Waveguide coupling photoelectric detector and preparation method thereof
By setting a hollow silicon dioxide template cavity and a germanium buffer layer on the SOI substrate, the silicon-germanium heterogeneous interface is avoided, and the photoresponsiveness and absorption rate of the Ge1-xSnx photodetector is improved, and the problem of interface defects is solved, so as to achieve More efficient photoelectric conversion and smaller device design.
Patent Information
- Application Number
- CN202411103522.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Silicon-based Ge1-xSnx photodetectors cause interface defects due to lattice mismatch at the silicon-germanium heterogeneous interface, affecting device performance, especially device responsiveness and high dark current.
A hollow silicon dioxide template cavity is provided on the SOI substrate, the germanium buffer layer and the Ge1-xSnx absorbing layer are grown in the silicon dioxide template cavity, and the optical signal is coupled into the Ge1-xSnx absorbing layer through the silicon dioxide layer to avoid passing through the silicon Germanium heterogeneous interface, thereby reducing the loss of interface defects to optical signals.
The photogenerated carrier absorption is significantly improved, the photoresponse is enhanced, the dark current level is reduced, and the smaller device size and higher integration is achieved, optimizing the photoelectric conversion efficiency.
Smart Images

Figure CN119008758A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of optoelectronic materials and devices, and in particular relates to a waveguide coupled photoelectric detector, and further relates to a method for preparing the waveguide coupled photoelectric detector. Background Art
[0002] With the increasing demand for intelligent applications such as big data, cloud computing, and AI, the new generation of information technology is developing rapidly. As an important development frontier, optical chips use photons instead of electrons as information carriers, showing the performance advantages of high speed, high density, low cost, and low power consumption. Due to its good electrical properties and CMOS process compatibility, silicon-based optoelectronic integration has become the most promising method in technology.
[0003] Silicon-based photodetectors are one of the important devices of silicon-based optoelectronic integration. Since the energy band structure of silicon cannot respond well to the short-wave infrared and mid-infrared bands, Ge with excellent optoelectronic properties and CMOS process compatibility is introduced. 1- x Sn x Material. 1-x Sn x According to the different light incident modes, detectors are mainly divided into two device structures: surface incident and waveguide coupled. Compared with the surface incident structure, the photodetector with waveguide coupled structure is easier to integrate with other optical waveguide devices and is suitable for on-chip integrated applications. At the same time, the incident direction of light in the photodetector with waveguide coupled structure is perpendicular to the transport direction of carriers, which can basically break the trade-off between responsivity and bandwidth, and obtain relatively high device responsivity while improving bandwidth. However, in the current photodetector related technologies, silicon-based Ge 1-x Sn x Photodetectors often have limited device performance due to interface defects caused by lattice mismatch at the silicon-germanium heterointerface. Therefore, it is necessary to conduct in-depth research to improve the structure of existing waveguide-coupled photodetectors. Summary of the invention
[0004] The present invention is based on the discovery and recognition of the following facts and problems by the inventors: 1-x Sn x In detectors, evanescent wave coupling structures are more common, Ge 1-x Sn x The absorption layer is above the silicon waveguide. After the optical signal from the silicon waveguide reaches the bottom of the absorption layer, it couples into the Ge with a refractive index greater than that of silicon through evanescent wave coupling. 1-x Sn x The absorption layer realizes the absorption detection of light. The heterojunction of silicon germanium is the evanescent wave coupled into Ge by silicon waveguide. 1-xSn x The dislocations and defects at the heterojunction interface will cause non-radiative recombination absorption of photons, reduce the number of effective photogenerated carriers, and thus cause high dark current and low responsivity of the detector. Therefore, it is necessary to study and improve it.
[0005] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, an embodiment of the present invention provides a waveguide coupled photodetector, which does not directly set Ge on the SOI substrate. 1-x Sn x Instead of using a silicon dioxide hollow template cavity on the SOI substrate, the epitaxy of germanium material is realized in the cavity, so that the optical signal is coupled into the detector without passing through the silicon-germanium heterojunction, thereby improving the performance of the device.
[0006] The waveguide coupled photodetector of the embodiment of the present invention comprises: an SOI substrate, a hollow silicon dioxide template cavity, a Ge 1-x Sn x Absorption zone and electrodes;
[0007] The SOI substrate comprises a silicon substrate layer and a buried oxide layer connected in sequence, a strip waveguide, a taper structure and a top silicon layer connected in sequence are arranged on the buried oxide layer, and the strip waveguide and the taper structure are connected to the Ge 1-x Sn x The absorption region is located at the same center along the direction of light propagation;
[0008] The hollow silica template cavity is arranged above the top silicon layer of the SOI substrate, a bottom window is arranged at the bottom silica layer of the silica template cavity to expose a portion of the top silicon layer of the SOI substrate, and an electrode hole is arranged at the top silica layer of the silica template cavity;
[0009] The Ge 1-x Sn x The absorption zone is arranged in the hollow silicon dioxide template cavity, and the Ge 1-x Sn x The absorption region includes a germanium buffer layer and a Ge 1-x Sn x The germanium buffer layer is arranged in the cavity between the bottom window and the top of the hollow silicon dioxide template cavity in a direction perpendicular to the top silicon layer; the Ge 1-x Sn x The absorption layer includes a P-type doped layer, an intrinsic layer and an N-type doped layer connected in sequence, wherein the P-type doped layer is connected to the germanium buffer layer, wherein 0≤x≤1;
[0010] The electrode is arranged above the hollow silica template cavity, and is connected to the Ge through the electrode hole at the top of the hollow silica template cavity. 1-x Sn x The absorption region is electrically connected.
