Negative electrode active material composition for lithium secondary battery, negative electrode comprising same, and lithium secondary battery
By using a silicon-based negative electrode active material combined with SiC or SiOx in a lithium secondary battery, the problem of increasing current density caused by the silicon-based negative electrode active material is solved, and the durability and resistance of the battery are improved. Features, achieving high energy density and high capacity battery performance.
Patent Information
- Application Number
- CN202410601274.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-05-15
- Publication Date
- 2024-11-22
AI Technical Summary
The use of silicon-based negative electrode active substances in lithium secondary batteries leads to an increase in current density, reducing the durability and resistance characteristics of the negative electrode, and affecting the life and performance of the battery.
Using a combination of carbon-based negative electrode active material and silicon-based negative electrode active material, the carbon-based negative electrode active material has a low orientation, and the silicon-based negative electrode active material contains SiC or SiOx, and the electrode insertion and deintercalation characteristics are improved by forming a porous structure. , ensure the durability of the negative electrode.
The resistance and life characteristics of lithium secondary batteries are improved, the durability and initial charging and discharging efficiency of the battery are enhanced, and the battery performance is ensured with high energy density and high capacity.
Smart Images

Figure BDA0004840651780000091 
Figure BDA0004840651780000101
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode active material composition for a lithium secondary battery, a negative electrode comprising the negative electrode active material composition, and a lithium secondary battery. Background Art
[0002] In recent years, as concerns about environmental issues have increased, exhaust gas emitted by vehicles using fossil fuels such as gasoline and diesel has been designated as one of the main causes of air pollution, and as a means to replace it, a lot of research is being conducted on electric vehicles (EVs), hybrid electric vehicles (HEVs), etc.
[0003] At the same time, as a power source for such electric vehicles (EVs), hybrid electric vehicles (HEVs), etc., lithium secondary batteries with high discharge voltage and power stability are mainly used. In addition, with the increase in demand for high-energy secondary batteries with high energy density, the development and research of high-capacity negative electrodes are being actively carried out for this purpose. Therefore, in recent years, in order to realize secondary batteries with high capacity and high energy density, silicon-based negative electrode active materials with higher discharge capacity than carbon-based negative electrode active materials are applied in negative electrodes for secondary batteries.
[0004] However, when a silicon-based negative electrode active material is used for the negative electrode, the current density applied to the carbon-based negative electrode active material increases, resulting in reduced durability of the negative electrode, thereby causing problems such as reduced resistance characteristics and life characteristics of lithium secondary batteries. Summary of the invention
[0005] Technical issues to be solved
[0006] An object of the present invention is to provide a negative electrode active material composition for a lithium secondary battery that improves the resistance characteristics and life characteristics of the secondary battery, and a negative electrode and a lithium secondary battery comprising the negative electrode active material composition.
[0007] Technical Solution
[0008] According to one aspect of the present invention, there is provided a negative electrode active material composition for a lithium secondary battery, comprising a carbon-based negative electrode active material and a silicon-based negative electrode active material, wherein the carbon-based negative electrode active material has an orientation degree (I) of less than 2.85 measured by X-ray diffraction (XRD). 004 / I 110 , where I 004 is the peak intensity of the (004) plane when XRD measurement is performed on the carbon-based negative electrode active material, I 110 is the peak intensity of the (110) plane when performing XRD measurement on the carbon-based negative electrode active material).
[0009] The silicon-based negative electrode active material may include SiC or SiO x (0 <x<2)。
[0010] The negative electrode active material composition may include 2 wt % or more of the silicon-based negative electrode active material based on the total weight of the negative electrode active material composition.
[0011] The silicon-based negative electrode active material may include SiC having a porous structure.
[0012] The silicon-based negative active material may include: carbon-based particles including pores; and a silicon-based coating layer formed on the pores or surfaces of the carbon-based particles.
[0013] According to another aspect of the present invention, a negative electrode for a lithium secondary battery is provided, comprising: a negative electrode current collector; and a negative electrode mixture layer formed on at least one side of the negative electrode current collector, wherein the negative electrode mixture layer comprises the negative electrode active material composition, a negative electrode conductive material and a negative electrode binder.
[0014] The negative electrode mixture layer may be provided in two or more layers on the negative electrode collector.
