Manufacturing process of far infrared mica tube
By using a process of mixing ceramic powder adhesive and modified polyester resin in mica tubes, the problem of difficult bonding between ceramic powder and mica paper was solved, and a high-strength far-infrared mica tube with good insulation properties was prepared, which is suitable for electrical insulation.
Patent Information
- Application Number
- CN202411278229.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-22
AI Technical Summary
Existing mica tubes are difficult to bond effectively with mica paper after the addition of ceramic powder, and are prone to delamination, resulting in a decrease in mechanical strength and insulation performance.
A resin-ceramic powder adhesive, comprising silicone-modified polyester resin and ceramic powder, is used to prepare far-infrared mica tubes through impregnation, drying, and rolling processes. Phenylalkoxysilane and aminosilane are used to improve the dispersibility and compatibility of the ceramic powder and enhance the interlayer bonding force.
The prepared far-infrared mica tube has a smooth surface, high strength and good insulation properties, can withstand high temperature, and has no delamination between layers, making it suitable for electrical insulation.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of mica tubes, and in particular to a manufacturing process of far-infrared mica tubes. Background Art
[0002] Mica tubes are divided into two categories based on the different binders. One is to dip a single mica paper into a resin binder, dry it to remove the solvent, roll it into shape, and then put it into an oven for curing. The other is to apply an inorganic binder on a single mica paper, dry it, roll it into shape, and then put it into an oven for curing. Mica tubes have high mechanical strength and are suitable for various motors and electrical appliances.
[0003] Mica tubes are used in hair dryers because some people have oily scalps. Adding ceramic powder to mica tubes can effectively control oil, improve the environment of hair follicles, and promote hair growth. However, ceramic powder is insoluble in glue and has poor compatibility with paper. Mica paper is not easy to roll and is prone to delamination, so it is difficult to combine ceramic powder and mica tubes, so there is room for improvement. Summary of the invention
[0004] In order to improve the bonding performance of mica tubes and ceramic powders, the present application provides a far-infrared mica tube manufacturing process.
[0005] The far-infrared mica tube manufacturing process provided in this application adopts the following technical solution: A far-infrared mica tube manufacturing process comprises the following steps: (1) beating mica ore powder to prepare mica paper for standby use; (2) preparing resin mixed with ceramic powder glue for standby use; (3) dipping the mica paper into a resin-mixed ceramic powder glue, and drying to obtain the ceramic powder mica paper; (4) Wipe the winding core clean, apply a release agent on the winding core, and roll the ceramic powder mica paper on the winding core to obtain a ceramic powder mica tube; (5) After the ceramic powder mica tube is baked and solidified, it is processed into a desired size and shape to obtain a far-infrared mica tube.
[0006] The far-infrared mica tube prepared by the above steps has a smooth surface, good strength, no delamination between layers, can be rolled into mica tubes with different wall thicknesses, and can be processed into different lengths and shapes as needed. It can be used in electrical insulation, has high strength and good insulation performance, can withstand high temperatures, and has good stability.
[0007] Preferably, the resin-mixed ceramic powder glue in step (2) comprises the following components in percentage by weight: 45%-55% of organosilicon-modified polyester resin, 20%-25% of methanol, 20%-25% of isopropanol, 0.8%-1.2% of curing agent, and 15%-17% of ceramic powder.
[0008] The resin mixed ceramic powder glue configured according to the above formula has good dispersibility and adhesion properties, which can improve the dispersibility of ceramic powder in glue, reduce the agglomeration and sinking of ceramic powder, and make the ceramic powder evenly distributed on the mica paper during the dipping process, thereby improving the bonding force between the ceramic powder and mica paper; the good adhesion and curing properties of the resin mixed ceramic powder glue improve the stability of the mica tube and reduce the occurrence of stratification of the mica tube. The prepared far-infrared mica tube has high strength and good insulation properties.
[0009] Preferably, the raw materials for preparing the organosilicon-modified polyester resin include phenylalkoxysilane and carboxyl polyester.
[0010] Organosilicon-modified polyester resin is obtained by modifying carboxyl polyester with phenylalkoxysilane. Phenylalkoxysilane can improve the weather resistance, heat resistance and strength of polyester resin, reduce the curing temperature of polyester, and shorten the curing time, so that the advantages of organosilicon and polyester resin complement each other. The introduction of organosilicon groups makes the polymer surface have stable siloxane bonds, which can interact with a variety of surface groups, enhance the interlayer bonding force of mica tubes through electrostatic interaction, van der Waals force, etc., and reduce the occurrence of stratification.
