High-stability composite rare earth permanent magnet material and preparation method thereof
Through the composite structure and Dy element distribution control of high Curie temperature base phase and high coercive force phase, the problem of insufficient coercive force and thermal stability in rare earth permanent magnet materials is solved, and high stability and low cost rare earths are achieved The preparation of permanent magnet material significantly improves the high-temperature performance of magnets.
Patent Information
- Application Number
- CN202411094534.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-10
- Publication Date
- 2024-11-22
AI Technical Summary
The magnet coercive force of existing rare earth permanent magnet materials is severely decayed with the increase of temperature, which is difficult to meet the requirements of wind power generation and permanent magnet motors for magnet use. The addition of heavy rare earth Dy elements leads to increased costs and reduced residual magnetism.
Using a composite structure of high Curie temperature base phase alloy and high coercive force alloy, high stability composite rare earth permanent magnet materials are prepared through induction smelting and rapid coagulation technology, and the distribution of Dy elements on the surface of the base phase grains is controlled to reduce non-uniform distribution. and inter-grain phase content enhances inter-grain exchange coupling effect.
Improve the residual magnetic temperature stability and coercive force temperature stability of magnets, reduce the amount of Dy elements, and significantly improve the high-temperature performance of magnets, including residual magnetic Br, coercive force HcJ, residual magnetic temperature coefficient α and coercive force Temperature coefficient β.
Smart Images

Figure CN119008156A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-stability composite rare earth permanent magnetic material and a preparation method thereof, belonging to the technical field of rare earth permanent magnetic materials. Background Art
[0002] The rare earth permanent magnet material Nd-Fe-B has high remanence and high magnetic energy product. It is an indispensable key material in modern transportation, clean energy, information, aerospace and other fields. However, the current rare earth permanent magnet material has low coercivity, especially with the increase of temperature, the coercivity decays seriously, which is difficult to meet the requirements of wind power generation and permanent magnet motors for magnets. The partial replacement of Fe by Co can increase the Curie temperature of the magnet and the saturation magnetization of the magnet. At the same time, the degree of attenuation of the remanence with the increase of temperature is weakened, and the thermal stability of the remanence is enhanced, but it will lead to a decrease in the coercivity of the magnet. 2 Fe 14 The B phase has an ultra-high magnetocrystalline anisotropy field, and its coercivity is much higher than that of Nd-Fe-B magnets, so adding heavy rare earth Dy can improve the coercivity of the magnet. Adding Co and Dy elements at the same time can improve the Curie temperature, room temperature coercivity and remanence temperature stability of the magnet.
[0003] In the existing method of adding Co and heavy rare earth Dy elements to improve the thermal stability of NdFeB magnets, Nd, Fe, Co, B and heavy rare earth Dy elements are directly mixed for smelting, powdering and sintering to form magnets. However, this method is used to evenly distribute the Dy element in the main phase grains of the magnet, and the amount of Dy element is large. Since the heavy rare earth Dy is very little in rare earth ores and is expensive, a large amount of Dy element will cause the cost of the magnet to rise sharply. Moreover, since the saturation magnetization intensity of Dy-Fe-B is low and the remanence is low, a large amount of Dy element will also cause the remanence of the magnet to decrease significantly. Therefore, Nd-(Fe, Co)-B and Dy alloys are mixed by a double alloy method, the coercive force of the magnet is improved, the Dy element is non-uniformly reduced, and the amount of Dy element used is reduced. However, due to the increase in the intergranular phase content, the remanence of the magnet is seriously reduced, and the intergranular coupling effect of the magnet is weakened when the intergranular phase content increases. Although the room temperature coercive force may be increased, it is difficult to further improve the temperature stability of the magnetic properties by increasing the intergranular phase content. Summary of the invention
[0004] In view of the shortcomings of the prior art, in order to improve the temperature stability of the magnetic properties of the magnet, reduce the dosage of the heavy rare earth Dy, prevent the increase of the intercrystalline phase content and significantly reduce the remanence of the magnet, enhance the intercrystalline interaction of the magnet, and further improve the coercive force and thermal stability, the present invention provides a high-stability composite rare earth permanent magnet material and a preparation method.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] 1. A high-stability composite rare earth permanent magnet material, which is made of a high Curie temperature base phase alloy and a high coercive force phase alloy, wherein the high-stability composite rare earth permanent magnet material has a high Curie temperature base phase and a high coercive force phase, and a shell phase exists on the surface of some high Curie temperature base phase grains;