[0015] According to another aspect of the present invention, a lithium secondary battery is provided, comprising the negative electrode.
[0016] Beneficial Effects
[0017] The negative electrode active material composition for a lithium secondary battery according to the present invention may include the carbon-based negative electrode active material and the silicon-based negative electrode active material, and the carbon-based negative electrode active material may have a low value of orientation. Therefore, even if the content of the silicon-based negative electrode active material in the negative electrode active material composition increases, the negative electrode can ensure durability, thereby improving the resistance characteristics and life characteristics of the secondary battery. DETAILED DESCRIPTION
[0018] Hereinafter, various embodiments according to the present invention will be described, but the embodiments may be modified into various other forms, and the scope thereof is not limited to the embodiments described below.
[0019] Negative electrode for lithium secondary battery
[0020] The negative electrode for a lithium secondary battery according to the present invention may include a negative electrode collector and a negative electrode mixture layer formed on at least one side of the negative electrode collector.
[0021] The negative electrode mixture layer may include a negative electrode active material composition, a negative electrode conductive material, and a negative electrode binder.
[0022] Negative electrode active material composition
[0023] The negative electrode active material composition may include a carbon-based negative electrode active material and a silicon-based negative electrode active material.
[0024] The carbon-based negative electrode active material is not particularly limited. For example, it may include at least one selected from artificial graphite, natural graphite, hard carbon, soft carbon, carbon black, acetylene black, Ketjen black, Super P, graphene, and fibrous carbon.
[0025] In an exemplary embodiment, the carbon-based negative electrode active material may include artificial graphite alone, or may include artificial graphite and natural graphite.
[0026] The silicon-based negative electrode active material may also be applicable to the present invention as long as it is a material that can generally be used as a negative electrode active material. For example, it may include at least one selected from SiC, SiO x (0 < x < 2), Si-Y alloy (where Y is an element selected from alkali metals, alkaline earth metals, transition metals, Group 13 elements, Group 14 elements, rare earth elements, and combinations thereof, and is not Si), Si-C composite, and pure Si.
[0027] In an exemplary embodiment, the silicon-based negative electrode active material may include SiC or SiO x (0 < x < 2).
[0028] In one embodiment, the silicon-based negative electrode active material may be SiC having a porous structure. Specifically, the silicon-based negative electrode active material may include carbon-based particles containing pores and a silicon-based coating formed on the pores or surface of the carbon-based particles. Since the silicon-based negative electrode active material has a porous structure, the volume expansion of the silicon-based negative electrode active material during charge and discharge of the secondary battery is suppressed. Therefore, the resistance characteristics, life characteristics, etc. of the secondary battery can be improved, and the initial charge and discharge efficiency of the silicon-based negative electrode active material is improved. Therefore, the initial efficiency of the secondary battery can be improved.
[0029] In one embodiment, based on the total weight of the negative electrode active material composition, the negative electrode active material composition may include 2% by weight or more of the silicon-based negative electrode active material. In addition, the negative electrode active material composition can improve the discharge capacity of the negative electrode including the negative electrode active material composition by including the silicon-based negative electrode active material. Based on the total weight of the negative electrode active material composition, if the negative electrode active material composition includes less than 2% by weight of the silicon-based negative electrode active material, the content of the silicon-based negative electrode active material included in the negative electrode active material composition is small, so the discharge capacity of the negative electrode may not be sufficiently improved.
[0030] In an exemplary embodiment, the carbon-based negative active material may have an orientation degree (I 004 / I 110 , where I 004 is the peak intensity of the (004) plane when XRD measurement is performed on the carbon-based negative electrode active material, I 110 is the peak intensity of the (110) plane when the carbon-based negative electrode active material is measured by XRD), the orientation degree (I 004 / I 110 ) can be a low value. In addition, when the content of the silicon-based negative electrode active material in the negative electrode active material composition increases, the current density applied to the carbon-based negative electrode active material increases, resulting in a decrease in the durability of the negative electrode containing the negative electrode active material composition, thereby reducing the resistance characteristics and life characteristics of the secondary battery. However, since the carbon-based negative electrode active material has a low orientation degree (I 004 / I 110 ), so the characteristics of lithium ion embedding and de-embedding in the carbon-based negative electrode active material can be improved. Therefore, even if the current density applied to the carbon-based negative electrode active material increases due to the increase in the content of the silicon-based negative electrode active material in the negative electrode active material composition, the negative electrode can ensure excellent durability, thereby improving the resistance characteristics and life characteristics of the secondary battery.
