Ra is the arithmetic mean surface roughness based on JIS B 0601-2001. The method for measuring the surface roughness Ra is specifically as described later in the examples.

[0023] The resin film 11 is a base material for ensuring the strength of the transparent conductive film X. In addition, the resin film 11 is a transparent resin film having flexibility. As the material of the resin film 11, for example, polyester resin, polyolefin resin, acrylic resin, polycarbonate resin, polyethersulfone resin, polyarylate resin, melamine resin, polyamide resin, polyimide resin, cellulose resin and polystyrene resin can be listed. As the polyester resin, for example, polyethylene terephthalate (PET), polybutylene terephthalate and polyethylene naphthalate can be listed. As the polyolefin resin, for example, polyethylene, polypropylene and cycloolefin polymer can be listed. As the acrylic resin, for example, polymethacrylate can be listed. As the material of the resin film 11, for example, from the viewpoint of transparency and strength, polyester resin is preferably used, and PET is more preferably used.

[0024] The surface of the easily adhesive layer 12 side in the resin film 11 may be subjected to a surface modification treatment. Examples of the surface modification treatment include a corona treatment, a plasma treatment, an ozone treatment, a primer treatment, a glow treatment, and a coupling agent treatment.

[0025] From the viewpoint of ensuring the strength of the transparent conductive film X, the thickness of the resin film 11 is preferably 10 μm or more, more preferably 20 μm or more, and further preferably 30 μm or more.

[0026] From the viewpoint of ensuring the handleability of the resin film 11 in a roll-to-roll method, the thickness of the resin film 11 is preferably 300 μm or less, more preferably 200 μm or less, and further preferably 150 μm or less.

[0027] The total light transmittance (JIS K 7375-2008) of the resin film 11 is preferably 60% or more, more preferably 80% or more, and further preferably 85% or more. Such a configuration is suitable for ensuring the transparency required for the transparent conductive film X when the transparent conductive film X is provided in a touch sensor device, a dimming element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, and an image display device. The total light transmittance of the resin film 11 is, for example, 100% or less.

[0028] The easy-adhesion layer 12 improves the adhesion of the transparent conductive layer 20 to the transparent substrate 10. The easy-adhesion layer 12 is a cured product of a curable resin composition containing a curable resin and particles in this embodiment. Examples of the curable resin include polyester resins, acrylic urethane resins, acrylic resins (excluding acrylic urethane resins), urethane resins (excluding acrylic urethane resins), amide resins, silicone resins, epoxy resins, and melamine resins. These curable resins may be used alone or in combination of two or more.

[0029] Examples of curable resins include ultraviolet curable resins and thermosetting resins. Ultraviolet curable resins are preferred because they can be cured without high-temperature heating and thus contribute to improved production efficiency of the transparent conductive film X.

[0030] As the particles, for example, inorganic oxide particles and organic particles can be cited. As the material of the inorganic oxide particles, for example, silicon dioxide, aluminum oxide, titanium dioxide, zirconium oxide, calcium oxide, tin oxide, indium oxide, cadmium oxide and antimony oxide can be cited. As the material of the organic particles, for example, polymethyl methacrylate, polystyrene, polyurethane, acrylic acid-styrene copolymer, benzoguanamine, melamine and polycarbonate can be cited. As the particles, inorganic oxide particles are preferably used, and silicon dioxide particles and / or zirconium oxide particles are more preferably used.

[0031] From the perspective of forming sufficient surface unevenness on the first surface 10a, the average particle size (D50) of the particles is preferably greater than 20 nm, more preferably greater than 25 nm, and further preferably greater than 30 nm. From the perspective of appropriately forming a crystalline transparent conductive layer 20 (from the perspective of suppressing the obstruction of crystallization of the transparent conductive layer 20), the average particle size of the particles is preferably less than 200 nm, more preferably less than 150 nm, further preferably less than 120 nm, and particularly preferably less than 100 nm. The average particle size (D50) of the particles is the median particle size in the volume-based particle size distribution (the particle size at which the volume cumulative frequency reaches 50% from the small diameter side), for example, based on the particle size distribution obtained by the laser diffraction / scattering method (the same applies to the average particle size of other particles).