[0007] The chemical formula of the high Curie temperature base phase alloy is composed of RE in atomic percentage. a Fe 100-a-b-c-d Co b M c B d , wherein 13.3≤a≤13.7, 5≤b≤15, 0.3≤c≤3×(a-13), 5.6≤d≤5.9; wherein M is an additive element, including three elements, Cu, Ga, and Zr, wherein the atomic percentage content of Cu is 0.05~(a-13.3) / 2, the atomic percentage content of Ga is 0.05~(a-13.3), and the atomic percentage content of Zr is 0.05~(a-13.3) / 1.5; RE is a rare earth element;
[0008] The chemical formula of the high coercivity phase alloy is composed of RE' in atomic percentage. e Fe 100-e-f-g-h Co f M' g B h , wherein 15≤e≤21, 0≤f≤5, 0.2≤g≤2.0, 5.0≤h≤6.0; M' is an added element, including any two or more elements of Cu, Al, Ga, Zr, Ti, Nb, Mo, Sn, and Ag, and RE' is a rare earth element.
[0009] 2. The high Curie temperature base phase alloy RE a Fe 100-a-b-c-d Co b M c B d The M element also includes any one or more of Al, Ti, Nb, Mo, Sn, and Ag elements.
[0010] 3. The high Curie temperature base phase alloy RE a Fe 100-a-b-c-d Co b M c B d The rare earth elements RE in the alloy include Pr and / or Nd, and the weight of the rare earth elements Pr and / or Nd is more than 70% of the total weight of the rare earth elements in the alloy.
[0011] 4. The rare earth element RE in the high Curie temperature base phase alloy further includes any one or more of La, Ce, Gd, Tb, Dy, Ho, Er, and Y.
[0012] 5. The high coercivity phase alloy RE' e Fe 100-e-f-g-h Co f M g B h The rare earth elements RE' in the alloy include Dy, and the content of Dy is more than 50% by weight of the total rare earth elements in the alloy.
[0013] 6. The rare earth element RE' in the high coercivity phase alloy further includes any one or more of La, Ce, Pr, Nd, Gd, Tb, Ho, Er, and Y.
[0014] 7. The high Curie temperature base phase alloy in the rare earth permanent magnet material accounts for 70% to 95% of the total weight of the alloy, and the high coercive force phase alloy accounts for 5% to 30% of the total weight of the alloy.
[0015] 8. The rare earth permanent magnet material comprises a high Curie temperature base phase, a high coercivity phase, and a shell phase on the surface of the base phase grains, and all of them are RE 2 Fe 14 B crystal phase structure, RE is a rare earth element.
[0016] 9. The present invention provides a method for preparing a high-stability composite rare earth permanent magnetic material, comprising the following steps:
[0017] (1) weighing and mixing ingredients according to the composition of the high-stability composite rare earth permanent magnet material to prepare a high Curie temperature base phase alloy and a high coercive force phase alloy respectively;
[0018] (2) The prepared high Curie temperature base phase alloy and high coercive force phase alloy are placed in the crucible of the induction melting rapid solidification furnace respectively, and the vacuum is evacuated to 0.1 Pa, and then heated to 600-900°C, and the temperature and vacuum are maintained. Argon is filled after 5-15 minutes, and electric heating is performed under the argon protection atmosphere. When the raw materials are melted into liquid, the molten liquid is poured onto a water-cooled copper roller with a linear speed of 1-3 m / s to obtain a high Curie temperature base phase alloy rapid solidification thin strip and a high coercive force phase alloy rare earth alloy rapid solidification thin strip with an average thickness of 0.1-0.6 mm respectively;
[0019] (3) mixing the obtained high Curie temperature base phase alloy quick-solidified thin strip and high coercive force alloy quick-solidified thin strip in a certain weight ratio, wherein the high Curie temperature base phase alloy is not less than 70wt.% of the weight of the mixed powder, and the high coercive force phase alloy powder is not less than 5wt.% of the weight of the mixed powder, placing the quick-solidified thin strip mixture into a hydrogen crushing furnace for hydrogen crushing to obtain a primary crushed powder, and then adding an organic protective medium of 0.3-1% of the total weight of the powder to the primary crushed powder, and then using a nitrogen gas flow mill to grind the primary crushed powder into an alloy powder with an average particle size of 1-5μm;
[0020] (4) The alloy powder is pressed into a shape in a 1-3T magnetic field press, and then cold isostatically pressed into a density of 3-5 g / cm 3 The pressure during isostatic pressing is 100MP-300MPa for the blank;
[0021] (5) Place the blank into the sintering furnace and evacuate the furnace to a vacuum of less than 3×10 -3 Pa, gradually heating up to a sintering temperature of 1040-1080°C, sintering for 1-4 hours, and naturally cooling to room temperature; then tempering, heat treatment at 850-950°C and 450-550°C for 1-4 hours, respectively, to obtain a composite rare earth permanent magnet material.