[0031] In one embodiment, the carbon-based negative active material may have an orientation degree (I) of about 2.85 or less as measured by X-ray diffraction. 004 / I 110 If the carbon-based negative electrode active material has an orientation degree (I) exceeding about 2.85 as measured by X-ray diffraction method, 004 / I 110 ), the embedding and de-embedding characteristics of lithium ions in the carbon-based negative electrode active material are reduced, resulting in reduced durability of the negative electrode, thereby the resistance characteristics and life characteristics of the secondary battery may be reduced.
[0032] In one embodiment, the negative electrode may have a surface area of about 1.4-1.7 g / cm 3 density.
[0033] In one embodiment, the negative electrode active material composition may be present in an amount of about 90-98 wt % based on the total weight of the negative electrode mixture layer.
[0034] As described above, the negative electrode active material composition may include the carbon-based negative electrode active material and the silicon-based negative electrode active material, and the carbon-based negative electrode active material may have a low value of orientation. Therefore, even if the content of the silicon-based negative electrode active material in the negative electrode active material composition increases, the negative electrode can ensure durability, thereby improving the resistance characteristics and life characteristics of the secondary battery.
[0035] Negative electrode conductive material
[0036] The negative electrode conductive material is used to impart conductivity to the negative electrode, and any conductive material commonly used in secondary batteries may be used without limitation. The negative electrode conductive material may include one or more selected from, for example, graphite, carbon black, carbon nanotubes, metal powder, and conductive oxides.
[0037] In one embodiment, the negative electrode conductive material may be included in an amount of about 0.1-3 wt % based on the total weight of the negative electrode mixture layer.
[0038] Anode Binder
[0039] The negative electrode binder may not be particularly limited as long as it is a component that facilitates the binding of the negative electrode active material composition, the negative electrode conductive material, etc., and the negative electrode current collector. The negative electrode binder may include at least one selected from a rubber-based binder and a water-soluble polymer-based binder.
[0040] The rubber-based adhesive may be a water-dispersible adhesive that is insoluble in water-based solvents such as water but can be smoothly dispersed in water-based solvents, for example, may include at least one selected from styrene butadiene rubber (SBR), hydrogenated nitrile butadiene rubber (HNBR), acrylonitrile butadiene rubber (acrylonitrile butadiene rubber), butyl rubber and fluoro rubber. Specifically, in terms of easy dispersion and excellent phase stability, the rubber-based adhesive may include at least one selected from styrene butadiene rubber and hydrogenated nitrile butadiene rubber.
[0041] In addition, the water-soluble polymer-based adhesive may be soluble in a water-based solvent such as water, and may include at least one selected from polyvinyl alcohol (PVA), polyacrylic acid (PAA), polyethylene glycol (PEG), polyacrylonitrile (PAN), polyacryl amide (PAM) and carboxylmethyl cellulose (CMC).
[0042] In one embodiment, the negative electrode binder may be included in an amount of about 2-5 wt % based on the total weight of the negative electrode mixture layer.
[0043] Negative electrode mixture layer
[0044] In an exemplary embodiment, the negative electrode mixture layer may be provided as two or more layers on the negative electrode current collector. In one embodiment, when the negative electrode mixture layer is provided as two layers, a first negative electrode mixture layer may be provided on at least one side of the negative electrode current collector, and a second negative electrode mixture layer may be provided on the first negative electrode mixture layer. The first negative electrode mixture layer and the second negative electrode mixture layer may each include the negative electrode active material composition, the negative electrode conductive material, and the negative electrode binder.
[0045] Negative current collector
[0046] The negative electrode current collector can be used without particular limitation as long as it is a current collector that is commonly used in the manufacture of the negative electrode of the secondary battery, does not cause chemical changes in the secondary battery and has conductivity. The current collector can use, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, a material that treats the surface of copper or stainless steel with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. In addition, fine concavoconvexity can be formed on the surface to enhance the binding force of the negative electrode active material, and can be used in various forms such as film, sheet, foil, net, porous body, foam, non-woven fabric, etc.