[0032] From the viewpoint of ensuring the surface unevenness of the first surface 10a, the content of the particles in the easy bonding layer 12 is preferably 1 mass part or more, more preferably 5 mass parts or more, and further preferably 8 mass parts or more per 100 mass parts of curable resin. The content of the particles in the easy bonding layer 12 is preferably 30 mass parts or less, more preferably 20 mass parts or less, and further preferably 12 mass parts or less per 100 mass parts of curable resin.

[0033] From the viewpoint of ensuring adhesion with the transparent conductive layer 20, the average thickness of the easy-adhesion layer 12 is preferably 1 nm or more, more preferably 5 nm or more, further preferably 7 nm or more, and particularly preferably 9 nm or more. From the viewpoint of thinning the transparent conductive film X, the average thickness of the easy-adhesion layer 12 is preferably 50 nm or less, more preferably 30 nm or less, and further preferably 20 nm or less. The method for measuring the average thickness of the easy-adhesion layer 12 is specifically described later in the examples.

[0034] The surface of the transparent conductive layer 20 side in the easy-adhesion layer 12 may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.

[0035] The thickness of the transparent substrate 10 is preferably 10 μm or more, more preferably 20 μm or more, and further preferably 30 μm or more. The thickness of the transparent substrate 10 is preferably 300 μm or less, more preferably 200 μm or less, and further preferably 150 μm or less. These configurations related to the thickness of the transparent substrate 10 are suitable for ensuring the handleability of the transparent conductive film X.

[0036] The total light transmittance (JIS K 7375-2008) of the transparent substrate 10 is preferably 60% or more, more preferably 80% or more, and further preferably 85% or more. Such a configuration is suitable for ensuring the transparency required for the transparent conductive film X when the transparent conductive film X is provided in a touch sensor device, a dimming element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, and an image display device. The total light transmittance of the transparent substrate 10 is, for example, 100% or less.

[0037] The transparent conductive layer 20 is a film having both light transmittance and conductivity. Such a transparent conductive layer 20 is formed of a transparent conductive material. As a transparent conductive material, for example, a transparent conductive oxide can be cited. In addition, the transparent conductive layer 20 is preferably a crystalline film. The transparent conductive layer 20 is a crystalline film suitable for suppressing a large change in resistance value in the transparent conductive layer 20 due to subsequent heating.

[0038] Whether the transparent conductive layer (in the transparent conductive film X, the transparent conductive layer 20 on the transparent substrate 10) is a crystalline film can be determined, for example, by the following method. First, the transparent conductive layer is immersed in hydrochloric acid with a concentration of 5% by mass at 20°C for 15 minutes. Then, the transparent conductive layer is washed with water and then dried. Next, on the exposed plane of the transparent conductive layer (in the transparent conductive film X, the surface 21 of the transparent conductive layer 20 on the opposite side of the transparent substrate 10), the resistance between a pair of terminals separated by a distance of 15 mm (terminal resistance) is measured. In this measurement, when the terminal resistance is less than 10 kΩ, it can be determined that the transparent conductive layer is a crystalline film. In addition, by observing the presence of grains in the transparent conductive layer using a transmission electron microscope, it can also be determined that the transparent conductive layer is a crystalline film.

[0039] As conductive oxides, for example, conductive oxides containing indium and conductive oxides containing antimony can be listed. As conductive oxides containing indium, for example, indium tin composite oxide (ITO), indium zinc composite oxide (IZO), indium gallium composite oxide (IGO) and indium gallium zinc composite oxide (IGZO) can be listed. As conductive oxides containing antimony, for example, antimony tin composite oxide (ATO) can be listed. From the viewpoint of achieving high transparency and good conductivity, as conductive oxides, conductive oxides containing indium are preferably used, and ITO is more preferably used. The ITO may also contain a metal or semimetal other than In and Sn in an amount less than the content of each of In and Sn.