[0011] Advantages and technical effects brought by the waveguide-coupled photodetector of the embodiment of the present invention:
[0012] 1. The waveguide coupled photodetector of the embodiment of the present invention does not directly set Ge on the SOI substrate. 1-x Sn x Instead of setting a hollow silicon dioxide template cavity, a window is set at the bottom of the silicon dioxide template cavity to expose the top silicon layer of the SOI substrate, and a germanium buffer layer is set at the bottom window of the silicon dioxide template cavity to reduce the area of the silicon-germanium heterogeneous interface. 1-x Sn x The absorption layer forms a lateral PIN photodetector structure in the hollow silicon dioxide template cavity. In the waveguide-coupled photodetector structure of the embodiment of the present invention, the optical signal is coupled into the Ge through the extremely thin silicon dioxide layer at the bottom of the silicon dioxide template cavity by evanescent wave coupling. 1-x Sn x The absorption layer does not pass through the germanium-silicon heterojunction, thus effectively reducing the loss and attenuation of the original high-density defects and dislocations at the germanium-silicon interface on the optical signal, significantly weakening the adverse effects of interface defects on carrier transmission, and achieving an effective photogenerated carrier absorption rate of up to 94.5% in the absorption region, and a light response of 1.2A / W at 1310nm. Compared with the existing technology of directly setting Ge on the SOI substrate 1-x Sn x The absorption layer, the waveguide-coupled photodetector of the embodiment of the present invention can effectively enhance the light response of the device, reduce the dark current level of the device, and open up a new way to optimize the photoelectric conversion efficiency;
[0013] 2. The waveguide-coupled photodetector of the embodiment of the present invention effectively improves the absorption rate of photogenerated carriers. Under the premise of maintaining the same level of photogenerated carrier absorption efficiency, the device design can be streamlined to achieve a smaller size and area. This transformation not only reduces the demand for raw materials and reduces resource consumption in the production process, but also promotes the development of optoelectronic components towards higher integration and more refinement, laying a solid foundation for the future development of optoelectronic integration technology.
[0014] In some embodiments, the thickness of the bottom silica layer of the hollow silica template cavity is 20 nm to 100 nm, preferably 50 nm.
[0015] In some embodiments, the bottom window of the hollow silica template cavity has a length of 10-12 μm and a width of 2-3 μm.
[0016] The present invention also discloses a method for preparing a waveguide coupled photoelectric detector, comprising the following steps:
[0017] a. forming a buried oxide layer on a silicon substrate, depositing a silicon layer on the buried oxide layer, and processing the silicon layer to obtain a strip waveguide, a taper structure and a top silicon layer to obtain an SOI substrate;
[0018] b. A hollow silica template cavity matrix is fabricated on the top silicon layer, a bottom window is opened on the bottom silica layer of the silica template cavity matrix to expose a portion of the top silicon layer, and a window is opened at the other end of the silica template cavity matrix in a horizontal direction and away from the bottom window;
[0019] c. Depositing a germanium buffer layer at the bottom window in the silicon dioxide template cavity matrix, so that the germanium buffer layer grows to the top of the silicon dioxide template cavity matrix in a direction perpendicular to the top silicon layer, and continuing to sequentially grow a P-type doped layer, an intrinsic layer and an N-type doped layer outside the germanium buffer layer to form a Ge 1-x Sn x The absorption layer, wherein 0≤x≤1, is completed in the hollow silica template cavity matrix. 1-x Sn x Preparation of the absorption zone;
[0020] d. In the Ge 1-x Sn x Depositing a silicon dioxide layer outside the absorption region to seal the hollow silicon dioxide template cavity matrix to form a hollow silicon dioxide template cavity;
[0021] e. Making an electrode on the top of the hollow silicon dioxide template cavity and connecting it to the Ge 1-x Sn x The absorption regions are electrically connected to prepare a waveguide-coupled photodetector.