[0011] Preferably, the raw materials for preparing the phenylalkoxysilane include methyltriethoxysilane, phenyltrichlorosilane and dimethyldichlorosilane.
[0012] Phenyl alkoxysilane synthesized by methyltriethoxysilane, phenyltrichlorosilane and dimethyldichlorosilane has good performance. Methyltriethoxysilane can improve the wettability of silane, improve the adhesion performance of glue, and enhance the interlayer bonding strength of mica tubes. At the same time, the silicon-oxygen bond can inhibit charge migration and electron flow, reduce the risk of breakdown, and thus improve the insulation performance; the introduction of phenyl can improve the high-temperature performance of silane, so that the mica tube also has good working performance under high temperature conditions; dimethyldichlorosilane can improve adhesion and has good weather resistance and aging resistance. The synergistic effect of the three can better improve the performance of silicone-modified polyester resin.
[0013] Preferably, the raw materials for preparing the carboxyl polyester include 1,4-cyclohexanedicarboxylic acid, terephthalic acid, isophthalic acid, neopentyl glycol and trimethylpentanediol.
[0014] 1,4-cyclohexanedicarboxylic acid and trimethylpentanediol are used as functional monomers. 1,4-cyclohexanedicarboxylic acid contains a cycloalkane structure, which can effectively improve the stability and strength of polyester, thereby improving the strength and stability of the mica tube; trimethylpentanediol has a polyhydroxy structure, which can improve the hydrolysis resistance, stability and impact resistance of polyester. The carboxyl polyester synthesized by 1,4-cyclohexanedicarboxylic acid, terephthalic acid, isophthalic acid, neopentyl glycol and trimethylpentanediol has good working performance, can effectively combine ceramic powder with mica paper, and improve the strength, heat resistance and stability of the mica tube.
[0015] Preferably, the mass ratio of the phenylalkoxysilane to the carboxyl polyester is (0.15-0.25):1.
[0016] The organosilicon-modified polyester resin prepared according to the above mass ratio has good insulation performance and high strength.
[0017] Preferably, the ceramic powder comprises 10000 mesh ceramic powder, aminosilane and hexadecyltrimethylammonium bromide.
[0018] Cetyltrimethylammonium bromide is used to help the ceramic powder to be evenly dispersed. The cetyltrimethylammonium bromide molecules are adsorbed on the surface of the ceramic powder, forming charges between the powder particles, and preventing the agglomeration and sedimentation of the particles through electrostatic repulsion; aminosilane is grafted onto the surface of the ceramic powder by reacting with hydroxyl groups to improve the compatibility of the ceramic powder. The amino group can react with silicone-modified polyester resin to improve the compatibility and reactivity of the ceramic powder in the resin-dispersed ceramic powder glue, thereby improving the bonding strength between the ceramic powder and the mica tube, reducing the occurrence of stratification, and improving the strength and insulation properties of the mica tube.
[0019] Preferably, the curing time of the resin-ceramic powder glue in step (2) is 5-13 minutes.
[0020] Preferably, the thickness of the ceramic powder mica paper in step (3) is 0.07-0.1 mm.
[0021] Preferably, the temperature for baking and curing in step (5) is 130-180°C, and the baking and curing comprises the following steps: keeping the ceramic powder mica tube at 35-45°C for 0.5-1.5h, heating it to 130°C and keeping it for 1.5-2.5 hours, then heating it to 180°C and keeping it for 3.5-4.5 hours, cooling it to 60-80°C and taking it out, removing the winding core, and obtaining a cured ceramic powder mica tube.
[0022] By performing baking and curing molding according to the above steps, the ceramic powder mica tube can be effectively cured and molded, the strength and insulation performance of the far-infrared mica tube can be improved, and the occurrence of stratification can be reduced.
[0023] In summary, the present application includes at least one of the following beneficial technical effects: 1. The far-infrared mica tube prepared by the above steps has a smooth surface, good strength, no delamination between layers, can be rolled into mica tubes with different wall thicknesses, and can be processed into different lengths and shapes as needed. It can be used in electrical insulation, has high strength and good insulation performance, can withstand high temperatures, and has good stability.