[0022] Preferably, the organic protective medium is a mixture of ethanol gasoline and glyceryl stearate, with a mass ratio of 9:1; in the process of heating to the sintering temperature, the heating rate is 10°C per minute, and the temperature is kept at 350°C, 550°C, and 850°C for 15 minutes respectively.
[0023] Beneficial effects of the present invention:
[0024] (1) The present invention controls the high Curie temperature base phase alloy composition, modulates the matching of rare earth and Cu, Ga, Zr and other element contents, modulates the intergranular phase distribution, reduces the intergranular phase content, and enhances the intergranular exchange coupling effect. At the same time, due to the enhanced intergranular exchange coupling effect, the size of the anti-magnetization domain wall increases, and the stability of the anti-magnetization domain wall is enhanced. In this way, the thermal disturbance effect is weakened, the temperature stability of the remanent magnetism of the magnet is improved, and the temperature stability of the coercive force is enhanced.
[0025] (2) The present invention prepares a sintered magnet by mixing a high Curie temperature base phase alloy powder and a high coercive force phase Dy-Fe-B alloy powder, thereby forming a composite structure of a high Curie temperature base phase, a base phase grain shell phase, and a high coercive force phase, thereby improving the coercive force of the magnet.
[0026] (3) The composite rare earth permanent magnet material of the present invention comprises a high Curie temperature base phase alloy powder and a high coercive force phase Dy-Fe-B alloy powder. The Dy element of the Dy-Fe-B alloy phase is mainly distributed on the surface of the base phase grains and the high coercive force phase at the surface of the high Curie temperature base phase grains. The content of Dy element inside the high Curie temperature base phase grains is very small, thereby achieving the purpose of reducing the use of Dy element.
[0027] (4) The high-stability composite rare earth permanent magnet material of the present invention has excellent performance. It has been determined that under high temperature conditions, the remanence of the magnet B r , coercive force H cJ , remanence temperature coefficient α, and coercive force temperature coefficient β are all higher than those of existing materials, and the performance is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The magnet scanning electron microscope image (SEM) of the permanent magnetic material of Example 2;
[0029] Figure 2 The Dy element distribution diagram of the electron probe microanalysis (EPMA) of the permanent magnetic material of Example 2;
[0030] Figure 3 It is a recovery curve diagram of the permanent magnetic material of Example 2 and the magnet of Comparative Example 1;
[0031] Figure 4 It is a fitting diagram of the measured curves of the after-effect field of thermal activation of the permanent magnet material of Example 2 and the magnet of Comparative Example 1. DETAILED DESCRIPTION
[0032] The specific implementation modes of the present invention are further described in detail below in conjunction with the embodiments.
