Modified flame-retardant ETFE cable material and processing method thereof

By adding specific components to the ETFE cable material to form flame retardant and protective layers, the problems of low flame retardant performance and prone to spontaneous ignition are solved, significantly extending the service life and enhancing insect and rat-proof performance.

CN119008104APending Publication Date: 2024-11-22GUANGDONG YILIAN ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411164969.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional ETFE cable materials have low flame retardant properties and are prone to spontaneous combustion in high temperature environments for a long time, which reduces service life.

Method used

Using modified ETFE cable material, by adding flame retardant, insulating agent, shielding agent and protective agent to the cable material, including aluminum hydroxide, dimethyl methyl phosphate, antimony oxide, molybdenum oxide, tetrafluoroethylene monomer, Ethylene monomer, polyvinylamine, aluminum foil, polyester film, bifenthrin, cyclohexylamine and capsaicin, etc., form flame retardant layer and protective layer, improve the flame retardant efficiency of cable materials and insect and mouse prevention performance.

Benefits of technology

It effectively improves the flame retardant performance of cable materials, avoids spontaneous combustion, extends service life, and enhances insect and rat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008104A_ABST
    Figure CN119008104A_ABST
Patent Text Reader

Abstract

The invention discloses a modified flame-retardant ETFE cable material and a processing method thereof.The modified flame-retardant ETFE cable material comprises an ETFE cable material, the ETFE cable material comprises a flame retardant, modified ETFE resin, an insulating agent, a shielding agent and a protective agent, and the flame retardant is prepared from, by weight, 40-60 parts of aluminum hydroxide, 20-40 parts of dimethyl methylphosphate, 10-20 parts of antimony oxide and 10-20 parts of molybdenum oxide; the flame retardant, the aluminum hydroxide, the dimethyl methylphosphate, the antimony oxide and the molybdenum oxide are uniformly mixed and then coated on the outer side of the cable material, so that the flame-retardant efficiency of the outer side of the cable material is improved, the spontaneous combustion phenomenon of the ETFE cable material is avoided, and the service life of the ETFE cable material is prolonged; the protective agent is arranged, the bifenthrin is added, so that the insect resistance of the ETFE cable material is improved, the cyclohexanephthalein amine and the capsaicin are added, the rat resistance of the ETFE cable material is improved, the phenomenon that the ETFE cable material is bitten by insects and rats is avoided, and the service life of the ETFE cable material is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ETFE cable materials, in particular to a modified flame-retardant ETFE cable material and a processing method thereof. Background Art

[0002] ETFE cable materials are mainly used to make corrosion-resistant parts, wear-resistant parts, seals, insulating parts and medical device parts, as well as wires, cable insulation layers, anti-corrosion equipment, sealing materials, pump valve bushings and chemical containers. ETFE ethylene-tetrafluoroethylene copolymer cable materials have a wide range of applications, mainly due to their excellent physical and chemical properties. Specifically, the characteristics of ETFE cable materials include: ETFE materials can resist corrosion from a variety of chemical substances, including strong acids, strong alkalis and other corrosive media, so they are very suitable for making anti-corrosion equipment and chemical containers; ETFE cable materials can maintain stable physical properties in high temperature environments, and their continuous working temperature range is from -65°C to +200°C, and they can withstand 300°C high-temperature cross-linking experiments, showing good high-temperature resistance; ETFE cable materials have good electrical insulation properties and are suitable as insulating layers for wires and cables to ensure the safe operation of electrical equipment; ETFE materials are easy to process and can be processed by various methods such as extrusion molding, making them suitable for large-scale production and application; in addition, ETFE cable materials are also widely used in industrial and agricultural building films, showing their application potential in the construction field. In summary, ETFE cable materials, due to their unique physical and chemical properties, play an important role in many fields, from industrial applications to the construction field, to medical equipment manufacturing, all of which reflect their wide application value and importance.

[0003] However, traditional ETFE cable materials have the following disadvantages:

[0004] Traditional ETFE cable materials have low flame retardancy. ETFE cable materials are prone to spontaneous combustion when operating in high temperature environments for a long time, which reduces the service life of ETFE cable materials. Summary of the invention

[0005] The purpose of the present invention is to provide a modified flame-retardant ETFE cable material and a processing method thereof, so as to solve the problems mentioned in the above background technology that the traditional ETFE cable material has low flame retardancy, the ETFE cable material is operated in a high temperature environment for a long time, the ETFE cable material is prone to spontaneous combustion, and the service life of the ETFE cable material is reduced.