[0024] 2. The resin mixed ceramic powder glue configured in the present application has good dispersibility and adhesion properties, which can improve the dispersibility of ceramic powder in the glue, reduce the agglomeration and sinking of ceramic powder, and make the ceramic powder evenly distributed on the mica paper during the dipping process, thereby improving the bonding force between the ceramic powder and the mica paper; the good adhesion and curing properties of the resin mixed ceramic powder glue improve the stability of the mica tube, reduce the occurrence of stratification of the mica tube, and the prepared far-infrared mica tube has high strength and good insulation properties.
[0025] 3. Phenyl alkoxysilane is used to modify carboxyl polyester to obtain silicone-modified polyester resin. Phenyl alkoxysilane can improve the weather resistance, heat resistance and strength of polyester resin, reduce the curing temperature of polyester, and shorten the curing time, so that the advantages of silicone and polyester resin complement each other. The introduction of silicone groups makes the polymer surface have stable siloxane bonds. Siloxane bonds can interact with a variety of surface groups, enhance the interlayer bonding of mica tubes through electrostatic interactions, van der Waals forces, etc., and reduce the occurrence of stratification. DETAILED DESCRIPTION
[0026] The present application discloses a far-infrared mica tube manufacturing process. The raw materials used in the present application can be obtained from commercially available raw materials unless otherwise specified. The present application is further described in detail below in conjunction with the embodiments: Raw materials: methyltriethoxysilane (CAS No.: 2031-67-6), phenyltrichlorosilane (CAS No.: 98-13-5), dimethyldichlorosilane (CAS No.: 75-78-5), neopentyl glycol (CAS No.: 126-30-7), trimethylpentanediol (CAS No.: 144-19-4), terephthalic acid (CAS No.: 100-21-0), 1,4-cyclohexane dioic acid (CAS No.: 1076-97-7), isophthalic acid (CAS No.: 121-91-5), catalyst is Monobutyl tin oxide (CAS No.: 51590-67-1), the heat stabilizer is triphenyl phosphite (CAS No.: 101-02-0), 10000 mesh ceramic powder was purchased from Donghai County Fucai Mineral Products Co., Ltd., aminosilane is KH-792 (CAS No.: 1760-24-3), hexadecyltrimethylammonium bromide (CAS No.: 57-09-0), the curing agent is N, N, N', N'-tetrakis (2-hydroxyethyl) adipamide (CAS No.: 6334-25-4), and the release agent was purchased from Guangdong Zhongke Hongtai New Materials.
[0027] Example 1 Preparation of silicone-modified polyester resin 17.18 kg of methyltriethoxysilane, 20.38 kg of phenyltrichlorosilane and 12.44 kg of dimethyldichlorosilane were mixed and dispersed in 100 L of a mixed solvent of toluene and acetone in a volume ratio of 1:1 to obtain a silane dispersion. 15 L of deionized water was added to the silane dispersion under the conditions of stirring at 200 rpm and a 50°C water bath. The addition was completed within 30 minutes, and the reaction was continued by heat preservation and stirring for 30 minutes to obtain a product solution. The product solution was rotary evaporated to remove the solvent to obtain phenylalkoxysilane.
[0028] 46.87 kg of neopentyl glycol, 7.31 kg of trimethylpentanediol, 71.02 kg of terephthalic acid, 4.3 kg of 1,4-cyclohexane dioic acid and 0.6 kg of catalyst were heated to melt to obtain a molten mixture, stirring was started at a stirring rate of 200 rpm, and after keeping warm for 1 hour, 1.4 kg of heat stabilizer was added, the temperature was raised to 240°C at a rate of 12°C / h for reaction for 2 hours, water was evaporated, and the temperature was kept warm for 1 hour, then the temperature was lowered to 180°C, 20 L of xylene and 12.54 kg of isophthalic acid were added, the temperature was raised to 220°C again for reaction for 2 hours, and then the reduced pressure distillation reaction was carried out at a constant temperature. After the acid value of the system was less than 8.0, the temperature was lowered to below 30°C to discharge the material to obtain a carboxyl polyester.
[0029] 86.96 kg of carboxyl polyester was heated and melted, 13.04 kg of phenyl alkoxy silane was added to the melted carboxyl polyester, and the mixture was stirred at a speed of 200 rpm for 30 minutes to obtain an organosilicon-modified polyester resin.
[0030] Preparation of ceramic powder 20 kg of 10000 mesh ceramic powder, 1 kg of aminosilane and 1 kg of hexadecyltrimethylammonium bromide were dispersed in 30 L of anhydrous ethanol solution, stirred at 500 rpm for 2 h, filtered and dried in an oven at 60° C. for 4 h to obtain ceramic powder.