[0033] Example 1 A high-stability composite rare earth permanent magnet material and preparation method
[0034] 1. Composite rare earth permanent magnet materials, including high Curie temperature base phase alloy and high coercivity phase alloy;
[0035] The chemical formula of the high Curie temperature base phase alloy is Nd in atomic percentage. 13.6 Fe 74.55 Co 5 Cu 0.1 Al 0.6 Ga 0.2 Zr 0.15 B 5.8 (i.e., Nd is 13.6 at.%, Fe is 74.55 at.%, Co is 5 at.%, Cu is 0.1 at.%, Al is 0.6 at.%, Ga is 0.2 at.%, Zr is 0.15 at.%, and B is 5.8 at.%);
[0036] The chemical formula of the high coercivity phase alloy is: Dy 19 Fe 74.75 Cu 0.05 Ga 0.11 Zr 0.09 B 6 (That is, Dy is 19at.%, Fe is 74.75at.%, Cu is 0.05at.%, Ga is 0.11at.%, Zr is 0.09at.%, and B is 6at.%).
[0037] 2. A method for preparing a high-stability composite rare earth permanent magnetic material, comprising the following steps:
[0038] (1) preparing high Curie temperature base phase alloy and high coercive force phase alloy respectively according to the composition of permanent magnet material alloy;
[0039] (2) Place the raw material high Curie temperature base phase alloy mixture into the crucible of the induction melting rapid solidification furnace and evacuate to 1×10 -1 After the temperature reaches 800°C, the temperature and vacuum are maintained. After 10 minutes, argon is filled in and then the temperature is heated. When the components are melted into liquid, the molten liquid is poured onto a water-cooled copper roller at a linear speed of 2 m / s to obtain an alloy quick-solidified thin strip with an average thickness of about 0.3 mm.
[0040] (3) Place the raw material high coercivity phase alloy mixture into the crucible of the induction melting rapid solidification furnace and evacuate to 1×10 - 1 After the temperature reaches 800°C, the temperature and vacuum are maintained. After 10 minutes, argon is filled in and then the temperature is heated. When the raw material components are melted into liquid, the molten liquid is poured onto a water-cooled copper roller at a linear speed of 2 m / s to obtain an alloy quick-solidified thin strip with an average thickness of about 0.3 mm.
[0041] (4) mixing a high Curie temperature base phase alloy quick-solidified thin ribbon and a high coercive force alloy quick-solidified thin ribbon in a mass ratio of 9.4:0.6, and then placing the quick-solidified thin ribbon mixture in a hydrogen crushing furnace for hydrogen crushing to obtain a primary crushed powder; adding an organic protective medium (the organic protective medium is composed of ethanol gasoline and stearyl glycerol in a mass ratio of 9:1) in an amount of 0.5% by weight of the powder to the primary crushed powder, and then adding nitrogen for air flow milling to grind the primary crushed powder into an alloy powder with an average particle size of about 3 μm;
[0042] (5) The alloy powder was pressed into a 2T magnetic field and formed into a density of about 3.5 g / cm in a cold isostatic press. 3 The blank, wherein the pressure during the isostatic pressing process is 200MPa;
[0043] (6) Place the blank into the sintering furnace and evacuate the furnace to a vacuum of less than 3×10 -3 Pa, and then slowly raise the temperature until it reaches the sintering temperature of 1065°C; keep it at this temperature for 2 hours, and cool it to room temperature with the furnace; then temper it and heat treat it at 900°C and 520°C for 2 hours respectively to further improve the coercive force of the magnet and obtain a high-stability composite rare earth permanent magnet material.
[0044] In the process of slowly heating up to the sintering temperature, the heating rate is controlled at 10°C per minute, and the temperatures are kept at 350°C, 550°C, and 850°C for 15 minutes respectively.
[0045] The main phase of the obtained high stability composite rare earth permanent magnet material is RE 2 Fe 14 B crystal, the magnet has a high Curie temperature base phase and a high coercive force phase, and a shell phase exists on the surface of some high Curie temperature base phase grains.
[0046] The magnetic properties of the permanent magnets at different temperatures, namely the remanence B, were measured using a NIM-200C permanent magnet material magnetic measuring instrument. r , coercive force H cJ The measurement temperature is room temperature 20℃, 80℃, 100℃, 120℃, 150℃, 180℃, the remanence of the magnet B r , coercive force H cJ , remanence temperature coefficient α, coercivity temperature coefficient β, see Table 1.
[0047] Remanence temperature coefficient α=[(B r (T)-B r (T 0 )) / (B r (T 0 )×(TT 0 ))]×100%, where B r (T) is the residual magnetization of the magnet at temperature T, T 0 =20℃.