[0006] To achieve the above object, the present invention provides the following technical scheme: a modified flame-retardant ETFE cable material, comprising an ETFE cable material, wherein the ETFE cable material comprises a flame retardant, a modified ETFE resin, an insulating agent, a shielding agent and a protective agent, wherein the flame retardant comprises the following components: by weight, 40 to 60 parts of aluminum hydroxide, 20 to 40 parts of dimethyl methyl phosphate, 10 to 20 parts of antimony oxide and 10 to 20 parts of molybdenum oxide, and the modified ETFE resin comprises the following components: by weight, 40 to 60 parts of tetrafluoroethylene monomer, 20 to 40 parts of ethylene monomer, and 10 to 20 parts of tetrafluoroethylene monomer. The insulating agent comprises the following components: by weight, 30-50 parts of polyethylene amine, 30-40 parts of polyolefin and 30-40 parts of fluorinated hydrocarbons; the shielding agent comprises the following components: by weight, 40-60 parts of aluminum foil and 40-60 parts of polyester film; the protective agent comprises the following components: by weight, 40-60 parts of polyimide film, 20-40 parts of bifenthrin, 10-20 parts of cyclohexylphthalamide and 10-20 parts of capsaicin.

[0007] As a preferred technical solution of the present invention, the flame retardant comprises the following components: 40 parts by weight of aluminum hydroxide, 40 parts by weight of dimethyl methyl phosphate, 10 parts by weight of antimony oxide and 10 parts by weight of molybdenum oxide; the modified ETFE resin comprises the following components: 50 parts by weight of tetrafluoroethylene monomer, 30 parts by weight of ethylene monomer and 20 parts by weight of allyl compound; the insulating agent comprises the following components: 30 parts by weight of polyethylene amine, 40 parts by weight of polyolefin and 30 parts by weight of fluorinated hydrocarbon; the shielding agent comprises the following components: 45 parts by weight of aluminum foil and 55 parts by weight of polyester film; the protective agent comprises the following components: 50 parts by weight of polyimide film, 20 parts by weight of bifenthrin, 15 parts by weight of cyclohexylphthalamide and 15 parts by weight of capsaicin.

[0008] As a preferred technical solution of the present invention, the flame retardant comprises the following components: 50 parts by weight of aluminum hydroxide, 20 parts by weight of dimethyl methyl phosphate, 20 parts by weight of antimony oxide and 10 parts by weight of molybdenum oxide; the modified ETFE resin comprises the following components: 40 parts by weight of tetrafluoroethylene monomer, 50 parts by weight of ethylene monomer and 10 parts by weight of allyl compound; the insulating agent comprises the following components: 30 parts by weight of polyethylene amine, 30 parts by weight of polyolefin and 40 parts by weight of fluorinated hydrocarbon; the shielding agent comprises the following components: 50 parts by weight of aluminum foil and 50 parts by weight of polyester film; the protective agent comprises the following components: 50 parts by weight of polyimide film, 30 parts by weight of bifenthrin, 10 parts by weight of cyclohexylphthalamide and 10 parts by weight of capsaicin.

[0009] As a preferred technical solution of the present invention, the flame retardant comprises the following components: 50 parts by weight of aluminum hydroxide, 20 parts by weight of dimethyl methyl phosphate, 10 parts by weight of antimony oxide and 20 parts by weight of molybdenum oxide; the modified ETFE resin comprises the following components: 40 parts by weight of tetrafluoroethylene monomer, 40 parts by weight of ethylene monomer and 20 parts by weight of allyl compound; the insulating agent comprises the following components: 40 parts by weight of polyethylene amine, 30 parts by weight of polyolefin and 30 parts by weight of fluorinated hydrocarbon; the shielding agent comprises the following components: 60 parts by weight of aluminum foil and 40 parts by weight of polyester film; the protective agent comprises the following components: 40 parts by weight of polyimide film, 40 parts by weight of bifenthrin, 10 parts by weight of cyclohexylphthalamide and 10 parts by weight of capsaicin.