[0031] Preparation of far-infrared mica tube (1) beating mica ore powder to prepare mica paper for standby use; (2) 45 kg of organosilicon-modified polyester resin, 25 kg of methanol, 25 kg of isopropanol, 0.8 kg of curing agent and 15 kg of ceramic powder were mixed, and stirred and dispersed at a speed of 200 rpm for 1 hour to obtain a resin-mixed ceramic powder glue for later use; (3) dipping the mica paper into the resin mixed ceramic powder glue for 30 minutes, and drying the impregnated mica paper in an oven at 60° C. to obtain the ceramic powder mica paper; (4) Wipe the winding core clean, apply a release agent on the winding core, and roll the ceramic powder mica paper on the winding core to obtain a ceramic powder mica tube; (5) The ceramic powder mica tube is kept at 35°C for 1.5 hours, heated to 130°C and kept for 1.5 hours, then heated to 180°C and kept for 4.5 hours, cooled to 60°C and taken out, the winding core is removed, and a solidified ceramic powder mica tube is obtained. The solidified ceramic powder mica tube is processed into a desired size and shape to obtain a far-infrared mica tube.
[0032] Example 2 Preparation of silicone-modified polyester resin 17.18 kg of methyltriethoxysilane, 20.38 kg of phenyltrichlorosilane and 12.44 kg of dimethyldichlorosilane were mixed and dispersed in 100 L of a mixed solvent of toluene and acetone in a volume ratio of 1:1 to obtain a silane dispersion. 15 L of deionized water was added to the silane dispersion under the conditions of stirring at 200 rpm and a 50°C water bath. The addition was completed within 30 minutes, and the reaction was continued by heat preservation and stirring for 30 minutes to obtain a product solution. The product solution was rotary evaporated to remove the solvent to obtain phenylalkoxysilane.
[0033] 46.87 kg of neopentyl glycol, 7.31 kg of trimethylpentanediol, 71.02 kg of terephthalic acid, 4.3 kg of 1,4-cyclohexane dioic acid and 0.6 kg of catalyst were heated to melt to obtain a molten mixture, stirring was started at a stirring rate of 200 rpm, and after keeping warm for 1 hour, 1.4 kg of heat stabilizer was added, the temperature was raised to 240°C at a rate of 12°C / h for reaction for 2 hours, water was evaporated, and the temperature was kept warm for 1 hour, then the temperature was lowered to 180°C, 20 L of xylene and 12.54 kg of isophthalic acid were added, the temperature was raised to 220°C again for reaction for 2 hours, and then the reduced pressure distillation reaction was carried out at a constant temperature. After the acid value of the system was less than 8.0, the temperature was lowered to below 30°C to discharge the material to obtain a carboxyl polyester.
[0034] 80 kg of carboxyl polyester was heated and melted, 20 kg of phenyl alkoxy silane was added to the melted carboxyl polyester, and the mixture was stirred at a speed of 200 rpm for 30 minutes to obtain an organosilicon-modified polyester resin.
[0035] Preparation of ceramic powder 20 kg of 10000 mesh ceramic powder, 1 kg of aminosilane and 1 kg of hexadecyltrimethylammonium bromide were dispersed in 30 L of anhydrous ethanol solution, stirred at 500 rpm for 2 h, filtered and dried in an oven at 60° C. for 4 h to obtain ceramic powder.
[0036] Preparation of far-infrared mica tube (1) beating mica ore powder to prepare mica paper for standby use; (2) 55 kg of organosilicon-modified polyester resin, 20 kg of methanol, 20 kg of isopropanol, 1.2 kg of curing agent and 17 kg of ceramic powder were mixed, and stirred and dispersed at a speed of 200 rpm for 1 hour to obtain a resin-mixed ceramic powder glue for later use; (3) dipping the mica paper into the resin mixed ceramic powder glue for 30 minutes, and drying the impregnated mica paper in an oven at 60° C. to obtain the ceramic powder mica paper; (4) Wipe the winding core clean, apply a release agent on the winding core, and roll the ceramic powder mica paper on the winding core to obtain a ceramic powder mica tube; (5) The ceramic powder mica tube is kept at 45°C for 0.5h, heated to 130°C and kept for 2.5 hours, then heated to 180°C and kept for 3.5 hours, cooled to 80°C and taken out, the winding core is removed, and a solidified ceramic powder mica tube is obtained. The solidified ceramic powder mica tube is processed into a desired size and shape to obtain a far-infrared mica tube.
