Cutting pyrolysis film integrated circuit packaging method
By using a three-layer structure pyrolytic film and eliminating its viscosity at high temperature, the problem of UV film residual glue in packaging substrate cutting is solved, the production efficiency and product quality are improved, the process flow is simplified and the cost is reduced.
Patent Information
- Application Number
- CN202411006416.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-22
AI Technical Summary
During the cutting process of packaging substrates, existing UV film technology is prone to residual glue, which reduces product quality, and has many processes, resulting in low production efficiency.
The pyrolysis film with a three-layer structure, including PET release film, foamed pressure-sensitive adhesive layer and transparent PET film, eliminates the viscosity of the pyrolysis film by baking, realizes automatic separation of semiconductor devices and tape, and simplifies the process flow.
Automatic separation between the product and the pyrolysis membrane is achieved, production efficiency and product quality are improved, production costs and process steps are reduced from 6 processes to 3.
Smart Images

Figure CN119008498A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chip packaging, in particular to a cutting pyrolysis film integrated circuit packaging method. Background Art
[0002] Cutting the package substrate is also an important step in the packaging process. In the previous step of the packaging process, after the electronic chip is mounted on the substrate and the circuit is connected, the substrate needs to be cut into small pieces of the required size in order to be assembled into the final electronic product. During the cutting process of the package substrate, it is important to ensure the consistency of the cutting size and accuracy to avoid damaging the chip or affecting the connection of the circuit.
[0003] The current process is to use UV film, put the substrate on the UV film, place the UV film on the cutting machine, and use the cutting knife to cut, while also cutting the substrate into the corresponding shape and size. After the cutting is completed, the UV film is exposed to the UV exposure machine for a certain period of time so that the UV film is hardened after being irradiated. The cut substrate is cleaned by a cleaning machine to remove the residue and pollution generated during the cutting process.
[0004] However, for electronic components with height differences, residual glue is prone to occur when using UV anti-viscosity film due to air residue, which reduces product quality. At the same time, the product production process is more complicated, which reduces production efficiency. Summary of the invention
[0005] The object of the present invention is to provide a method for cutting pyrolysis film integrated circuit packaging to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solution: a method for cutting pyrolysis film integrated circuit packaging, comprising the following steps:
[0007] Step 1: Product film pasting: Paste the pyrolytic film on the product surface to prepare for subsequent cutting;
[0008] Step 2: Cut the product into individual pieces along the cutting path;
[0009] Step 3: Baking: The high temperature eliminates the stickiness of the pyrolysis film, making it easier to separate the product from the pyrolysis film.
[0010] Furthermore, the pyrolysis film consists of a three-layer structure, the first layer is a PET release film, the thickness of the PET release film is 30-70μm; the second layer is a foamed pressure-sensitive adhesive layer, the thickness of the foamed pressure-sensitive adhesive layer is 35-45μm; the third layer is a transparent PET film, the thickness of the transparent PET film is 50-100μm.
[0011] Furthermore, the PET release film is torn off when the product is film-applied in step 1.
[0012] Furthermore, the foamed pressure-sensitive adhesive layer is directly bonded to the surface of the product.
[0013] Furthermore, during the baking in step three, the oven temperature is set to 120-160° C., and the drying time is set to 1-3 minutes, until the stickiness of the pyrolysis film completely disappears.
[0014] Furthermore, after baking in step three, the product is turned upside down on the top of the material receiving box, and the product falls directly into the material receiving box.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] The cutting pyrolysis film integrated circuit packaging method is provided with a pyrolysis film, and the pyrolysis film can completely lose its stickiness after heating, thereby realizing automatic separation of semiconductor devices and adhesive tape, simplifying the manufacturing process, and improving production efficiency and product quality.