[0048] Coercivity temperature coefficient β = [(H cJ (T)-H cJ (T 0 )) / (H cJ (T 0 )×(TT 0 ))]×100%, where H cJ (T) is the coercive force of the magnet at temperature T, T 0 =20℃.
[0049] Table 1 Performance parameters of rare earth permanent magnet materials of Example 1
[0050] T(℃) <![CDATA[B r (kGs)]]> <![CDATA[H cJ (no)]]> α(% / ℃) β(% / ℃) 20 13.43 19.56 - - 80 12.8 12.96 -0.078 -0.562 100 12.52 10.99 -0.085 -0.548 120 12.21 9.1 -0.091 -0.535 150 11.77 6.62 -0.095 -0.509 180 11.22 4.61 -0.103 -0.478
[0051] Example 2 A high-stability composite rare earth permanent magnet material and preparation method
[0052] The composition of the composite rare earth permanent magnet material includes a high Curie temperature base phase alloy and a high coercivity phase alloy; the chemical formula of the high Curie temperature base phase alloy is Nd 13.0 G 0.5 Fe 68.38 Co 11 Cu 0.05 Al 0.9 Ga 0.2 Zr 0.12 Ti 0.05 B 5.8 The chemical formula of high coercivity phase alloy is Dy in atomic percentage. 19 Fe 73.78 Cu 0.05 Al 0.9 Ga 0.2 Zr 0.12 Ti 0.05 B 5.9 .
[0053] The method for preparing the high-stability composite rare earth permanent magnetic material comprises the following steps:
[0054] (1) preparing high Curie temperature base phase alloy and high coercivity phase alloy respectively according to composition requirements;
[0055] (2) Place the raw material high Curie temperature base phase alloy mixture into the crucible of the induction melting rapid solidification furnace and evacuate to 1×10 -1 After Pa, it is electrically heated to 800°C and maintained at this temperature and vacuum degree. After 10 minutes, argon gas is filled in and then electrically heated. When the raw material components are melted into liquid, the molten liquid is poured onto a water-cooled copper roller with a linear speed of 2m / s to obtain an alloy quick-solidified thin strip with an average thickness of about 0.3mm.
[0056] (3) Place the raw material high coercivity phase alloy mixture into the crucible of the induction melting rapid solidification furnace and evacuate to 1×10 - 1 After Pa, it is electrically heated to 800°C, and the temperature and vacuum are maintained. After 10 minutes, argon gas is filled in, and then it is electrically heated. When the raw material components are melted into liquid, the molten liquid is poured onto a water-cooled copper roller with a linear speed of 2m / s to obtain an alloy quick-solidified thin strip with an average thickness of about 0.3mm.
[0057] (4) mixing a high Curie temperature base phase alloy quick-solidified ribbon and a high coercive force alloy quick-solidified ribbon in a mass ratio of 9:1, and then placing the quick-solidified ribbon mixture in a hydrogen crushing furnace for hydrogen crushing to obtain a primary crushed powder; adding an organic protective medium (the organic protective medium is composed of ethanol gasoline and stearyl glycerol in a mass ratio of 9:1) in an amount of 0.5% by weight of the powder to the primary crushed powder, and then adding nitrogen for air flow milling to grind the primary crushed powder into an alloy powder with an average particle size of about 3 μm;
[0058] (5) The alloy powder after air flow milling was pressed into a 2T magnetic field and a density of about 3.5 g / cm was formed in a cold isostatic press. 3 The blank, wherein the pressure during the isostatic pressing process is 200MPa;
[0059] (6) Place the blank into the sintering furnace and evacuate the furnace to a vacuum of less than 3×10 -3 Pa, and then slowly heat up until it reaches the sintering temperature of 1070°C; keep at this temperature for 2 hours, and cool to room temperature with the furnace; then temper, heat treat at 900°C and 520°C for 2 hours respectively, to further improve the coercive force of the magnet and obtain a permanent magnet.
[0060] During the process of heating to the sintering temperature, the heating rate was controlled at 10°C per minute, and the temperatures were kept at 350°C, 550°C, and 850°C for 15 minutes respectively.