[0037] Example 3 Preparation of silicone-modified polyester resin 17.18 kg of methyltriethoxysilane, 20.38 kg of phenyltrichlorosilane and 12.44 kg of dimethyldichlorosilane were mixed and dispersed in 100 L of a mixed solvent of toluene and acetone in a volume ratio of 1:1 to obtain a silane dispersion. 15 L of deionized water was added to the silane dispersion under the conditions of stirring at 200 rpm and a 50°C water bath. The addition was completed within 30 minutes, and the reaction was continued by heat preservation and stirring for 30 minutes to obtain a product solution. The product solution was rotary evaporated to remove the solvent to obtain phenylalkoxysilane.
[0038] 46.87 kg of neopentyl glycol, 7.31 kg of trimethylpentanediol, 71.02 kg of terephthalic acid, 4.3 kg of 1,4-cyclohexane dioic acid and 0.6 kg of catalyst were heated to melt to obtain a molten mixture, stirring was started at a stirring rate of 200 rpm, and after keeping warm for 1 hour, 1.4 kg of heat stabilizer was added, the temperature was raised to 240°C at a rate of 12°C / h for reaction for 2 hours, water was evaporated, and the temperature was kept warm for 1 hour, then the temperature was lowered to 180°C, 20 L of xylene and 12.54 kg of isophthalic acid were added, the temperature was raised to 220°C again for reaction for 2 hours, and then the reduced pressure distillation reaction was carried out at a constant temperature. After the acid value of the system was less than 8.0, the temperature was lowered to below 30°C to discharge the material to obtain a carboxyl polyester.
[0039] 83.33 kg of carboxyl polyester was heated and melted, 16.67 kg of phenyl alkoxy silane was added to the melted carboxyl polyester, and the mixture was stirred at a speed of 200 rpm for 30 minutes to obtain an organosilicon-modified polyester resin.
[0040] Preparation of ceramic powder 20 kg of 10000 mesh ceramic powder, 1 kg of aminosilane and 1 kg of hexadecyltrimethylammonium bromide were dispersed in 30 L of anhydrous ethanol solution, stirred at 500 rpm for 2 h, filtered and dried in an oven at 60° C. for 4 h to obtain ceramic powder.
[0041] Preparation of far-infrared mica tube (1) beating mica ore powder to prepare mica paper for standby use; (2) 50 kg of organosilicon-modified polyester resin, 22.5 kg of methanol, 22.5 kg of isopropanol, 1 kg of curing agent and 16 kg of ceramic powder were mixed, and stirred and dispersed at a speed of 200 rpm for 1 hour to obtain a resin-mixed ceramic powder glue for later use; (3) dipping the mica paper into the resin mixed ceramic powder glue for 30 minutes, and drying the impregnated mica paper in an oven at 60° C. to obtain the ceramic powder mica paper; (4) Wipe the winding core clean, apply a release agent on the winding core, and roll the ceramic powder mica paper on the winding core to obtain a ceramic powder mica tube; (5) The ceramic powder mica tube is kept at 40°C for 1 hour, heated to 130°C and kept for 2 hours, then heated to 180°C and kept for 4 hours, cooled to 70°C and taken out, the winding core is removed, and a solidified ceramic powder mica tube is obtained. The solidified ceramic powder mica tube is processed into a desired size and shape to obtain a far-infrared mica tube.
[0042] Example 4 Example 4 is based on Example 3. The only difference between Example 4 and Example 3 is that in Example 4, phenyltrichlorosilane is not added when preparing phenylalkoxysilane.
[0043] Example 5 Example 5 is based on Example 3. The only difference between Example 5 and Example 3 is that in Example 5, phenyltrichlorosilane and dimethyldichlorosilane are not added when preparing phenylalkoxysilane.
[0044] Example 6 Example 6 is based on Example 3. The only difference between Example 6 and Example 3 is that in Example 6, 1,4-cyclohexanedicarboxylic acid is not added when preparing the carboxyl polyester.
[0045] Example 7 Example 7 is based on Example 3. The only difference between Example 7 and Example 3 is that in Example 7, no trimethylpentanediol is added when preparing the carboxyl polyester.