[0017] In this solution, the cutting process is reduced from 6 to 3 steps, which improves the product yield and reduces the production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a comparison chart of the yield rate before and after the improvement of the present invention;
[0019] Figure 2 The process flow chart before and after the improvement of the present invention;
[0020] Figure 3 This is a structural diagram of the pyrolysis membrane before and after improvement of the present invention. DETAILED DESCRIPTION
[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] The current process is to use UV film, attach the substrate to the UV film, place the UV film on a cutting machine, and use a cutting knife to cut it, while also cutting the substrate into corresponding shapes and sizes. After cutting, the UV film is exposed to the UV exposure machine for a certain period of time so that the UV film hardens after being irradiated. The cut substrate is cleaned by a cleaning machine to remove residues and contaminants generated during the cutting process. However, for electronic components with height differences, residual glue is prone to occur when using UV anti-viscosity film due to air residue. At the same time, in order to improve work efficiency and reduce manufacturing costs, issues such as material utilization and material waste rate usually need to be considered.
[0023] like Figure 1-Figure 3 As shown, a method for cutting pyrolysis film integrated circuit packaging comprises the following steps:
[0024] Step 1: Product film pasting: Paste the pyrolytic film on the surface of the product to prepare for subsequent cutting. The pyrolytic film consists of a three-layer structure: the first layer is a PET release film with a thickness of 30-70 μm; the second layer is a foamed pressure-sensitive adhesive layer with a thickness of 35-45 μm; the third layer is a transparent PET film with a thickness of 50-100 μm.
[0025] In a specific embodiment of the present solution, the thickness of the PET release film is 30 μm, the thickness of the foamed pressure-sensitive adhesive layer is 35 μm; the thickness of the transparent PET film is 50 μm;
[0026] In another specific embodiment of the present solution, the thickness of the PET release film is 70 μm, the thickness of the foamed pressure-sensitive adhesive layer is 45 μm; the thickness of the transparent PET film is 100 μm;
[0027] Another thing you need to know is that the foamed pressure-sensitive adhesive layer is directly bonded to the product surface, and the PET release film is torn off when the product is bonded in step one.
[0028] Step 2: Cut the product into individual pieces along the cutting path;
[0029] Step 3: Baking: The high temperature eliminates the stickiness of the pyrolysis film, making it easier to separate the product from the pyrolysis film.
[0030] Among them, during step three baking, the oven temperature is set to 120-160°C, and the drying time is set to 1-3 minutes.
[0031] After step three of baking, the product is turned upside down on the top of the receiving box. After baking, the stickiness of the foamed pressure-sensitive adhesive layer is eliminated, and the product falls directly into the receiving box under its own gravity.
[0032] refer to Figure 2 It can be seen that compared with the prior art, this technical solution eliminates the steps of UV exposure, film tearing and single product cleaning, shortening the entire process from the original six steps to three steps, thereby achieving the effect of improving efficiency.
[0033] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is limited by the attached embodiments and their equivalents.
Claims
1. A method for cutting pyrolysis film integrated circuit packaging, characterized in that: The following steps are involved: Step 1: Product film pasting: Paste the pyrolytic film on the product surface to prepare for subsequent cutting; Step 2: Cut the product into individual pieces along the cutting path; Step 3: Baking: The high temperature eliminates the stickiness of the pyrolysis film, making it easier to separate the product from the pyrolysis film.
2. A method for cutting pyrolysis film integrated circuit packaging according to claim 1, characterized in that: The pyrolysis film consists of a three-layer structure, wherein the first layer is a PET release film with a thickness of 30-70 μm; the second layer is a foamed pressure-sensitive adhesive layer with a thickness of 35-45 μm; and the third layer is a transparent PET film with a thickness of 50-100 μm.
3. A method for cutting pyrolysis film integrated circuit packaging according to claim 2, characterized in that: The PET release film is torn off when the product is film-applied in step 1.
4. A method for cutting pyrolysis film integrated circuit packaging according to claim 2, characterized in that: The foamed pressure-sensitive adhesive layer is directly bonded to the surface of the product.
5. The method for cutting pyrolysis film integrated circuit packaging according to claim 1, characterized in that: During the baking in step 3, the oven temperature is set to 120-160° C., and the drying time is set to 1-3 minutes, until the stickiness of the pyrolysis film completely disappears.
6. A method for cutting pyrolysis film integrated circuit packaging according to claim 1, characterized in that: After baking in step 3, the product is turned upside down on the top of the material receiving box, and the product falls directly into the material receiving box.