[0010] As a preferred technical solution of the present invention, the flame retardant comprises the following components: 60 parts by weight of aluminum hydroxide, 20 parts by weight of dimethyl methyl phosphate, 10 parts by weight of antimony oxide and 10 parts by weight of molybdenum oxide; the modified ETFE resin comprises the following components: 50 parts by weight of tetrafluoroethylene monomer, 30 parts by weight of ethylene monomer and 20 parts by weight of allyl compound; the insulating agent comprises the following components: 30 parts by weight of polyethylene amine, 35 parts by weight of polyolefin and 35 parts by weight of fluorinated hydrocarbon; the shielding agent comprises the following components: 40 parts by weight of aluminum foil and 60 parts by weight of polyester film; the protective agent comprises the following components: 40 parts by weight of polyimide film, 20 parts by weight of bifenthrin, 20 parts by weight of cyclohexylphthalamide and 20 parts by weight of capsaicin.

[0011] The present invention discloses a method for processing a modified flame-retardant ETFE cable material, comprising the following steps:

[0012] Step 1: Prepare the guide core: twist a plurality of modified ETFE resins to form a guide core, and use an extruder to extrude the guide core to make it compact;

[0013] Step 2: preparing an insulating layer: covering the outer side of the prepared conductor core with an insulating agent to form an insulating layer;

[0014] Step 3: preparing a shielding layer: covering the outer side of the prepared insulating layer with a shielding agent to form a shielding layer;

[0015] Step 4: preparing a flame retardant layer: covering the outer side of the prepared shielding layer with a flame retardant to form a flame retardant layer;

[0016] Step 5: Prepare a protective layer: Cover the protective agent on the outside of the prepared flame retardant layer to form a protective layer.

[0017] As a preferred technical solution of the present invention, the specific process of preparing the modified ETFE resin in step 1 is to twist 40-60 parts of tetrafluoroethylene monomer, 30-50 parts of ethylene monomer and 10-20 parts of allyl compound into one strand through a twister, and then compact it through an extruder.

[0018] As a preferred technical solution of the present invention, the specific process of preparing the insulating agent in the step 2 is to put 30-60 parts of polyethylene amine, 30-40 parts of polyolefin and 30-40 parts of fluorinated hydrocarbons into the reactor in sequence and mix them evenly. The specific process of preparing the shielding agent in the step 3 is to bond 40-60 parts of aluminum foil and 40-60 parts of polyester film in sequence together. The specific process of preparing the flame retardant in the step 4 is to put 40-60 parts of aluminum hydroxide, 20-40 parts of dimethyl methyl phosphate, 10-20 parts of antimony oxide and 10-20 parts of molybdenum oxide in sequence into the reactor and mix them evenly. The specific process of preparing the protective agent in the step 5 is to put 20-40 parts of bifenthrin, 10-20 parts of cyclohexylphthalamide and 10-20 parts of capsaicin in sequence into the reactor, mix them evenly and bond them to one side of 40-60 parts of polyimide film.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. By setting the flame retardant, aluminum hydroxide, dimethyl methyl phosphate, antimony oxide and molybdenum oxide are evenly mixed and coated on the outside of the cable material, the flame retardant efficiency of the outer side of the cable material itself is improved, the spontaneous combustion of ETFE cable material is avoided, and the service life of ETFE cable material is extended;

[0021] 2. By setting the protective agent, the addition of bifenthrin improves the insect resistance of ETFE cable materials, and the addition of cyclohexylphthalamide and capsaicin improves the rodent resistance of ETFE cable materials, avoiding the phenomenon of ETFE cable materials being bitten by insects and rodents, and extending the service life of ETFE cable materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Embodiment 1:

[0025] See also Figure 1 The present invention provides a modified flame-retardant ETFE cable material, comprising an ETFE cable material, wherein the ETFE cable material comprises a flame retardant, a modified ETFE resin, an insulating agent, a shielding agent and a protective agent, wherein the flame retardant comprises the following components: by weight, 40 to 60 parts of aluminum hydroxide, 20 to 40 parts of dimethyl methyl phosphate, 10 to 20 parts of antimony oxide and 10 to 20 parts of molybdenum oxide, and the modified ETFE resin comprises the following components: by weight, 40 to 60 parts of tetrafluoroethylene monomer, 30 to 50 parts of ethylene monomer parts and 10-20 parts of allyl compounds, the insulating agent comprises the following components: by weight, 30-60 parts of polyethylene amine, 30-40 parts of polyolefin and 30-40 parts of fluorinated hydrocarbons, the shielding agent comprises the following components: by weight, 40-60 parts of aluminum foil and 40-60 parts of polyester film, and the protective agent comprises the following components: by weight, 40-60 parts of polyimide film, 20-40 parts of bifenthrin, 10-20 parts of cyclohexylphthalamide and 10-20 parts of capsaicin.