[0046] Example 8 Example 8 is based on Example 3. The only difference between Example 8 and Example 3 is that in Example 8, the amount of phenylalkoxysilane used is 9.09 kg, and the amount of carboxyl polyester used is 90.91 kg.
[0047] Example 9 Example 9 is based on Example 3. The only difference between Example 9 and Example 3 is that in Example 9, the amount of phenylalkoxysilane used is 23.08 kg, and the amount of carboxyl polyester used is 76.92 kg.
[0048] Example 10 Example 10 is based on Example 3. The only difference between Example 10 and Example 3 is that in Example 10, the organosilicon-modified polyester resin is replaced by carboxyl polyester.
[0049] Embodiment 11 Example 11 is based on Example 3. The only difference between Example 11 and Example 3 is that aminosilane is not added when preparing the ceramic powder in Example 11.
[0050] Example 12 Example 12 is based on Example 3. The only difference between Example 12 and Example 3 is that hexadecyltrimethylammonium bromide is not added when preparing the ceramic powder in Example 12.
[0051] Example 13 Example 13 is based on Example 3, and the only difference between Example 13 and Example 3 is that in Example 13, the ceramic powder is replaced with 10000 mesh ceramic powder.
[0052] Performance testing (1) Strength test: Use a universal tester to test the maximum kilogram force (kgf) that a sample with a wall thickness of 1 mm can withstand. Prepare three samples for each sample, calculate the strength (kgf / mm) using kilogram force and wall thickness (mm), and take the average value after measurement.
[0053] (2) Insulation performance test: Test the insulation strength of the sample with a thickness of 0.75 mm and record the breakdown voltage. Each sample is tested three times and the average value is taken after measurement. The results are recorded in Table 1.
[0054] (3) Observe whether the sample has delamination after processing and record the results in Table 1.
[0055] Table 1 Test results of far-infrared mica tube insulation performance, strength and delamination Test results Strength (kgf / mm) Breakdown voltage(kV) Layering Example 1 0.28 11.6 No stratification Example 2 0.29 11.7 No stratification Example 3 0.30 12.0 No stratification Example 4 0.27 11.3 No stratification Example 5 0.25 11.1 No stratification Example 6 0.25 11.5 No stratification Example 7 0.26 11.4 No stratification Example 8 0.26 11.2 No stratification Example 9 0.27 11.4 No stratification Example 10 0.22 10.8 Layering Embodiment 11 0.26 11.1 Layering Example 12 0.24 10.9 Slight delamination Example 13 0.21 10.4 Layering It can be seen from Table 1 that the strength of Examples 1-3 is greater than 0.28 kgf / mm, the breakdown voltage is greater than 11.6 kV, and no delamination occurs, which shows that the far-infrared mica tube prepared in this application has good insulation, stability and high strength.
[0056] As can be seen from Table 1, the only difference between Examples 4 and 5 and Example 3 is that: in Example 4, phenyltrichlorosilane is not added when preparing phenylalkoxysilane, and in Example 5, phenyltrichlorosilane and dimethyldichlorosilane are not added when preparing phenylalkoxysilane. Compared with Example 3, Examples 4 and 5 have reduced insulation performance and strength. This is because phenyltrichlorosilane is not added, the introduction of phenyl structure is lacking, the heat resistance is reduced, and the stability of the silicone-modified polyester resin is reduced; further, dimethyldichlorosilane is not added, the adhesion of the resin mixed ceramic powder glue is reduced, the bonding force is weakened, and the stability of the mica tube is reduced, and the insulation performance and strength are reduced.
[0057] As can be seen from Table 1, the only difference between Examples 6 and 7 and Example 3 is that 1,4-cyclohexanedicarboxylic acid is not added when preparing the carboxyl polyester in Example 6, and trimethylpentanediol is not added when preparing the carboxyl polyester in Example 7. Compared with Example 3, the insulation performance and strength of Examples 6 and 7 are reduced. This is because the lack of introduction of functional monomers reduces the stability of the carboxyl polyester, thereby reducing the insulation performance and strength of the far-infrared mica tube.