[0022] Advantages and technical effects of the method for preparing a waveguide-coupled photodetector according to an embodiment of the present invention:
[0023] 1. The method of the embodiment of the present invention adopts a template-assisted epitaxy method to prepare Ge 1-x Sn x Waveguide coupled photodetector, Ge is not grown directly on SOI substrate 1-x Sn x Instead, a hollow silicon dioxide template cavity substrate is prepared first, a window is opened at the bottom of the template cavity substrate to expose the top silicon layer, and a germanium buffer layer and Ge are epitaxially grown at the bottom window of the silicon dioxide template cavity substrate.1-x Sn x The absorption layer is formed to form a lateral PIN photodetector structure; in the photodetector prepared by the embodiment of the present invention, the optical signal is coupled into the Ge through the extremely thin silicon dioxide layer at the bottom of the silicon dioxide template cavity by evanescent wave coupling, not through the germanium silicon heterojunction. 1-x Sn x The absorption layer effectively reduces the loss and attenuation of optical signals caused by the high-density defects and dislocations at the original germanium-silicon interface, significantly weakens the adverse effects of interface defects on carrier transmission, and achieves an effective photogenerated carrier absorption rate of up to 94.5% in the absorption region;
[0024] 2. Compared with the prior art, the method of the embodiment of the present invention directly grows Ge on the SOI substrate. 1-x Sn x The absorption layer has a photoresponsivity of 1.2A / W at 1310nm, which effectively enhances the photoresponsivity of the device and reduces the dark current level of the device, opening up a new way to optimize the photoelectric conversion efficiency;
[0025] 3. The method of the embodiment of the present invention can effectively improve the absorption rate of photogenerated carriers. Under the premise of maintaining the same level of photogenerated carrier absorption efficiency, the device design can be simplified and the size and area of the device can be reduced. This change not only reduces the demand for raw materials, but also reduces the resource consumption in the production process, and further promotes the development of optoelectronic components towards higher integration and more sophisticated directions.
[0026] In some embodiments, in step b, the method for making the hollow silica template cavity matrix includes:
[0027] b1, depositing silicon dioxide on the top silicon layer to form a bottom silicon dioxide layer, and processing a bottom window on the bottom silicon dioxide layer to expose a portion of the top silicon layer;
[0028] b2, depositing a silicon layer on the bottom silicon dioxide layer, processing the silicon layer and depositing silicon dioxide around the silicon layer to form a silicon dioxide coating layer, so that the silicon layer is surrounded by the silicon dioxide coating layer;
[0029] b3. A window is opened on the silica coating layer, wherein the window and the bottom window are located at both ends of the silicon layer in the horizontal direction, and the silicon layer is removed through the window to expose the top silicon layer at the bottom window, thereby obtaining a hollow silica template cavity substrate.
[0030] In some embodiments, in step b1 and / or step b2, the silicon dioxide is deposited by a method including thermal oxidation, atmospheric pressure chemical vapor deposition, low pressure chemical vapor deposition or plasma chemical vapor deposition.
[0031] In some embodiments, in step b2, the silicon layer is made of polycrystalline silicon or amorphous silicon; and / or, the silicon layer is deposited by plasma chemical vapor deposition.
[0032] In some embodiments, in step b3, the method of removing the silicon layer includes etching the silicon layer using wet etching.
[0033] In some embodiments, in the step b1, the processing method of the bottom window includes processing the silicon dioxide layer by electron beam exposure or inductively coupled plasma etching.
[0034] In some embodiments, in step b3, the processing method of the window on the silicon dioxide coating layer includes processing the silicon dioxide coating layer by electron beam exposure or inductively coupled plasma etching.
[0035] In some embodiments, in step c, the growth method of the germanium buffer layer, the P-type doping layer, the intrinsic layer or the N-type doping layer includes at least one of a chemical vapor deposition method and a high temperature diffusion method.
[0036] In some embodiments, in step e, the preparation of the electrode includes: preparing an electrode hole on the top of the hollow silica template cavity by electron beam exposure or inductively coupled plasma etching, and evaporating metal in the electrode hole by electron beam evaporation to obtain the electrode; preferably, the metal includes at least one of Ni, Cr, Ti, and Au. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 3 is a schematic diagram of the structure of a waveguide-coupled photodetector according to an embodiment of the present invention, in which the direction in which light propagates in the waveguide is parallel to the x-axis in the device coordinate axis.
[0038] Figure 2a-2m is a schematic flow chart of a method for preparing a waveguide-coupled photodetector according to an embodiment of the present invention;
[0039] a: forming a buried oxide layer on a silicon substrate; b: obtaining an SOI substrate; c: forming a bottom silicon dioxide layer of a hollow silicon dioxide template cavity; d: opening a bottom window on the bottom silicon dioxide layer of the silicon dioxide template cavity; e: depositing a silicon layer on the bottom silicon dioxide layer; f: thinning the silicon layer; g: patterning the silicon layer; h: depositing a silicon dioxide coating layer outside the silicon layer; i: opening a window on the silicon dioxide coating layer; j: removing the silicon layer; k: forming a Ge 1-x Sn x Absorption region; l: in Ge 1-x Sn x Silicon dioxide is deposited outside the absorption region; m: electrode preparation.
[0040] Figure 3 This is a side light field distribution diagram of the waveguide-coupled photodetector prepared in Example 1 of the present invention.
[0041] Figure 4 This is a diagram of the photogenerated carrier absorption power of the waveguide-coupled photodetector prepared in Example 1 of the present invention.
[0042] Figure 5 This is a light response curve diagram of the waveguide-coupled photodetector manufactured in Example 1 of the present invention under different bias voltages.
[0043] Figure 6 Schematic diagram of the structure of the waveguide coupled photodetector of comparative example 1.
[0044] Figure 7 This is a photoresponsivity curve of the waveguide-coupled photodetector of comparative example 1 under different bias voltages.
[0045] Reference numerals: SOI substrate 100; silicon substrate layer 110; buried oxide layer 120; top silicon layer 130; strip waveguide 140; taper structure 150; bottom silicon dioxide layer 200; silicon layer 300; silicon dioxide template layer 400; Ge 1-x Sn x Absorption region 500 ; electrode 600 . DETAILED DESCRIPTION
[0046] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.