[0026] The present invention discloses a method for processing a modified flame-retardant ETFE cable material, comprising the following steps:

[0027] Step 1: Prepare the guide core: twist a plurality of modified ETFE resins to form a guide core, and use an extruder to extrude the guide core to make it compact;

[0028] Step 2: preparing an insulating layer: covering the outer side of the prepared conductor core with an insulating agent to form an insulating layer;

[0029] Step 3: preparing a shielding layer: covering the outer side of the prepared insulating layer with a shielding agent to form a shielding layer;

[0030] Step 4: preparing a flame retardant layer: covering the outer side of the prepared shielding layer with a flame retardant to form a flame retardant layer;

[0031] Step 5: Prepare a protective layer: Cover the protective agent on the outside of the prepared flame retardant layer to form a protective layer.

[0032] The specific process of preparing the modified ETFE resin in step 1 is to twist 40-60 parts of tetrafluoroethylene monomer, 30-50 parts of ethylene monomer and 10-20 parts of allyl compound into one strand through a twister, and then compress it through an extruder.

[0033] The specific process of preparing the insulating agent in step 2 is to put 30-60 parts of polyethylene amine, 30-40 parts of polyolefin and 30-40 parts of fluorinated hydrocarbons into the reactor in sequence and mix them evenly. The specific process of preparing the shielding agent in step 3 is to bond 40-60 parts of aluminum foil and 40-60 parts of polyester film in sequence together. The specific process of preparing the flame retardant in step 4 is to put 40-60 parts of aluminum hydroxide, 20-40 parts of dimethyl methyl phosphate, 10-20 parts of antimony oxide and 10-20 parts of molybdenum oxide in sequence into the reactor and mix them evenly. The specific process of preparing the protective agent in step 5 is to put 20-40 parts of bifenthrin, 10-20 parts of cyclohexylphthalamide and 10-20 parts of capsaicin in sequence into the reactor, mix them evenly and bond them to one side of 40-60 parts of polyimide film.

[0034] Embodiment 2:

[0035] See also Figure 1 The invention provides a modified flame-retardant ETFE cable material, comprising an ETFE cable material, wherein the ETFE cable material comprises a flame retardant, a modified ETFE resin, an insulating agent, a shielding agent and a protective agent, wherein the flame retardant comprises the following components: by weight, 40 parts of aluminum hydroxide, 40 parts of dimethyl methyl phosphate, 10 parts of antimony oxide and 10 parts of molybdenum oxide, the modified ETFE resin comprises the following components: by weight, 50 parts of tetrafluoroethylene monomer, 30 parts of ethylene monomer and 20 parts of allyl compound, the insulating agent comprises the following components: by weight, 30 parts of polyethylene amine, 40 parts of polyolefin and 30 parts of fluorinated hydrocarbon, the shielding agent comprises the following components: by weight, 45 parts of aluminum foil and 55 parts of polyester film, and the protective agent comprises the following components: by weight, 50 parts of polyimide film, 20 parts of bifenthrin, 15 parts of cyclohexylphthalamide and 15 parts of capsaicin.

[0036] The present invention discloses a method for processing a modified flame-retardant ETFE cable material, comprising the following steps:

[0037] Step 1: Prepare the guide core: twist a plurality of modified ETFE resins to form a guide core, and use an extruder to extrude the guide core to make it compact;

[0038] Step 2: preparing an insulating layer: covering the outer side of the prepared conductor core with an insulating agent to form an insulating layer;

[0039] Step 3: preparing a shielding layer: covering the outer side of the prepared insulating layer with a shielding agent to form a shielding layer;

[0040] Step 4: preparing a flame retardant layer: covering the outer side of the prepared shielding layer with a flame retardant to form a flame retardant layer;

[0041] Step 5: Prepare a protective layer: Cover the protective agent on the outside of the prepared flame retardant layer to form a protective layer.

[0042] The specific process of preparing the modified ETFE resin in step 1 is to twist 50 parts of tetrafluoroethylene monomer, 30 parts of ethylene monomer and 20 parts of allyl compound into one strand through a twister, and then compress it through an extruder.