[0040] The content of tin oxide in ITO is relative to indium oxide (In 2 O 3 ) and tin oxide (SnO 2) is preferably 1% by mass or more, more preferably 3% by mass or more, further preferably 5% by mass or more, and particularly preferably 7% by mass or more. The ratio of the number of tin atoms in ITO to the number of indium atoms (tin atoms / indium atoms) is preferably 0.01 or more, more preferably 0.03 or more, further preferably 0.05 or more, and particularly preferably 0.07 or more. These compositions are suitable for ensuring the durability of the transparent conductive layer 20. In addition, the ratio of the content of tin oxide in ITO to the total content of indium oxide and tin oxide is preferably 15% by mass or less, more preferably 13% by mass or less, and further preferably 12% by mass or less. The ratio of the number of tin atoms in ITO to the number of indium atoms (tin atoms / indium atoms) is preferably 0.15 or less, more preferably 0.13 or less, and further preferably 0.12 or less. From the viewpoint of low resistance of the transparent conductive layer 20, these compositions are preferred.

[0041] The tin oxide ratio in ITO can be identified, for example, as follows. First, the existence ratio of indium atoms (In) and tin atoms (Sn) in ITO, which is the object of measurement, is determined by X-ray photoelectron spectroscopy. The ratio of the number of Sn atoms in ITO to the number of In atoms is determined based on the existence ratios of In and Sn in ITO. Thus, the tin oxide ratio in ITO is obtained. In addition, the tin oxide ratio in ITO can also be determined based on the tin oxide (SnO) of the ITO target used in sputtering film formation. 2 ) content ratio.

[0042] The transparent conductive layer 20 contains rare gas atoms (atoms E) having an atomic number greater than that of argon. Examples of such rare gas atoms include krypton (Kr) and xenon (Xe), with Kr being preferred. In addition, the transparent conductive layer 20 may also contain argon (Ar). In the present embodiment, the rare gas atoms in the transparent conductive layer 20 originate from rare gas atoms used as a sputtering gas in the sputtering method described later for forming the transparent conductive layer 20. In the present embodiment, the transparent conductive layer 20 is a film (sputtered film) formed by the sputtering method. The presence of atoms E in the transparent conductive layer 20 helps to improve the adhesion of the transparent conductive layer 20 to the transparent substrate 10 as described later. Examples of methods for determining whether the transparent conductive layer 20 contains atoms E include fluorescent X-ray analysis and Rutherford Backscattering Spectrometry (RBS).

[0043] The content ratio of atoms E in the transparent conductive layer 20 is preferably 0.0001 atomic % or more in the entire region in the thickness direction D, and is preferably 1 atomic % or less, more preferably 0.5 atomic % or less, further preferably 0.3 atomic % or less, and particularly preferably 0.2 atomic % or less. As a method for identifying the content ratio of rare gas atoms in the transparent conductive layer 20, for example, fluorescent X-ray analysis and Rutherford backscattering spectroscopy (RBS) can be cited. Even if it is less than the detection limit value in the identification method of the content ratio of rare gas atoms, when the presence of atoms E is confirmed by the above-mentioned determination method of atoms E in the transparent conductive layer 20, the transparent conductive layer 20 contains atoms E.

[0044] From the viewpoint of reducing the resistance of the transparent conductive layer 20, the thickness of the transparent conductive layer 20 is preferably 10 nm or more, more preferably 20 nm or more, and further preferably 30 nm or more. In addition, from the viewpoint of ensuring bendability (difficulty of cracking when bent), the thickness of the transparent conductive layer 20 is preferably 300 nm or less, more preferably 150 nm or less, further preferably 120 nm or less, further preferably 100 nm or less, and particularly preferably 80 nm or less.