[0047] like Figure 1 As shown, the waveguide coupled photodetector of the embodiment of the present invention comprises: an SOI substrate 100, a hollow silicon dioxide template cavity, a Ge 1-x Sn x The SOI substrate 100 includes a silicon substrate layer 110 and a buried oxide layer 120 connected in sequence, and a strip waveguide 140, a taper structure 150 and a top silicon layer 130 connected in sequence are arranged on the buried oxide layer 120. The strip waveguide 140, the taper structure 150 and the Ge 1-x Sn x The absorption region 500 is located at the same center along the light propagation direction. The taper structure 150 is used for the strip waveguide 140 and the Ge 1-x Sn x The light field width between the absorption regions 500 is transitional.
[0048] The hollow silica template cavity is composed of a bottom silica layer 200 and a silica template layer 400. The bottom silica layer 200 is disposed above the top silicon layer 130 of the SOI substrate 100, a bottom window is disposed on the bottom silica layer 200 to expose a portion of the top silicon layer 130, and an electrode hole is disposed in the top silica layer of the hollow silica template cavity.
[0049] Ge 1-x Sn x The absorption region 500 is set in the hollow silicon dioxide template cavity. 1-x Sn x The absorption region 500 includes a germanium buffer layer and a Ge 1-x Sn x The absorption layer and the germanium buffer layer are arranged in the cavity between the bottom window and the top of the bottom silicon dioxide layer 200 of the silicon dioxide template cavity in a direction perpendicular to the top silicon layer 130; Ge 1-x Sn x The absorption layer includes a P-type doped layer, an intrinsic layer and an N-type doped layer which are connected in sequence, and the P-type doped layer is connected to the germanium buffer layer, wherein 0≤x≤1.
[0050] The electrode 600 is disposed above the hollow silicon dioxide template cavity and is connected to the Ge 1-x Sn x The absorption region 500 is electrically connected.
[0051] The waveguide coupled photodetector of the embodiment of the present invention does not directly set Ge on the SOI substrate. 1-x Sn x Instead of setting a hollow silicon dioxide template cavity, a window is set at the bottom of the silicon dioxide template cavity to expose the top silicon layer of the SOI substrate, and a germanium buffer layer is set at the bottom window of the silicon dioxide template cavity to reduce the area of the silicon-germanium heterogeneous interface. A Ge1-xSnx absorption layer is set outside the germanium buffer layer to form a lateral PIN photodetector structure in the hollow silicon dioxide template cavity. In the waveguide-coupled photodetector structure of the embodiment of the present invention, the optical signal is coupled into the Ge through the extremely thin silicon dioxide layer at the bottom of the silicon dioxide template cavity by evanescent wave coupling. 1-x Sn x The absorption layer does not pass through the germanium-silicon heterojunction, thus effectively reducing the loss and attenuation of the original high-density defects and dislocations at the germanium-silicon interface on the optical signal, significantly weakening the adverse effects of interface defects on carrier transmission, and achieving an effective photogenerated carrier absorption rate of up to 94.5% in the absorption region. 1-x Sn xIn the absorption region, the waveguide-coupled photodetector of the embodiment of the present invention can effectively enhance the light responsivity of the device and reduce the dark current level of the device. The light responsivity at 1310 nm is 1.2 A / W, which opens up a new way to optimize the photoelectric conversion efficiency.
[0052] The waveguide-coupled photodetector of the embodiment of the present invention effectively improves the absorption rate of photogenerated carriers. Under the premise of maintaining the same level of photogenerated carrier absorption efficiency, the device design can be streamlined to achieve a smaller size and area. This transformation not only reduces the demand for raw materials and reduces resource consumption in the production process, but also promotes the development of optoelectronic components towards higher integration and more refinement, laying a solid foundation for the future development of optoelectronic integration technology.
[0053] In some embodiments, the thickness of the silicon dioxide layer 200 at the bottom of the silicon dioxide template cavity is 20nm to 100nm, preferably 50nm. In the embodiment of the present invention, the thickness of the silicon dioxide layer at the bottom of the silicon dioxide template cavity is preferably selected so that the optical signal is coupled into the Ge through the extremely thin silicon dioxide layer. 1-x Sn x The absorption layer is beneficial to improving the absorption efficiency of the absorption layer, reducing the dark current level of the device, and enhancing the light response of the device.
[0054] In some embodiments, the bottom window of the silicon dioxide template cavity has a length of 10-12 μm and a width of 2-3 μm. In the embodiment of the present invention, the top silicon layer of the SOI substrate is exposed at the bottom window of the silicon dioxide template cavity, and a germanium buffer layer is arranged at the window to further realize epitaxial growth of Ge. 1-x Sn x The embodiment of the present invention has no particular limitation on the size of the bottom window, as long as a germanium buffer layer can be grown on the top silicon layer exposed at the window.