[0058] As can be seen from Table 1, the only difference between Examples 8, 9, and 10 and Example 3 is that the mass ratio of phenyl alkoxy silane to carboxyl polyester in Example 8 is 0.1:1, the mass ratio of phenyl alkoxy silane to carboxyl polyester in Example 9 is 0.3:1, and the organosilicon-modified polyester resin is replaced with carboxyl polyester in Example 10. Compared with Example 3, the insulation performance and strength of Examples 8, 9, and 10 are reduced. This is because the mass ratio of phenyl alkoxy silane to carboxyl polyester is not within the specified range. Too much or too little phenyl alkoxy silane will affect the adhesion and stability of the organosilicon-modified polyester resin, thereby reducing the insulation performance and strength. Without adding phenyl alkoxy silane, there is a lack of silicon-oxygen bonds, the bonding force between the glue and the substrate interface is greatly reduced, the adhesion and stability are weakened, and the insulation performance, strength and stability are significantly reduced, and the product also has a stratification phenomenon.
[0059] As can be seen from Table 1, the only difference between Examples 11, 12, and 13 and Example 3 is that: in Example 11, aminosilane is not added when preparing the ceramic powder, in Example 12, hexadecyltrimethylammonium bromide is not added when preparing the ceramic powder, and in Example 13, the ceramic powder is replaced with 10000 mesh ceramic powder. Compared with Example 3, Examples 11, 12, and 13 have reduced insulation performance, strength, and stability. This is because without the addition of aminosilane, the compatibility of the ceramic powder with the silicone-modified polyester resin and mica paper deteriorates, and the binding force is weakened; without the addition of hexadecyltrimethylammonium bromide, the ceramic powder lacks electrostatic repulsion, is easy to agglomerate and settle, has poor binding force with mica paper, is easy to fall off, and has stratification; when the ceramic is replaced with unmodified 10000 mesh ceramic powder, the dispersibility and compatibility are further reduced, the insulation performance and strength are further reduced, and stratification occurs.
[0060] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A far-infrared mica tube manufacturing process, characterized in that: The steps include: (1) beating mica ore powder to prepare mica paper for later use; (2) Prepare resin mixed with ceramic powder glue and set aside; (3) impregnating the mica paper into a resin-mixed ceramic powder glue solution, and drying to obtain the ceramic powder mica paper; (4) Wipe the core clean, apply a release agent on the core, and roll the ceramic powder mica paper on the core to obtain a ceramic powder mica tube; (5) After the ceramic powder mica tube is baked and solidified, it is processed into a desired size and shape to obtain a far-infrared mica tube.
2. The far-infrared mica tube manufacturing process according to claim 1, characterized in that: The resin-mixed ceramic powder glue in step (2) comprises the following components in percentage by weight: 45%-55% of organosilicon-modified polyester resin, 20%-25% of methanol, 20%-25% of isopropanol, 0.8%-1.2% of curing agent, and 15%-17% of ceramic powder.
3. A far-infrared mica tube manufacturing process according to claim 2, characterized in that: The raw materials for preparing the organosilicon-modified polyester resin include phenyl alkoxy silane and carboxyl polyester.
4. A far-infrared mica tube manufacturing process according to claim 3, characterized in that: The raw materials for preparing the phenylalkoxysilane include methyltriethoxysilane, phenyltrichlorosilane and dimethyldichlorosilane.
5. The far-infrared mica tube manufacturing process according to claim 3 is characterized by: The raw materials for preparing the carboxyl polyester include 1,4-cyclohexanedicarboxylic acid, terephthalic acid, isophthalic acid, neopentyl glycol and trimethylpentanediol.
6. The manufacturing process of a far-infrared mica tube according to claim 3, characterized in that: The mass ratio of the phenylalkoxysilane to the carboxyl polyester is (0.15-0.25):
1.
7. The manufacturing process of a far-infrared mica tube according to claim 2, characterized in that: The ceramic powder comprises 10000 mesh ceramic powder, aminosilane and hexadecyltrimethylammonium bromide.
8. The manufacturing process of a far-infrared mica tube according to claim 2, characterized in that: The curing time of the resin mixed with ceramic powder glue in step (2) is 5-13 minutes.
9. The far-infrared mica tube manufacturing process according to claim 1, characterized in that: The thickness of the ceramic powder mica paper in step (3) is 0.07-0.1 mm.
10. The far-infrared mica tube manufacturing process according to claim 1, characterized in that: The temperature for baking and curing in step (5) is 130-180°C, and the baking and curing comprises the following steps: keeping the ceramic powder mica tube at 35-45°C for 0.5-1.5h, heating it to 130°C and keeping it for 1.5-2.5 hours, then heating it to 180°C and keeping it for 3.5-4.5 hours, cooling it to 60-80°C and taking it out, removing the winding core, and obtaining a cured ceramic powder mica tube.