[0043] The specific process of preparing the insulating agent in step 2 is to put 30 parts of polyethylene amine, 40 parts of polyolefin and 30 parts of fluorinated hydrocarbons into the reactor in sequence and mix them evenly. The specific process of preparing the shielding agent in step 3 is to bond 45 parts of aluminum foil and 55 parts of polyester film together in sequence. The specific process of preparing the flame retardant in step 4 is to put 40 parts of aluminum hydroxide, 40 parts of dimethyl methyl phosphate, 10 parts of antimony oxide and 10 parts of molybdenum oxide into the reactor in sequence and mix them evenly. The specific process of preparing the protective agent in step 5 is to put 20 parts of cypermethrin, 15 parts of cyclohexylphthalamide and 15 parts of capsaicin into the reactor in sequence, mix them evenly and bond them to one side of 50 parts of polyimide film.

[0044] Embodiment 3:

[0045] See also Figure 1 The invention provides a modified flame-retardant ETFE cable material, comprising an ETFE cable material, wherein the ETFE cable material comprises a flame retardant, a modified ETFE resin, an insulating agent, a shielding agent and a protective agent, wherein the flame retardant comprises the following components: by weight, 50 parts of aluminum hydroxide, 20 parts of dimethyl methyl phosphate, 20 parts of antimony oxide and 10 parts of molybdenum oxide, the modified ETFE resin comprises the following components: by weight, 40 parts of tetrafluoroethylene monomer, 50 parts of ethylene monomer and 10 parts of allyl compound, the insulating agent comprises the following components: by weight, 30 parts of polyethylene amine, 30 parts of polyolefin and 40 parts of fluorinated hydrocarbon, the shielding agent comprises the following components: by weight, 50 parts of aluminum foil and 50 parts of polyester film, and the protective agent comprises the following components: by weight, 50 parts of polyimide film, 30 parts of bifenthrin, 10 parts of cyclohexylphthalamide and 10 parts of capsaicin.

[0046] The present invention discloses a method for processing a modified flame-retardant ETFE cable material, comprising the following steps:

[0047] Step 1: Prepare the guide core: twist a plurality of modified ETFE resins to form a guide core, and use an extruder to extrude the guide core to make it compact;

[0048] Step 2: preparing an insulating layer: covering the outer side of the prepared conductor core with an insulating agent to form an insulating layer;

[0049] Step 3: preparing a shielding layer: covering the outer side of the prepared insulating layer with a shielding agent to form a shielding layer;

[0050] Step 4: preparing a flame retardant layer: covering the outer side of the prepared shielding layer with a flame retardant to form a flame retardant layer;

[0051] Step 5: Prepare a protective layer: Cover the protective agent on the outside of the prepared flame retardant layer to form a protective layer.

[0052] The specific process of preparing the modified ETFE resin in step 1 is to twist 40 parts of tetrafluoroethylene monomer, 50 parts of ethylene monomer and 10 parts of allyl compound into one strand through a twister, and then compress it through an extruder.

[0053] The specific process of preparing the insulating agent in step 2 is to put 30 parts of polyethylene amine, 30 parts of polyolefin and 40 parts of fluorinated hydrocarbons into the reactor in sequence and mix them evenly. The specific process of preparing the shielding agent in step 3 is to bond 50 parts of aluminum foil and 50 parts of polyester film together in sequence. The specific process of preparing the flame retardant in step 4 is to put 50 parts of aluminum hydroxide, 20 parts of dimethyl methyl phosphate, 20 parts of antimony oxide and 10 parts of molybdenum oxide into the reactor in sequence and mix them evenly. The specific process of preparing the protective agent in step 5 is to put 30 parts of cypermethrin, 10 parts of cyclohexylphthalamide and 10 parts of capsaicin into the reactor in sequence, mix them evenly and bond them to one side of 50 parts of polyimide film.

[0054] Embodiment 4:

[0055] See also Figure 1 The invention provides a modified flame-retardant ETFE cable material, comprising an ETFE cable material, wherein the ETFE cable material comprises a flame retardant, a modified ETFE resin, an insulating agent, a shielding agent and a protective agent, wherein the flame retardant comprises the following components: by weight, 50 parts of aluminum hydroxide, 20 parts of dimethyl methyl phosphate, 10 parts of antimony oxide and 20 parts of molybdenum oxide, the modified ETFE resin comprises the following components: by weight, 40 parts of tetrafluoroethylene monomer, 40 parts of ethylene monomer and 20 parts of allyl compound, the insulating agent comprises the following components: by weight, 40 parts of polyethylene amine, 30 parts of polyolefin and 30 parts of fluorinated hydrocarbon, the shielding agent comprises the following components: by weight, 60 parts of aluminum foil and 40 parts of polyester film, and the protective agent comprises the following components: by weight, 40 parts of polyimide film, 40 parts of bifenthrin, 10 parts of cyclohexylphthalamide and 10 parts of capsaicin.