[0047] In addition, the method for manufacturing the negative electrode for the lithium secondary battery is not particularly limited. Exemplarily, the negative electrode can be manufactured by: coating the negative electrode slurry containing the negative electrode active material composition, the negative electrode conductive material, the negative electrode binder, a solvent, etc. on the negative electrode current collector by a method such as rod coating, casting or spraying, and drying at about 70-100° C. to form the negative electrode mixture layer.
[0048] The solvent can be, for example, dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. Considering the coating thickness of the composition for forming the negative electrode mixture layer and the manufacturing yield, the amount of the solvent used only needs to be sufficient to dissolve or disperse the active material, conductive material, and binder and to make the composition have a viscosity that can exhibit excellent thickness uniformity during subsequent coating for forming the negative electrode mixture layer.
[0049] Lithium secondary battery
[0050] The lithium secondary battery may include the negative electrode for the lithium secondary battery. Specifically, the lithium secondary battery may include the negative electrode and the positive electrode for the lithium secondary battery according to any one of the above specific embodiments, and may selectively further include or not include a separator interposed between the positive electrode and the negative electrode.
[0051] The positive electrode may contain a lithium-transition metal composite oxide as an active material. Specifically, the lithium-transition metal composite oxide may be an NCM-based positive electrode active material represented by the chemical formula Li x Ni a Co b Mn c O y (0 < x ≤ 1.1, 2 ≤ y ≤ 2.02, 0 < a < 1, 0 < b < 1, 0 < c < 1, 0 < a + b + c ≤ 1) or a lithium iron phosphate (LFP)-based positive electrode active material represented by the chemical formula LiFePO4.
[0052] The separator may include a porous polymer membrane prepared from a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, an ethylene / methacrylate copolymer, etc. In addition, the separator may further include a non-woven fabric formed from glass fibers with a high melting point, polyethylene terephthalate fibers, etc.
[0053] Examples
[0054] Hereinafter, the present invention will be described in more detail by way of examples. The following examples show an example of the present invention, and the present invention is not limited thereto.
[0055] Examples 1 to 5 and Comparative Examples 1 to 6
[0056] A negative electrode active material composition containing artificial graphite as a carbon-based negative electrode active material and SiC as a silicon-based negative electrode active material, carbon nanotubes (CNT) as a negative electrode conductive material, and styrene-butadiene rubber (SBR) as a negative electrode binder are mixed with water as a solvent to prepare a negative electrode slurry. At this time, based on the solid weight of the negative electrode slurry, the negative electrode slurry contains 98% by weight of the negative electrode active material composition, 0.1% by weight of the negative electrode conductive material, and 1.9% by weight of the negative electrode binder.
[0057] In addition, based on the total weight of the negative electrode active material composition, the negative electrode active material compositions of Examples 1 to 5 and Comparative Examples 1 to 6 contain SiC or SiO with the contents shown in Table 1 below x (0 < x < 2). At this time, SiC has a porous structure and contains carbon-based particles containing pores and a silicon-based coating formed in the pores or on the surface of the carbon-based particles.
[0058] After that, the prepared negative electrode slurry is coated on a copper foil as a negative electrode current collector and dried at 80 °C to manufacture a negative electrode.
[0059] After that, a sample is taken from the negative electrode using a scrapper, and then the orientation degree (I 004 / I 110 ) of artificial graphite is measured using an XRD device (Empyrean from PANalytical). At this time, the measurement conditions are as follows: 2θ = 10° to 80°, scanning speed (° / S) = 3, step size is 0.025° / step.
[0060] The measurement results of the orientation degrees of artificial graphite respectively contained in the negative electrode active material compositions of Examples 1 to 5 and Comparative Examples 1 to 6 are shown in Table 1 below.
[0061] [Table 1]
[0062] <![CDATA[Orientation degree (I 004 / I 110 )]]> SiC content (weight %) <![CDATA[SiO x Content (weight %)]]> Example 1 2.09 11 - Example 2 2.36 11 - Example 3 2.85 2 - Example 4 2.07 - 11 Example 5 2.81 - 6 Comparative Example 1 3.12 11 - Comparative Example 2 4.37 11 - Comparative Example 3 3.12 13 - Comparative Example 4 3.40 1 - Comparative Example 5 3.82 - 11 Comparative Example 6 3.52 - 6
[0063] Evaluation of battery performance
[0064] A slurry containing an NCM-based active material as a lithium-transition metal composite oxide is coated on an aluminum foil and dried to manufacture a positive electrode.