[0045] The total light transmittance (JIS K 7375-2008) of the transparent conductive layer 20 is preferably 60% or more, more preferably 80% or more, and further preferably 85% or more. Such a configuration is suitable for ensuring transparency in the transparent conductive layer 20. The total light transmittance of the transparent conductive layer 20 is, for example, 100% or less.

[0046] The total light transmittance (JIS K 7375-2008) of the transparent conductive film X is preferably 60% or more, more preferably 80% or more, and further preferably 85% or more. Such a configuration is suitable for ensuring the transparency required for the transparent conductive film X when the transparent conductive film X is provided in a touch sensor device, a dimming element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, and an image display device. The total light transmittance of the base film 10 is, for example, 100% or less.

[0047] The transparent conductive film X is produced, for example, as follows.

[0048] First, if Figure 2A As shown, a resin film 11 is prepared.

[0049] Then, if Figure 2B As shown, the easy-adhesion layer 12 is formed on one surface of the resin film 11 in the thickness direction D. By forming the easy-adhesion layer 12 on the resin film 11, the transparent substrate 10 is manufactured.

[0050] The easy-adhesion layer 12 can be formed by applying the above-mentioned curable resin composition on the resin film 11 to form a coating film, and then curing the coating film. When the curable resin composition contains an ultraviolet curable resin, the coating film is cured by ultraviolet irradiation. When the curable resin composition contains a thermosetting resin, the coating film is cured by heating.

[0051] The exposed surface of the easy-adhesion layer 12 formed on the resin film 11 may be subjected to surface modification treatment as required. When plasma treatment is performed as the surface modification treatment, argon gas is used as an inert gas, for example. In addition, the discharge power in the plasma treatment is, for example, 10 W or more, and, for example, 5000 W or less.

[0052] Then, if Figure 2C As shown, the transparent conductive layer 20 is formed on the transparent substrate 10 (transparent conductive layer forming step). Specifically, the transparent conductive layer 20 is formed by forming a transparent conductive material on the easy-adhesion layer 12 in the transparent substrate 10 by sputtering.

[0053] In the sputtering method, it is preferable to use a sputtering film forming device that can perform a film forming process in a roll-to-roll manner. In the production of the transparent conductive film X, when a roll-to-roll sputtering film forming device is used, a long transparent substrate 10 is made to travel from a delivery roll provided in the device to a take-up roll, and a material is formed on the transparent substrate 10 to form a transparent conductive layer 20. In addition, in the sputtering method, a sputtering film forming device having one film forming chamber can be used, and a sputtering film forming device having a plurality of film forming chambers sequentially arranged along the travel path of the transparent substrate 10 can also be used.

[0054] In the sputtering method, specifically, a sputtering gas (inert gas) is introduced into a film forming chamber of a sputtering film forming device under vacuum conditions, and a negative voltage is applied to a target on a cathode arranged in the film forming chamber. As a result, a glow discharge is generated, gas atoms are ionized, the gas ions collide with the target surface at high speed, the target material is ejected from the target surface, and the ejected target material is deposited on the transparent substrate 10. As a target material, for example, a sintered body of the conductive oxide described above with respect to the transparent conductive layer 20 is used. As a sputtering gas, a rare gas atom (atom E) having an atomic number greater than argon is used. Atom E has a mass greater than argon. Therefore, atom E is suitable for colliding with the target with an energy higher than that of argon, and therefore, is suitable for ejecting the target material from the target surface with high energy. As atom E, Kr is preferably used. As a sputtering gas, a mixed gas containing atom E and argon can also be used.

[0055] The sputtering method is preferably a reactive sputtering method. In the reactive sputtering method, for example, in addition to the sputtering gas, oxygen as a reactive gas is also introduced into the film forming chamber. In the reactive sputtering method, the ratio of the amount of oxygen introduced into the film forming chamber to the total amount of the sputtering gas and oxygen introduced is, for example, 0.01% by flow or more, and, for example, 15% by flow or less.