[0061] The main phase of the obtained high stability composite rare earth permanent magnet material is RE 2 Fe 14 B crystal, the magnet has a high Curie temperature base phase and a high coercive force phase, and a shell phase exists on the surface of some high Curie temperature base phase grains.
[0062] The magnetic properties of the permanent magnets at different temperatures were measured using a NIM-200C permanent magnet material magnetic measuring instrument. The measuring temperatures were 20°C, 80°C, 100°C, 120°C, 150°C, and 180°C. r , coercive force H cJ , remanence temperature coefficient α, coercivity temperature coefficient β, see Table 2.
[0063] Table 2 Performance parameters of rare earth permanent magnet materials in Example 2
[0064] T(℃) <![CDATA[B r (kGs)]]> <![CDATA[H cJ (no)]]> α(% / ℃) β(% / ℃) 20 13.36 18.64 - - 80 12.78 11.94 -0.072 -0.599 100 12.57 10.09 -0.074 -0.573 120 12.33 8.33 -0.077 -0.553 150 11.94 6.35 -0.082 -0.507 180 11.59 4.86 -0.083 -0.462
[0065] Figure 1 This is a scanning electron microscope (SEM) image of the magnet of Example 2. The gray part in the image is the main phase RE 2 Fe 14 B grain, the brighter part is the intergranular rare earth-rich phase.
[0066] Figure 2 for Figure 1 Dy element distribution map of electron probe microanalysis (EPMA).
[0067] Figure 2 The uneven distribution of Dy elements can be seen from the color depth. The red dotted line part is the Dy-rich RE 2 Fe 14 The main phase B can maintain high anisotropy and provide high coercivity. The white dotted line part is the main phase RE 2 Fe 14 B, the area with low Dy content inside the grain. The Dy element is mainly distributed on the surface of the base phase grains, which can improve the anisotropy and coercivity of the grain boundaries. The Dy element has a low content inside the grains, which can reduce the amount of heavy rare earth Dy element and achieve the purpose of reducing heavy rare earth.
[0068] Comparative Example 1
[0069] A rare earth permanent magnet material, the raw material alloy chemical formula in atomic percentage is
[0070] Nd 11.82 G 0.45 Dy 1.72 Fe 68.88 Co 10 Cu 0.05 Al 0.9 Ga 0.2 Zr 0.12 Ti 0.05 B 5.81 .
[0071] The material is made by the method of Example 2, and the main phase of the permanent magnet obtained is RE 2 Fe 14 B crystal.
[0072] The difference between the preparation methods is that the permanent magnetic material has only one crystal phase, so there is no need to mix two crystal phase powders.
[0073] The performance parameters of the permanent magnetic material of Comparative Example 1 were measured using the above-mentioned NIM-200C permanent magnetic material magnetic measuring instrument. The measuring temperatures were 20°C, 80°C, 100°C, 120°C, 150°C, and 180°C, respectively. The measured remanence B r , coercive force H cJ , remanence temperature coefficient α, coercivity temperature coefficient β, see Table 3.
[0074] Table 3 Performance parameters of rare earth permanent magnet materials in comparative example 1
[0075] T(℃) <![CDATA[B r (kGs)]]> <![CDATA[H cj (no)]]> α(% / ℃) β(% / ℃) 20 13.17 17.56 - - 80 12.56 10.93 -0.077 -0.63 100 12.33 9.15 -0.079 -0.599 120 12.1 7.6 -0.081 -0.567 150 11.76 5.64 -0.082 -0.522 180 11.34 4.07 -0.087 -0.48
[0076] The contents of Dy, Co, and Nd in the permanent magnet of Comparative Example 1 are basically the same as those in Example 2, but the magnet of Comparative Example 1 does not mix the high Curie temperature base phase alloy powder and the high coercive force phase Dy-Fe-B alloy powder, and the magnet does not form a composite structure of high Curie temperature base phase, base phase grain shell phase, and high coercive force phase, so the coercive force of the magnet of Example 2 at all temperatures is higher than that of Comparative Example 1.