[0056] The present invention discloses a method for processing a modified flame-retardant ETFE cable material, comprising the following steps:

[0057] Step 1: Prepare the guide core: twist a plurality of modified ETFE resins to form a guide core, and use an extruder to extrude the guide core to make it compact;

[0058] Step 2: preparing an insulating layer: covering the outer side of the prepared conductor core with an insulating agent to form an insulating layer;

[0059] Step 3: preparing a shielding layer: covering the outer side of the prepared insulating layer with a shielding agent to form a shielding layer;

[0060] Step 4: preparing a flame retardant layer: covering the outer side of the prepared shielding layer with a flame retardant to form a flame retardant layer;

[0061] Step 5: Prepare a protective layer: Cover the protective agent on the outside of the prepared flame retardant layer to form a protective layer.

[0062] The specific process of preparing the modified ETFE resin in step 1 is to twist 40 parts of tetrafluoroethylene monomer, 40 parts of ethylene monomer and 20 parts of allyl compound into one strand through a twister, and then compress it through an extruder.

[0063] The specific process of preparing the insulating agent in step 2 is to put 40 parts of polyethylene amine, 30 parts of polyolefin and 30 parts of fluorinated hydrocarbons into the reactor in sequence and mix them evenly. The specific process of preparing the shielding agent in step 3 is to bond 45 parts of aluminum foil and 55 parts of polyester film together in sequence. The specific process of preparing the flame retardant in step 4 is to put 50 parts of aluminum hydroxide, 20 parts of dimethyl methyl phosphate, 10 parts of antimony oxide and 20 parts of molybdenum oxide into the reactor in sequence and mix them evenly. The specific process of preparing the protective agent in step 5 is to put 40 parts of cypermethrin, 10 parts of cyclohexylphthalamide and 10 parts of capsaicin into the reactor in sequence, mix them evenly and bond them to one side of 40 parts of polyimide film.

[0064] Embodiment 5:

[0065] See also Figure 1 The invention provides a modified flame-retardant ETFE cable material, comprising an ETFE cable material, wherein the ETFE cable material comprises a flame retardant, a modified ETFE resin, an insulating agent, a shielding agent and a protective agent, wherein the flame retardant comprises the following components: by weight, 60 parts of aluminum hydroxide, 20 parts of dimethyl methyl phosphate, 10 parts of antimony oxide and 10 parts of molybdenum oxide, the modified ETFE resin comprises the following components: by weight, 50 parts of tetrafluoroethylene monomer, 30 parts of ethylene monomer and 20 parts of allyl compound, the insulating agent comprises the following components: by weight, 30 parts of polyethylene amine, 35 parts of polyolefin and 35 parts of fluorinated hydrocarbon, the shielding agent comprises the following components: by weight, 40 parts of aluminum foil and 60 parts of polyester film, and the protective agent comprises the following components: by weight, 40 parts of polyimide film, 20 parts of bifenthrin, 20 parts of cyclohexylphthalamide and 20 parts of capsaicin.

[0066] The present invention discloses a method for processing a modified flame-retardant ETFE cable material, comprising the following steps:

[0067] Step 1: Prepare the guide core: twist a plurality of modified ETFE resins to form a guide core, and use an extruder to extrude the guide core to make it compact;

[0068] Step 2: preparing an insulating layer: covering the outer side of the prepared conductor core with an insulating agent to form an insulating layer;

[0069] Step 3: preparing a shielding layer: covering the outer side of the prepared insulating layer with a shielding agent to form a shielding layer;

[0070] Step 4: preparing a flame retardant layer: covering the outer side of the prepared shielding layer with a flame retardant to form a flame retardant layer;

[0071] Step 5: Prepare a protective layer: Cover the protective agent on the outside of the prepared flame retardant layer to form a protective layer.

[0072] The specific process of preparing the modified ETFE resin in step 1 is to twist 50 parts of tetrafluoroethylene monomer, 30 parts of ethylene monomer and 20 parts of allyl compound into one strand through a twister, and then compress it through an extruder.