[0056] The gas pressure in the film forming chamber in film forming by sputtering (sputtering film forming) is, for example, 0.02 Pa or more, and, for example, 1 Pa or less.

[0057] From the viewpoint of promoting the crystal growth of the material to be formed and forming the transparent conductive layer 20 in the form of a good crystal film, the temperature of the transparent substrate 10 during sputtering is preferably 10° C. or higher, more preferably 20° C. or higher, and further preferably 30° C. or higher. From the viewpoint of suppressing outgassing from the transparent substrate 10 during sputtering and forming the transparent conductive layer 20 in the form of a good crystal film, the temperature of the transparent substrate 10 during sputtering is preferably 100° C. or lower, more preferably 70° C. or lower, and further preferably 50° C. or lower.

[0058] As a power source for applying a voltage to the target, for example, a DC power source, an AC power source, an MF power source, and an RF power source can be listed. As a power source, a DC power source and an RF power source can also be used together. The absolute value of the discharge voltage in sputtering film formation is, for example, 50 V or more, and, for example, 500 V or less. The horizontal magnetic field intensity on the target is, for example, 10 mT or more, and, for example, 100 mT or less.

[0059] As described above, the transparent conductive film X can be manufactured.

[0060] The transparent conductive layer 20 in the transparent conductive film X may also be Figure 3 The transparent conductive layer 20 is patterned as schematically shown. The transparent conductive layer 20 can be patterned by etching the transparent conductive layer 20 through a predetermined etching mask. The patterned transparent conductive layer 20 functions as a wiring pattern, for example.

[0061] In the transparent conductive film X, as described above, the surface roughness Ra of the first surface 10a of the transparent substrate 10 is 1.50 nm or more, preferably 1.60 nm or more, and more preferably 1.65 nm or more, and the transparent conductive layer 20 is formed on the first surface 10a. Such a structure is suitable for ensuring a high anchoring effect of the first surface 10a on the transparent conductive layer 20, and helps to improve the adhesion of the transparent conductive layer 20 to the transparent substrate 10.

[0062] In addition, in the transparent conductive film X, the transparent conductive layer 20 contains rare gas atoms having an atomic number greater than argon. Such a transparent conductive layer 20 can be formed by sputtering a transparent conductive material on the first surface 10a of the transparent substrate 10 as described above. In the sputtering film formation, atoms E (rare gas atoms having an atomic number greater than argon) are used as sputtering gas. In such sputtering film formation, compared with sputtering film formation using argon as sputtering gas, the transparent conductive material can be deposited by colliding with the transparent substrate 10 at a high energy. This helps to improve the adhesion of the transparent conductive layer 20 to the transparent substrate 10.

[0063] The transparent conductive film X as described above is suitable for achieving high adhesion of the transparent conductive layer 20 to the transparent substrate 10. Specifically, it is shown in the examples and comparative examples described later.

[0064] Example

[0065] The present invention is specifically described below with reference to the following examples. However, the present invention is not limited to the examples. In addition, the specific numerical values ​​of the following amounts (contents), physical property values, parameters, etc. can be replaced by the upper limits (values ​​defined in the form of "below" or "less than") or lower limits (values ​​defined in the form of "above" or "greater than") of the amounts (contents), physical property values, parameters, etc. corresponding to them recorded in the above-mentioned "Specific Embodiments".

[0066] [Example 1]

[0067] First, a roll of a long transparent substrate S (product name "DIAFOIL T910E125", thickness 125 μm, manufactured by Mitsubishi Chemical Corporation) was prepared. The transparent substrate S is composed of a polyethylene terephthalate (PET) film (thickness 125 μm) as a resin film and an easy-adhesion layer formed on one side of the PET film. The easy-adhesion layer contains silica particles (average particle size 30 nm) as particles. The average thickness of the easy-adhesion layer is 10 nm.