[0077] The rare earth RE content of the magnet in Comparative Example 1 is 13.99at.%, which is higher than 13.7at.%. Since the high Curie temperature base phase alloy component cannot be controlled independently and the intergranular phase distribution is difficult to modulate, the remanence of the magnet in Comparative Example 1 is lower, and the remanence of the magnet in Example 2 is higher than that in Comparative Example 1.
[0078] Figure 3 It is the recovery curve diagram of the magnet of comparative example 1 and the magnet of embodiment 2.
[0079] The recovery curve of comparative example 1 is basically flat. The recovery curve of the magnet of Example 2 has a large slope and exhibits magnetoelastic behavior, which is a characteristic of intercrystalline exchange coupling. The magnet of Example 2 controls the high Curie temperature base phase composition, modulates the intercrystalline phase distribution, reduces the intercrystalline phase content, and enhances the intercrystalline exchange coupling. On the basis of adding Dy-Fe-B powder, a composite structure of high Curie temperature base phase, base phase grain shell phase, and high coercive force phase is formed, which can improve the coercive force of the magnet.
[0080] Figure 4 It is a fitting diagram of the measured curves of the thermal activation after-effect field of the magnets of Comparative Example 1 and Example 2. af is 0.40kOe, and the magnet H of Example 2 af It is 0.36 kOe. The effective field after thermal activation of the magnet in Example 2 is low, which indicates that the intercrystalline coupling effect is stronger.
[0081] The magnet of Comparative Example 1 does not use a mixture of high Curie temperature base phase alloy powder and high coercive force phase Dy-Fe-B alloy powder to prepare a sintered magnet, which makes it difficult to modulate the intercrystalline exchange coupling effect, resulting in weak intercrystalline exchange coupling, thereby increasing the thermal disturbance effect, increasing the thermal activation aftereffect field, and reducing the coercive force temperature coefficient.
[0082] The present invention modulates the intercrystalline exchange coupling effect, the intercrystalline exchange coupling effect is enhanced, and the size of the reverse magnetization domain wall is increased, so that the thermal disturbance effect is weakened, the remanence temperature stability is improved, and the coercive force temperature stability is enhanced.
[0083] The above embodiments are only for the purpose of clearly illustrating the present invention, and are not intended to limit the implementation methods. For those skilled in the art, other equivalent or similar changes can be made based on the concept of the present invention, and these changes are all within the scope of protection of the present invention.
Claims
1. A high-stability composite rare earth permanent magnet material, characterized in that: The high-stability composite rare earth permanent magnet material is made of a high Curie temperature base phase alloy and a high coercive force phase alloy. The high-stability composite rare earth permanent magnet material has a high Curie temperature base phase and a high coercive force phase, and a shell phase exists on the surface of some high Curie temperature base phase grains. The chemical formula of the high Curie temperature base phase alloy is composed of RE in atomic percentage. a Fe 100-a-b-c-d Co b M c B d , where 13.3≤a≤13.7, 5≤b≤15, 0.3≤c≤3×(a-13), 5.6≤d≤5.9; Wherein, M is an additive element, including Cu, Ga, and Zr, wherein the atomic percentage content of Cu is 0.05 to (a-13.3) / 2, the atomic percentage content of Ga is 0.05 to (a-13.3), and the atomic percentage content of Zr is 0.05 to (a-13.3) / 1.5; RE is a rare earth element; The chemical formula of the high coercivity phase alloy is composed of RE' in atomic percentage. e Fe 100-e-f-g-h Co f M' g B h , where 15≤e≤21, 0≤f≤5, 0.2≤g≤2.0, 5.0≤h≤6.0; M' is an added element, including any two or more elements of Cu, Al, Ga, Zr, Ti, Nb, Mo, Sn, and Ag, and RE' is a rare earth element.
2. The composite rare earth permanent magnet material according to claim 1, wherein: The high Curie temperature base phase alloy RE a Fe 100-a-b-c-d Co b M c B d The M element also includes any one or more of Al, Ti, Nb, Mo, Sn, and Ag elements.
3. The composite rare earth permanent magnet material according to claim 1, wherein: The high Curie temperature base phase alloy RE a Fe 100-a-b-c-d Co b M c B d The rare earth elements RE in the alloy include Pr and / or Nd, and the weight of the rare earth elements Pr and / or Nd is more than 70% of the total weight of the rare earth elements in the alloy.