[0073] The specific process of preparing the insulating agent in step 2 is to put 30 parts of polyethylene amine, 35 parts of polyolefin and 35 parts of fluorinated hydrocarbons into the reactor in sequence and mix them evenly. The specific process of preparing the shielding agent in step 3 is to bond 40 parts of aluminum foil and 60 parts of polyester film together in sequence. The specific process of preparing the flame retardant in step 4 is to put 60 parts of aluminum hydroxide, 20 parts of dimethyl methyl phosphate, 10 parts of antimony oxide and 10 parts of molybdenum oxide into the reactor in sequence and mix them evenly. The specific process of preparing the protective agent in step 5 is to put 20 parts of cypermethrin, 20 parts of cyclohexylphthalamide and 20 parts of capsaicin into the reactor in sequence, mix them evenly and bond them to one side of 40 parts of polyimide film.

[0074] In the present invention, 40 to 60 parts of tetrafluoroethylene monomer, 30 to 50 parts of ethylene monomer and 10 to 20 parts of allyl compound are twisted into a strand by a twisting machine, and the strands are pressed by an extruder, and a plurality of modified ETFE resins are twisted to form a conductor core, and the conductor core is extruded by an extruder to make it compact; 30 to 60 parts of polyvinyl amine, 30 to 40 parts of polyolefin and 30 to 40 parts of fluorinated hydrocarbon are sequentially put into a reaction kettle and mixed evenly, and an insulating agent is covered on the outer side of the prepared conductor core to form an insulating layer; 40 to 60 parts of aluminum foil and 40 to 60 parts of polyester film are sequentially bonded on Together, a shielding agent is covered on the outside of the prepared insulating layer to form a shielding layer; 40-60 parts of aluminum hydroxide, 20-40 parts of dimethyl methyl phosphate, 10-20 parts of antimony oxide and 10-20 parts of molybdenum oxide are put into a reactor in sequence and mixed evenly, and a flame retardant is covered on the outside of the prepared shielding layer to form a flame retardant layer; 20-40 parts of cypermethrin, 10-20 parts of cyclohexylphthalamide and 10-20 parts of capsaicin are put into a reactor in sequence, mixed evenly and bonded to one side of 40-60 parts of a polyimide film, and a protective agent is covered on the outside of the prepared flame retardant layer to form a protective layer.

[0075] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A modified flame-retardant ETFE cable material, comprising an ETFE cable material, characterized in that: The ETFE cable material comprises a flame retardant, a modified ETFE resin, an insulating agent, a shielding agent and a protective agent. The flame retardant comprises the following components: by weight, 40-60 parts of aluminum hydroxide, 20-40 parts of dimethyl methyl phosphate, 10-20 parts of antimony oxide and 10-20 parts of molybdenum oxide. The modified ETFE resin comprises the following components: by weight, 40-60 parts of tetrafluoroethylene monomer, 30-50 parts of ethylene monomer and 10-20 parts of allyl compound. The insulating agent comprises the following components: 30-60 parts of polyethylene amine, 30-40 parts of polyolefin and 30-40 parts of fluorinated hydrocarbons, the shielding agent comprises the following components: 40-60 parts of aluminum foil and 40-60 parts of polyester film, and the protective agent comprises the following components: 40-60 parts of polyimide film, 20-40 parts of bifenthrin, 10-20 parts of cyclohexylphthalamide and 10-20 parts of capsaicin, by weight.

2. A modified flame-retardant ETFE cable material according to claim 1, characterized in that: The flame retardant comprises the following components: 40 parts of aluminum hydroxide, 40 parts of dimethyl methyl phosphate, 10 parts of antimony oxide and 10 parts of molybdenum oxide, by weight; the modified ETFE resin comprises the following components: 50 parts of tetrafluoroethylene monomer, 30 parts of ethylene monomer and 20 parts of allyl compound, by weight; the insulating agent comprises the following components: 30 parts of polyethylene amine, 40 parts of polyolefin and 30 parts of fluorinated hydrocarbon, by weight; the shielding agent comprises the following components: 45 parts of aluminum foil and 55 parts of polyester film, by weight; the protective agent comprises the following components: 50 parts of polyimide film, 20 parts of bifenthrin, 15 parts of cyclohexylphthalamide and 15 parts of capsaicin, by weight.