[0068] Next, a transparent conductive layer with a thickness of 125 nm was formed on the easy-adhesion layer in the transparent substrate by reactive sputtering (transparent conductive layer forming process). In this process, a roll-to-roll sputtering film forming device (DC magnetron sputtering film forming device) was used. The device has a film forming chamber that can make a working film (work film) travel in a roll-to-roll manner and perform a film forming process. The conditions for sputtering film forming in this process are as follows.

[0069] During the sputtering film formation, the sputtering film formation device is evacuated until the ultimate vacuum degree in the film formation chamber reaches 0.9×10 -4After 0.2 Pa, krypton (Kr) as a sputtering gas (inert gas) and oxygen as a reactive gas are introduced into the film forming chamber, and the gas pressure in the film forming chamber is set to 0.2 Pa. The ratio of the amount of oxygen introduced into the film forming chamber to the total amount of sputtering gas (Kr) and oxygen introduced is set to about 3.1% flow rate. In addition, as a target, a sintered body of indium oxide and tin oxide (ITO with a tin oxide concentration of 10% by mass) is used. As a power source for applying voltage to the target, a DC power supply is used. The horizontal magnetic field strength on the target is set to 90mT. The film forming temperature (the temperature of the transparent substrate for stacking the transparent conductive layer) is set to 30°C.

[0070] As described above, a transparent conductive film of Example 1 was produced. The transparent conductive film of Example 1 includes a transparent substrate S with an easy-adhesion layer and a transparent conductive layer on the easy-adhesion layer. The transparent conductive layer is an ITO layer (thickness 125 nm) containing Kr.

[0071] [Example 2]

[0072] The transparent conductive film of Example 2 was prepared in the same manner as the transparent conductive film of Example 1 except for the following contents. In the transparent conductive layer forming step, a first layer with a thickness of 62.5 nm and a second layer with a thickness of 62.5 nm (second sputtering film forming) were sequentially formed on the easy-adhesive layer side of the transparent substrate S, forming a transparent conductive layer (thickness 125 nm). The conditions for the first sputtering film forming of the first layer were the same as the conditions for the sputtering film forming described above in Example 1. In the second sputtering film forming of the second layer, argon (Ar) was used as the sputtering gas, and the ratio of the oxygen introduced into the film forming chamber to the total introduction amount of the sputtering gas (Ar) and oxygen was set to about 3.1% flow rate. The other conditions for the second sputtering film forming were the same as the conditions for the sputtering film forming described above in Example 1.

[0073] The transparent conductive film of Example 2 comprises: a transparent substrate S and a transparent conductive layer on the easy-adhesion layer (the easy-adhesion layer is provided directly below the transparent conductive layer). The transparent conductive layer comprises, in order from the transparent substrate side, an ITO layer containing Kr (first layer) and an ITO layer containing Ar (second layer).

[0074] [Comparative Example 1]

[0075] The transparent conductive film of Comparative Example 1 was prepared in the same manner as the transparent conductive film of Example 1 except for the following contents. In the transparent conductive layer forming step, the transparent conductive layer was formed on the side of the long transparent substrate S on which the easy-adhesion layer was not formed. In addition, Ar was used as the sputtering gas, and the ratio of the amount of oxygen introduced into the film forming chamber to the total amount of the sputtering gas (Ar) and oxygen introduced was set to about 3.1% by flow.

[0076] The transparent conductive film of Comparative Example 1 includes a transparent substrate S and a transparent conductive layer (there is no easy-adhesion layer directly below the transparent conductive layer). The transparent conductive layer is an ITO layer (thickness 125 nm) containing Ar.

[0077] [Comparative Example 2]

[0078] A transparent conductive film of Comparative Example 2 was produced in the same manner as the transparent conductive film of Example 1 except for the following: In the transparent conductive layer forming step, a transparent conductive layer was formed on the surface of the long transparent substrate S on which the easily adhesive layer was not formed.