[0055] The present invention also provides a method for preparing a waveguide-coupled photodetector, comprising the following steps:
[0056] a. forming a buried oxide layer on a silicon substrate, depositing a silicon layer on the buried oxide layer, and processing the silicon layer to obtain a strip waveguide, a taper structure and a top silicon layer to obtain an SOI substrate;
[0057] b. A hollow silica template cavity matrix is fabricated on the top silicon layer, a bottom window is opened on the bottom silica layer of the silica template cavity matrix to expose a portion of the top silicon layer, and a window is opened at the other end of the silica template cavity matrix in a horizontal direction and away from the bottom window;
[0058] c. Depositing a germanium buffer layer at the bottom window in the silicon dioxide template cavity matrix, so that the germanium buffer layer grows to the top of the silicon dioxide template cavity matrix in a direction perpendicular to the top silicon layer, and continuing to sequentially grow a P-type doped layer, an intrinsic layer and an N-type doped layer outside the germanium buffer layer to form a Ge 1-x Sn x The absorption layer, wherein 0≤x≤1, is completed in the hollow silica template cavity matrix. 1-x Sn x Preparation of the absorption zone;
[0059] d. In the Ge 1-x Sn x Depositing a silicon dioxide layer outside the absorption region to seal the hollow silicon dioxide template cavity matrix to form a hollow silicon dioxide template cavity;
[0060] e. Making an electrode on the top of the hollow silicon dioxide template cavity and connecting it to the Ge 1-x Sn x The absorption regions are electrically connected to prepare a waveguide-coupled photodetector.
[0061] The method of the embodiment of the present invention adopts the template-assisted epitaxy method to prepare Ge 1-x Sn x Waveguide coupled photodetector, Ge is not grown directly on SOI substrate 1-x Sn x Instead, a hollow silicon dioxide template cavity substrate is prepared first, a window is opened at the bottom of the template cavity substrate to expose the top silicon layer, and a germanium buffer layer and Ge are epitaxially grown at the bottom window of the silicon dioxide template cavity substrate. 1-x Sn x The absorption layer is formed to form a lateral PIN photodetector structure; in the photodetector prepared by the embodiment of the present invention, the optical signal is coupled into the Ge through the extremely thin silicon dioxide layer at the bottom of the silicon dioxide template cavity by evanescent wave coupling, not through the germanium silicon heterojunction. 1-x Sn x The absorption layer effectively reduces the loss and attenuation of optical signals caused by the original high-density defects and dislocations at the germanium-silicon interface, significantly weakens the adverse effects of interface defects on carrier transmission, and achieves an effective photogenerated carrier absorption rate of up to 94.5% in the absorption region.
[0062] Compared with the prior art, the method of the embodiment of the present invention directly grows Ge on the SOI substrate. 1-x Sn x The absorption layer effectively enhances the photoresponsivity of the device and reduces the dark current level of the device. The photoresponsivity at 1310nm is 1.2A / W, which opens up a new way to optimize the photoelectric conversion efficiency.
[0063] The method of the embodiment of the present invention can effectively improve the absorption rate of photogenerated carriers. Under the premise of maintaining the same level of photogenerated carrier absorption efficiency, the device design can be simplified and the size and area of the device can be reduced. This transformation not only reduces the demand for raw materials, but also reduces the resource consumption in the production process, and further promotes the development of optoelectronic components towards higher integration and more sophisticated directions.
[0064] In some embodiments, in step b, the method for making the hollow silica template cavity matrix includes:
[0065] b1, depositing silicon dioxide on the top silicon layer to form a bottom silicon dioxide layer, and processing a bottom window on the bottom silicon dioxide layer to expose a portion of the top silicon layer;
[0066] b2, depositing a silicon layer on the bottom silicon dioxide layer, processing the silicon layer and depositing silicon dioxide around the silicon layer to form a silicon dioxide coating layer, so that the silicon layer is surrounded by the silicon dioxide coating layer;
[0067] b3. A window is opened on the silica coating layer, wherein the window and the bottom window are located at both ends of the silicon layer in the horizontal direction, and the silicon layer is removed through the window to expose the top silicon layer at the bottom window, thereby obtaining a hollow silica template cavity substrate.
[0068] The embodiment of the present invention has no particular limitation on the window opened on the silicon dioxide coating layer in step b3, as long as the silicon layer can be removed and a germanium buffer layer, a P-type doped layer, an intrinsic layer or an N-type doped layer can be deposited through the window in the subsequent process to form a Ge 1-x Sn x The absorption zone can be applicable to the embodiments of the present invention.
[0069] In some embodiments, in step b1 and / or step b2, the deposition method of silicon dioxide includes thermal oxidation, atmospheric pressure chemical vapor deposition, low pressure chemical vapor deposition or plasma chemical vapor deposition. The low pressure chemical vapor deposition method (also called LP-CVD) of the embodiment of the present invention refers to a chemical vapor deposition method performed under conditions below one atmosphere.
[0070] In some embodiments, in step b2, the silicon layer is made of polycrystalline silicon or amorphous silicon.
[0071] In some embodiments, in step b2, the deposition method of the silicon layer includes plasma chemical vapor deposition.
[0072] In some embodiments, in step b3, the method of removing the silicon layer includes etching the silicon layer using wet etching.
[0073] In some embodiments, in the step b1, the processing method of the bottom window includes processing the silicon dioxide layer by electron beam exposure or inductively coupled plasma etching.
[0074] In some embodiments, in step b3, the processing method of the window on the silicon dioxide coating layer includes processing the silicon dioxide coating layer by electron beam exposure or inductively coupled plasma etching.