4. The high-stability composite rare earth permanent magnet material according to claim 3, wherein: The rare earth element RE in the high Curie temperature base phase alloy further includes any one or more of La, Ce, Gd, Tb, Dy, Ho, Er, and Y.
5. The composite rare earth permanent magnet material according to claim 1, wherein The high coercive force phase alloy RE' e Fe 100-e-f-g-h Co f M g B h The rare earth elements RE' in the alloy include Dy, and the content of Dy is more than 50% by weight of the total rare earth elements in the alloy.
6. The composite rare earth permanent magnet material according to claim 5, characterized in that: The rare earth element RE' in the high coercivity phase alloy further includes any one or more of La, Ce, Pr, Nd, Gd, Tb, Ho, Er, and Y.
7. The composite rare earth permanent magnet material according to claim 1, wherein The high Curie temperature base phase alloy in the rare earth permanent magnet material accounts for 70% to 95% of the total weight of the alloy, and the high coercive force phase alloy accounts for 5% to 30% of the total weight of the alloy.
8. The composite rare earth permanent magnet material according to claim 1, wherein: The rare earth permanent magnet material includes a high Curie temperature base phase, a high coercive force phase, and a shell phase on the surface of the base phase grains, and all of them are RE2Fe 14 B crystal phase structure, RE is a rare earth element.
9. A method for preparing a high-stability composite rare earth permanent magnet material according to any one of claims 1 to 8, characterized in that: The method includes the following steps: (1) Weighing and mixing the ingredients according to the composition of the high-stability composite rare earth permanent magnet material to prepare a high Curie temperature base phase alloy and a high coercive force phase alloy respectively; (2) The prepared high Curie temperature base phase alloy and high coercive force phase alloy are placed in the crucible of the induction melting rapid solidification furnace respectively, evacuated to 0.1 Pa, and then heated to 600-900 ° C., maintaining this temperature and vacuum degree, filling with argon gas after 5-15 minutes, and electrically heating under the argon protective atmosphere. When the raw materials are melted into liquid, the melt is poured onto a water-cooled copper roller with a linear speed of 1-3 m / s to obtain a high Curie temperature base phase alloy rapid solidification thin strip and a high coercive force phase alloy rare earth alloy rapid solidification thin strip with an average thickness of 0.1-0.6 mm respectively; (3) mixing the obtained high Curie temperature base phase alloy quick-solidified thin ribbon and high coercivity alloy quick-solidified thin ribbon in a certain weight ratio, wherein the high Curie temperature base phase alloy accounts for no less than 70 wt.% of the weight of the mixed powder, and the high coercivity phase alloy powder accounts for no less than 5 wt.% of the weight of the mixed powder, placing the quick-solidified thin ribbon mixture into a hydrogen crushing furnace for hydrogen crushing to obtain a primary crushed powder, and then adding an organic protective medium in an amount of 0.3-1% of the total weight of the powder to the primary crushed powder, and then using a nitrogen gas flow mill to grind the primary crushed powder into an alloy powder with an average particle size of 1-5 μm; (4) The alloy powder is pressed into a shape in a 1-3T magnetic field press, and then cold isostatically pressed into a density of 3-5g / cm 3 The pressure during the isostatic pressing process is 100MP-300MPa; (5) Place the blank into the sintering furnace and evacuate the furnace to a vacuum of less than 3×10 -3 Pa, gradually heating to a sintering temperature of 1040-1080°C, sintering for 1-4 hours, and naturally cooling to room temperature; then tempering, heat treating at 850-950°C and 450-550°C for 1-4 hours respectively, to obtain a composite rare earth permanent magnet material.
10. The preparation method according to claim 9, characterized in that The organic protective medium is a mixture of ethanol gasoline and glyceryl stearate, with a mass ratio of 9:
1. During the heating process to the sintering temperature, the heating rate is 10°C per minute, and the temperature is maintained at 350°C, 550°C, and 850°C for 15 minutes respectively.
Citation Information
Cited By
Preparation method of high-performance rare earth permanent magnet material
CN121148891A
Preparation method of high-performance rare earth permanent magnet material
CN121148891B