[0079] The transparent conductive film of Comparative Example 2 includes a transparent substrate S and a transparent conductive layer (there is no easy-adhesion layer directly below the transparent conductive layer). The transparent conductive layer is an ITO layer (thickness 125 nm) containing Kr.

[0080] [Comparative Example 3]

[0081] A transparent conductive film of Comparative Example 3 was prepared in the same manner as the transparent conductive film of Example 1 except for the following contents. In the transparent conductive layer formation step, Ar was used as the sputtering gas, and the ratio of the amount of oxygen introduced into the film forming chamber to the total amount of the sputtering gas (Ar) and oxygen introduced was set to about 3.1% by flow.

[0082] The transparent conductive film of Comparative Example 3 includes a transparent substrate S and a transparent conductive layer (with an easy-adhesion layer directly below the transparent conductive layer). The transparent conductive layer is an ITO layer (thickness 125 nm) containing Ar.

[0083] 〈Thickness of transparent conductive layer〉

[0084] The thickness of the transparent conductive layer of each transparent conductive film in Examples 1, 2 and Comparative Examples 1 to 3 was measured by observation using a field emission transmission electron microscope (FE-TEM). Specifically, first, a cross-sectional observation sample of each transparent conductive layer in Examples 1, 2 and Comparative Examples 1 to 3 was prepared by the FIB microsampling method. In the FIB microsampling method, a FIB device (product name "FB2200", manufactured by Hitachi) was used, and the acceleration voltage was set to 10 kV. Next, the cross section of the transparent conductive layer in the cross-sectional observation sample was observed using FE-TEM, and the thickness of the transparent conductive layer was measured in the observed image. In this observation, a FE-TEM device (product name "JEM-2800", manufactured by JEOL) was used, and the acceleration voltage was set to 200 kV.

[0085] 〈Crystallinity〉

[0086] The crystallinity of each transparent conductive layer in Examples 1 and 2 and Comparative Examples 1 to 3 was investigated as follows. Each transparent conductive layer in Examples 1 and 2 and Comparative Examples 1 and 2 was a crystalline film.

[0087] The transparent conductive layer in Comparative Example 3 is not a crystalline film.

[0088] First, the transparent conductive layer on the transparent substrate S is immersed in hydrochloric acid with a concentration of 5 mass % at 20° C. for 15 minutes. Then, the transparent conductive layer is washed with water and then dried. Next, on the exposed plane of the transparent conductive layer, the resistance between a pair of terminals separated by a distance of 15 mm (terminal resistance) is measured. In this measurement, when the terminal resistance is 10 kΩ or less, the transparent conductive layer is judged to be a crystalline film.

[0089] 〈Surface roughness〉

[0090] The roughness of the first surface (the surface on the transparent conductive layer side) of the transparent substrate was investigated for each transparent conductive film of Examples 1 and 2 and Comparative Examples 1 to 3. Specifically, in the manufacturing process of the transparent conductive film, the surface roughness Ra (arithmetic mean surface roughness based on JIS B 0601-2001) of the first surface of the transparent substrate before the transparent conductive layer formation step was obtained from a 1 μm square observation image obtained using an atomic force microscope (product name "Dimention-Edge SPM SYSTEM", manufactured by Bruker) . The surface roughness Ra (nm) of the transparent conductive layer is shown in Table 1.

[0091] 〈Sliding test〉

[0092] For each of the transparent conductive films of Examples 1 and 2 and Comparative Examples 1 to 3, the adhesion of the transparent conductive layer to the transparent substrate was investigated as follows.

[0093] First, a sample film (10 cm in MD direction × 5 cm in TD direction) was cut out from a transparent conductive film (transparent substrate / transparent conductive layer). Next, the transparent substrate side of the sample film was bonded to a glass plate via a strong double-sided tape. Next, the glass plate with the sample film was mounted on the table of a sliding tester (product name "10-link pen tester", manufactured by MTM). Next, a sliding test was performed on the transparent conductive layer of the sample film on the glass plate using the sliding tester. Specifically, after ethanol was dripped onto the transparent conductive layer of the sample film, the dripping portion was subjected to a reciprocating motion of a sliding piece (wipe) as a sliding member in the MD direction 400 times (alcohol sliding test) while the sliding piece was pressed with a load of 2 kg.