[0075] In some embodiments, in step c, the growth method of the germanium buffer layer, the P-type doping layer, the intrinsic layer or the N-type doping layer includes at least one of a chemical vapor deposition method and a high temperature diffusion method.
[0076] In some embodiments, in step e, the preparation of the electrode includes: preparing an electrode hole on the top of the hollow silica template cavity by electron beam exposure or inductively coupled plasma etching, and evaporating metal in the electrode hole by electron beam evaporation to obtain the electrode; preferably, the metal includes at least one of Ni, Cr, Ti, and Au.
[0077] The method for preparing the waveguide-coupled photodetector according to the embodiment of the present invention is described in detail below with reference to the embodiments and drawings.
[0078] Example 1 Preparation method of waveguide coupled photodetector
[0079] (1) Preparation of SOI substrate
[0080] like Figure 2a and 2b As shown, a buried oxide layer 120 with a thickness of 3 μm is formed on a silicon substrate 110, a silicon layer with a thickness of 220 nm is deposited on the buried oxide layer 120, an electron beam exposure technique is used to form a pattern on the silicon layer, and then an inductively coupled plasma etching process is used to obtain a strip waveguide 140 and a taper structure 150 (see Figure 1 ), the width of the strip waveguide 140 is 0.45 μm, the inlet width of the tapered structure 150 is 0.45 μm, the outlet width is 2 μm, and the length is 50 μm, and the SOI substrate 100 is manufactured.
[0081] (2) Preparation of hollow silica template cavity matrix
[0082] like Figure 2c A bottom silicon dioxide layer 200 with a thickness of 50 nm is deposited on the SOI substrate 100 by plasma chemical vapor deposition.
[0083] like Figure 2dAn electron beam exposure technique is used to form a pattern on the bottom silicon dioxide layer 200, and then an inductively coupled plasma etching process is used to form a bottom window on the bottom silicon dioxide layer 200, wherein the length of the bottom window is 10 μm and the width is 3 μm.
[0084] like Figure 2e A silicon layer 300 made of polycrystalline silicon is deposited on the bottom silicon dioxide layer 200 by plasma chemical vapor deposition. The thickness of the grown silicon layer 300 should be greater than the height of the PIN structure in the detector to be prepared.
[0085] like Figure 2f The size of the silicon layer 300 is thinned by chemical mechanical polishing until the thickness required by the detector is reached.
[0086] like Figure 2g , the silicon layer 300 is processed by electron beam exposure technology to meet Ge 1-x Sn x The size of the absorption region 500 is required. For example, the size of the processed silicon layer 300 is equal to the width of the Ge to be prepared in the direction of light propagation. 1-x Sn x The width of the absorption region 500 is consistent, which can be 10 μm; the length in the direction perpendicular to the light propagation direction should be greater than the Ge 1-x Sn x The absorption area is 500 mm long, and the excess length is about 2 to 3 μm. The length can be set to 22 μm. The part exceeding the detector length is Figure 2d The processed silicon dioxide layer 200 corresponds to the window. The thickness of the silicon layer 300 after processing is 0.5 μm.
[0087] like Figure 2h , silicon dioxide is deposited around the silicon layer 300 using a plasma chemical vapor deposition method to form a silicon dioxide coating layer.
[0088] like Figure 2i , using electron beam exposure technology Figure 2h A silicon dioxide coating layer is formed in the process, and a window is opened to expose the silicon layer 300 coated thereon. Figure 2c The bottom windows opened in the bottom silicon dioxide layer 200 are respectively located at two ends of the silicon layer 300 in the horizontal direction, that is, at two ends of the detector to be manufactured.
[0089] like Figure 2j ,pass Figure 2i The window opened in the middle silicon dioxide coating layer is completely etched by wet etching to completely etch the silicon layer 300 until the top silicon layer 130 below the bottom window opened in the bottom silicon dioxide layer 200 is exposed, thereby forming a hollow silicon dioxide template cavity matrix.
[0090] (3) Preparation of Ge 1-x Sn x Absorption area
[0091] like Figure 2k , using ultra-high vacuum chemical vapor deposition (UHV / CVD at less than 10 -6 A germanium buffer layer is first grown at the bottom window opened by the bottom silicon dioxide layer 200, and then Ge is sequentially prepared on the germanium buffer layer by a high temperature diffusion method. 1-x Sn x The P-type doped layer, intrinsic layer, and N-type doped layer of the layer finally form Ge 1-x Sn x Absorption zone 500.
[0092] (5) Preparation of hollow silica template cavity
[0093] like Figure 2l , using chemical vapor deposition technology, in the PIN structure formed above, that is, Ge 1-x Sn x A layer of silicon dioxide is deposited on the absorption region 500, and passivation treatment is performed to seal the silicon dioxide template cavity matrix to form a silicon dioxide template layer 400. The silicon dioxide template layer 400 and the bottom silicon dioxide layer 200 form a hollow silicon dioxide template cavity, and the interior of the cavity is coated with Ge 1-x Sn x Absorption zone 500.
[0094] (5) Preparation of electrodes
[0095] like Figure 2l An electrode pattern is formed on the top of the silicon dioxide template cavity by electron beam exposure, and an inductively coupled plasma etching technique is used to etch the top silicon dioxide layer of the silicon dioxide template cavity to form an electrode hole.