3. A modified flame-retardant ETFE cable material according to claim 1, characterized in that: The flame retardant comprises the following components: 50 parts of aluminum hydroxide, 20 parts of dimethyl methyl phosphate, 20 parts of antimony oxide and 10 parts of molybdenum oxide, by weight; the modified ETFE resin comprises the following components: 40 parts of tetrafluoroethylene monomer, 50 parts of ethylene monomer and 10 parts of allyl compound, by weight; the insulating agent comprises the following components: 30 parts of polyethylene amine, 30 parts of polyolefin and 40 parts of fluorinated hydrocarbon, by weight; the shielding agent comprises the following components: 50 parts of aluminum foil and 50 parts of polyester film, by weight; the protective agent comprises the following components: 50 parts of polyimide film, 30 parts of bifenthrin, 10 parts of cyclohexylphthalamide and 10 parts of capsaicin, by weight.

4. A modified flame-retardant ETFE cable material according to claim 1, characterized in that: The flame retardant comprises the following components: 50 parts of aluminum hydroxide, 20 parts of dimethyl methyl phosphate, 10 parts of antimony oxide and 20 parts of molybdenum oxide, by weight; the modified ETFE resin comprises the following components: 40 parts of tetrafluoroethylene monomer, 40 parts of ethylene monomer and 20 parts of allyl compound, by weight; the insulating agent comprises the following components: 40 parts of polyethylene amine, 30 parts of polyolefin and 30 parts of fluorinated hydrocarbon, by weight; the shielding agent comprises the following components: 60 parts of aluminum foil and 40 parts of polyester film, by weight; the protective agent comprises the following components: 40 parts of polyimide film, 40 parts of bifenthrin, 10 parts of cyclohexylphthalamide and 10 parts of capsaicin, by weight.

5. The modified flame-retardant ETFE cable material according to claim 1, characterized in that: The flame retardant comprises the following components: 60 parts of aluminum hydroxide, 20 parts of dimethyl methyl phosphate, 10 parts of antimony oxide and 10 parts of molybdenum oxide, by weight; the modified ETFE resin comprises the following components: 50 parts of tetrafluoroethylene monomer, 30 parts of ethylene monomer and 20 parts of allyl compound, by weight; the insulating agent comprises the following components: 30 parts of polyethylene amine, 35 parts of polyolefin and 35 parts of fluorinated hydrocarbon, by weight; the shielding agent comprises the following components: 40 parts of aluminum foil and 60 parts of polyester film, by weight; the protective agent comprises the following components: 40 parts of polyimide film, 20 parts of bifenthrin, 20 parts of cyclohexylphthalamide and 20 parts of capsaicin, by weight.

6. A method for processing a modified flame-retardant ETFE cable material according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1: Prepare the guide core: twist a plurality of modified ETFE resins to form a guide core, and use an extruder to extrude the guide core to make it compact; Step 2: preparing an insulating layer: covering the outer side of the prepared conductor core with an insulating agent to form an insulating layer; Step 3: preparing a shielding layer: covering the outer side of the prepared insulating layer with a shielding agent to form a shielding layer; Step 4: preparing a flame retardant layer: covering the outer side of the prepared shielding layer with a flame retardant to form a flame retardant layer; Step 5: Prepare a protective layer: Cover the protective agent on the outside of the prepared flame retardant layer to form a protective layer.

7. A method for processing a modified flame-retardant ETFE cable material according to claim 6, characterized in that: The specific process of preparing the modified ETFE resin in step 1 is to twist 40-60 parts of tetrafluoroethylene monomer, 30-50 parts of ethylene monomer and 10-20 parts of allyl compound into one strand through a twister, and then compress it through an extruder.

8. The method for processing a modified flame-retardant ETFE cable material according to claim 6, characterized in that: The specific process of preparing the insulating agent in the step 2 is to put 30-60 parts of polyethylene amine, 30-40 parts of polyolefin and 30-40 parts of fluorinated hydrocarbons into the reactor in sequence and mix them evenly; the specific process of preparing the shielding agent in the step 3 is to bond 40-60 parts of aluminum foil and 40-60 parts of polyester film in sequence; the specific process of preparing the flame retardant in the step 4 is to put 40-60 parts of aluminum hydroxide, 20-40 parts of dimethyl methyl phosphate, 10-20 parts of antimony oxide and 10-20 parts of molybdenum oxide in sequence into the reactor and mix them evenly; the specific process of preparing the protective agent in the step 5 is to put 20-40 parts of bifenthrin, 10-20 parts of cyclohexylphthalamide and 10-20 parts of capsaicin in sequence into the reactor, mix them evenly and bond them to one side of 40-60 parts of polyimide film.