[0094] Then, during and after the sliding test, the transparent conductive layer of the sample film was observed using a laser microscope (product name "VK-X1000", manufactured by KEYENCE) to confirm whether the transparent conductive layer was peeled off. Regarding the adhesion of the transparent conductive layer to the transparent substrate, the case where no peeling of the transparent conductive layer was confirmed after the sliding test was evaluated as "excellent", the case where peeling of the transparent conductive layer was confirmed in a very small part after the sliding test was evaluated as "good", the case where peeling of the transparent conductive layer was not confirmed at the stage of 50 reciprocating movements, but peeling of the transparent conductive layer was confirmed on the entire surface after the sliding test (400 reciprocating movements) was evaluated as "poor", and the case where peeling of the transparent conductive layer was confirmed on the entire surface after 50 reciprocating movements was evaluated as "very poor".

[0095] Table 1 shows the evaluation results.

[0096] <Confirmation of Kr atoms in the transparent conductive layer>

[0097] The presence or absence of Kr atoms in each transparent conductive layer in Examples 1, 2 and Comparative Examples 1 to 3 was confirmed as follows. First, a scanning fluorescent X-ray analyzer (product name "ZSX PrimusIV", manufactured by Rigaku Corporation) was used to repeatedly perform fluorescent X-ray analysis measurements 5 times under the following measurement conditions, and the average value of each scanning angle was calculated to produce an X-ray spectrum. Then, by confirming the presence of a peak near a scanning angle of 28.2° in the produced X-ray spectrum, it was confirmed that Kr atoms were contained in the transparent conductive layer. In this way, it was confirmed that each transparent conductive layer in Examples 1, 2 and Comparative Example 2 contained Kr atoms and that each transparent conductive layer in Comparative Examples 1 and 3 did not contain Kr.

[0098] <Measurement conditions>

[0099] Spectrum; Kr-KA.

[0100] Measuring diameter: 30mm.

[0101] Atmosphere: Vacuum.

[0102] Target: Rh.

[0103] Tube voltage: 50kV.

[0104] Tube current: 60mA.

[0105] First order filter: Ni40.

[0106] Scanning angle (deg): 27.0~29.5.

[0107] Step(deg):0.020.

[0108] Speed ​​(deg / min): 0.75.

[0109] Attenuator:1 / 1.

[0110] Slit:S2.

[0111] Spectroscopic crystal: LiF(200).

[0112] Detector:SC.

[0113] PHA: 100-300.

[0114] [Table 1]

[0115]

[0116] It should be noted that the above invention is provided as an exemplary embodiment of the present invention, but it is only an example and is not to be construed as limiting. Modifications of the present invention that are clear to those skilled in the art are also included in the claims.

[0117] Industrial Applicability

[0118] The transparent conductive film of the present invention is preferably used in, for example, a foldable display panel.

Claims

1. A transparent conductive film comprising: a transparent substrate having a first surface and a second surface opposite to the first surface; and The transparent conductive layer on the first surface, wherein The first surface has a surface roughness Ra of 1.50 nm or more, The transparent conductive layer contains rare gas atoms having an atomic number greater than that of argon.

2. The transparent conductive film according to claim 1, wherein The rare gas atom is krypton.

3. The transparent conductive film according to claim 1, wherein The transparent conductive layer is a crystalline film.

4. The transparent conductive film according to claim 1, wherein The surface roughness Ra is less than 2.50 nm.

5. The transparent conductive film according to any one of claims 1 to 4, wherein The transparent substrate has an easy-adhesion layer forming the first surface, and the easy-adhesion layer has an average thickness of 50 nm or less.