[0096] like Figure 2m Electron beam evaporation technology is used to evaporate metal Ni in the electrode hole to form a metal electrode 600, which is connected to Ge 1- x Sn x The absorption regions 500 are electrically connected to prepare a waveguide-coupled photodetector.
[0097] The performance of the waveguide coupled photodetector prepared in this embodiment was tested, and the test results are shown in Figure 3-5 .
[0098] Test conditions: The waveguide coupled photodetector was tested under a 1310nm single mode light source.
[0099] Figure 3This is a side light field distribution diagram of the waveguide coupled photodetector obtained in Example 1. The numerical value represents the electric field intensity. The larger the numerical value, the greater the electric field intensity, and the greater the light field intensity at the corresponding position. Figure 3 As shown, light propagates along the strip waveguide 140 and the taper structure 150 to the device, and is coupled upward to the Ge by means of an evanescent wave. 1-x Sn x Absorption region 500. Ge 1-x Sn x The light field intensity is the largest at the front end of the absorption region, and gradually decays along the x direction as the light propagates, and the light field intensity decays to a very small level at the end of the device.
[0100] Figure 4 The figure is a diagram of the absorption power of photogenerated carriers of the waveguide-coupled photodetector prepared in Example 1. The waveguide-coupled photodetector prepared in Example 1 effectively reduces the influence of defects at the germanium-silicon heterointerface on carriers, so that the effective absorption rate of photogenerated carriers in the absorption region reaches 94.5%.
[0101] Figure 5 The photoresponsivity curve of the waveguide coupled photodetector prepared in Example 1 under different bias voltages is shown in FIG. Figure 5 As shown, under a reverse bias voltage of -1 V, the photoresponsivity of the waveguide-coupled photodetector at 1310 nm is 1.2 A / W, which can achieve a high photoresponsivity.
[0102] Comparative Example 1
[0103] Comparative Example 1 is a waveguide coupled photodetector used in the prior art, and its structure is as follows: Figure 6 As shown, including SOI substrate, Ge 1-x Sn x Absorption region and electrode; the SOI substrate comprises a silicon substrate layer and a buried oxide layer connected in sequence, on which a strip waveguide (not shown in the figure), a taper structure (not shown in the figure) and a top silicon layer connected in sequence are arranged.
[0104] The main difference from Example 1 is that in Example 1, a germanium buffer layer and a Ge 1- x Sn x The absorption layer forms Ge 1-x Sn x Absorption region, Ge 1-x Sn x The size of the absorption region is the same as that of the photodetector in Example 1.
[0105] The performance of the waveguide coupled photodetector of this comparative example was tested, and the test results are shown in Figure 7 .
[0106] Figure 7: is a light response curve of the waveguide coupled photodetector of comparative example 1 under different bias voltages. Figure 7 As shown, under a reverse bias voltage of -1 V, the photoresponsivity of the photodetector at 1310 nm is only 0.96 A / W.
[0107] The photodetector of Comparative Example 1 has a distinct germanium-silicon heterogeneous interface in its structure, and the high-density defects and dislocations therein will cause loss and attenuation of the optical signal, which will have an adverse effect on the photoresponsivity of the device, resulting in the photoresponsivity of the photodetector being only 0.96A / W at 1310nm. The photodetector of the embodiment of the present invention does not directly grow Ge on the SOI substrate. 1-x Sn x Instead, a hollow silicon dioxide template cavity is set up, and a germanium buffer layer and Ge are sequentially deposited on the top silicon layer exposed by the bottom window of the silicon dioxide template cavity. 1-x Sn x The absorption layer forms a lateral PIN photodetector structure in the silicon dioxide template cavity. The optical signal is coupled into the Ge through the extremely thin silicon dioxide layer at the bottom of the silicon dioxide template cavity through the evanescent wave coupling method, without passing through the germanium-silicon heterojunction. 1-x Sn x The absorption layer significantly weakens the adverse effects of interface defects and significantly improves the light response.
[0108] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0109] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A waveguide coupled photodetector, characterized in that: include: SOI substrate, hollow silica template cavity, Ge 1-x Sn x Absorption zone and electrodes; The SOI substrate comprises a silicon substrate layer and a buried oxide layer connected in sequence, a strip waveguide, a taper structure and a top silicon layer connected in sequence are arranged on the buried oxide layer, and the strip waveguide and the taper structure are connected to the Ge 1-x Sn x The absorption region is located at the same center along the direction of light propagation; The hollow silica template cavity is arranged above the top silicon layer of the SOI substrate, a bottom window is arranged at the bottom silica layer of the silica template cavity to expose a portion of the top silicon layer of the SOI substrate, and an electrode hole is arranged at the top silica layer of the silica template cavity; The Ge 1-x Sn x The absorption zone is arranged in the hollow silicon dioxide template cavity, and the Ge 1-x Sn x The absorption region includes a germanium buffer layer and a Ge 1-x Sn x The germanium buffer layer is arranged in the cavity between the bottom window and the top of the hollow silicon dioxide template cavity in a direction perpendicular to the top silicon layer; the Ge 1-x Sn x The absorption layer includes a P-type doped layer, an intrinsic layer and an N-type doped layer connected in sequence, wherein the P-type doped layer is connected to the germanium buffer layer, wherein 0≤x≤1; The electrode is arranged above the hollow silica template cavity, and is connected to the Ge through the electrode hole at the top of the hollow silica template cavity. 1-x Sn x The absorption region is electrically connected.
2. The waveguide coupled photodetector according to claim 1, characterized in that: The thickness of the bottom silica layer of the hollow silica template cavity is 20 nm-100 nm, preferably 50 nm.
3. The waveguide coupled photodetector according to claim 1, characterized in that: The bottom window of the hollow silica template cavity has a length of 10-12 μm and a width of 2-3 μm.
4. A method for preparing a waveguide coupled photodetector, characterized in that: The steps include: a. forming a buried oxide layer on a silicon substrate, depositing a silicon layer on the buried oxide layer, and processing the silicon layer to obtain a strip waveguide, a taper structure and a top silicon layer to obtain an SOI substrate; b. A hollow silica template cavity matrix is fabricated on the top silicon layer, a bottom window is opened on the bottom silica layer of the silica template cavity matrix to expose a portion of the top silicon layer, and a window is opened at the other end of the silica template cavity matrix in a horizontal direction and away from the bottom window; c. Depositing a germanium buffer layer at the bottom window in the silicon dioxide template cavity matrix, so that the germanium buffer layer grows to the top of the silicon dioxide template cavity matrix in a direction perpendicular to the top silicon layer, and continuing to sequentially grow a P-type doped layer, an intrinsic layer and an N-type doped layer outside the germanium buffer layer to form a Ge 1-x Sn x The absorption layer, wherein 0≤x≤1, is completed in the hollow silica template cavity matrix. 1-x Sn x Preparation of the absorption zone; d. In the Ge 1-x Sn x Depositing a silicon dioxide layer outside the absorption region to seal the hollow silicon dioxide template cavity matrix to form a hollow silicon dioxide template cavity; e. Making an electrode on the top of the hollow silicon dioxide template cavity and connecting it to the Ge 1-x Sn x The absorption regions are electrically connected to prepare a waveguide-coupled photodetector.
5. The method for preparing a waveguide-coupled photodetector according to claim 4, characterized in that: In the step b, the method for preparing the hollow silica template cavity matrix comprises: b1, depositing silicon dioxide on the top silicon layer to form a bottom silicon dioxide layer, and processing a bottom window on the bottom silicon dioxide layer to expose a portion of the top silicon layer; b2, depositing a silicon layer on the bottom silicon dioxide layer, processing the silicon layer and depositing silicon dioxide around the silicon layer to form a silicon dioxide coating layer, so that the silicon layer is surrounded by the silicon dioxide coating layer; b3. A window is opened on the silica coating layer, wherein the window and the bottom window are located at both ends of the silicon layer in the horizontal direction, and the silicon layer is removed through the window to expose the top silicon layer at the bottom window, thereby obtaining a hollow silica template cavity substrate.
6. The method for preparing a waveguide-coupled photodetector according to claim 5, characterized in that: In step b1 and / or step b2, the silicon dioxide is deposited in a manner including thermal oxidation, atmospheric pressure chemical vapor deposition, low pressure chemical vapor deposition or plasma chemical vapor deposition.
7. The method for preparing a waveguide-coupled photodetector according to claim 5, characterized in that: In the step b2, the silicon layer is made of polycrystalline silicon or amorphous silicon; and / or the silicon layer is deposited by plasma chemical vapor deposition; In the step b3, the method of removing the silicon layer includes etching the silicon layer by wet etching.
8. The method for preparing a waveguide-coupled photodetector according to claim 5, characterized in that: In the step b1, the processing method of the bottom window includes processing the silicon dioxide layer by electron beam exposure or inductively coupled plasma etching; And / or, in the step b3, the processing method of the window on the silicon dioxide coating layer includes processing the silicon dioxide coating layer by electron beam exposure or inductively coupled plasma etching.
9. The method for preparing a waveguide-coupled photodetector according to claim 4, characterized in that: In the step c, the growth method of the germanium buffer layer, the P-type doping layer, the intrinsic layer or the N-type doping layer includes at least one of a chemical vapor deposition method and a high temperature diffusion method.
10. The method for preparing a waveguide-coupled photodetector according to claim 4, characterized in that: In the step e, the preparation of the electrode comprises: preparing an electrode hole on the top of the hollow silica template cavity by electron beam exposure or inductively coupled plasma etching, and evaporating metal in the electrode hole by electron beam evaporation to obtain the electrode; Preferably, the metal includes at least one of Ni, Cr, Ti and Au.
Citation Information
Patent Citations
Photodetector and method of manufacture thereof
CN112534590A
All-silicon-doped multi-junction electric field enhanced germanium optical waveguide detector
CN113035982A
Germanium-silicon photoelectric detector
CN115832095A
Surface plasmon nano-cavity integrated nano air channel optical mixer
CN115954402A
Co-Integration of Photonic Devices on a Silicon Photonics Platform
US20120288971A1
Cited By
High-performance surface incidence silicon-based germanium detector structure and preparation method thereof
CN122002916A
A high-performance face incidence germanium-on-silicon detector structure and a preparation method thereof
CN122002916B