[0065] A polyolefin separator is inserted between the manufactured positive electrode and each negative electrode comprising the negative electrode active material composition of Examples 1 to 5 and Comparative Examples 1 to 6 to manufacture an electrode assembly, and the electrode assembly is placed in a soft package for a secondary battery, and an electrolyte is injected and then sealed to manufacture soft-pack lithium secondary batteries of Examples 1-1 to 5-1 and Comparative Examples 1-1 to 6-1, respectively, wherein the electrolyte is an electrolyte in which 1M LiPF6 is dissolved in a solvent mixed with ethylene carbonate (EC) and diethyl carbonate (DEC).
[0066] The internal resistance, room temperature capacity retention rate, and rapid charge capacity retention rate of each of the soft-pack lithium secondary batteries produced above were evaluated, and the results are shown in Table 2. The evaluation method of each battery performance is as follows.
[0067] 1) Internal resistance
[0068] For the lithium secondary batteries of Examples 1-1 to 5-1 and Comparative Examples 1-1 to 6-1, the direct current internal resistance (DC-IR) was measured by discharging for 10 seconds at a charge and discharge rate (C-rate) of 1C at a state of charge (SoC) of 50%.
[0069] 2) Capacity retention rate at room temperature (25°C)
[0070] For the lithium secondary batteries of Examples 1-1 to 5-1 and Comparative Examples 1-1 to 6-1, the discharge capacity of the lithium secondary battery was measured by repeatedly discharging at 0.3C to 2.5V at a temperature of 25°C, then charging at a constant current (CC) to 4.2V, and then charging at a constant voltage (CV) of 0.05C. Based on the measured discharge capacity of the lithium secondary battery, 0.33C CC / CV charging and 0.5C discharge were repeated 400 times in the range of SoC 4% to 98%, thereby measuring the capacity retention rate during the normal temperature life characteristic evaluation.
[0071] 3) Fast charging capacity retention rate
[0072] For the lithium secondary batteries of Examples 1-1 to 5-1 and Comparative Examples 1-1 to 6-1, at a temperature of 25°C, in a charging mode of changing the charge and discharge rate, after reaching a depth of discharge (DoD) of 72% within 35 minutes, they were discharged at a charge and discharge rate of 0.33C, and this charging and discharging was repeated 300 times, and then the discharge capacity retention rate relative to the initial discharge capacity was measured as a percentage (%), thereby evaluating the fast charge capacity retention rate, respectively.
[0073] [Table 2]
[0074]
[0075]
[0076] As can be seen from Table 2, it is confirmed that the secondary batteries of Examples 1-1 to 5-1 have higher room temperature capacity retention rates and fast charging capacity retention rates than the secondary batteries of Comparative Examples 1-1 to 6-1. In addition, it is confirmed that the secondary batteries of Examples 1-1 and 2-1 have lower DC-IR than the secondary batteries of Comparative Examples 1-1 to 6-1, the secondary batteries of Examples 3-1 and 4-1 have lower DC-IR than the secondary batteries of Comparative Examples 2-1 to 6-1, and the secondary battery of Example 5-1 has lower DC-IR than the secondary batteries of Comparative Examples 3-1 to 6-1. It can be seen that the secondary battery according to the present invention contains a negative electrode active material composition containing a carbon-based negative electrode active material having an orientation degree of less than 2.85, thereby having improved resistance characteristics and life characteristics.
[0077] In addition, it was confirmed that the secondary batteries of Examples 1-1 to 5-1 respectively contained the negative electrode active material compositions of Examples 1 to 5 containing 2 wt % or more of the silicon-based negative electrode active material based on the total weight of the negative electrode active material composition. It can be seen that the secondary battery according to the present invention contains a negative electrode active material composition containing a carbon-based negative electrode active material having an orientation degree of 2.85 or less and 2 wt % or more of the silicon-based negative electrode active material based on the total weight of the negative electrode active material composition, thereby having improved resistance characteristics and life characteristics.
[0078] The embodiments of the present invention are described in detail above, but this is only exemplary, and those skilled in the art should understand that various modifications and other equivalent embodiments can be implemented. Therefore, the true technical protection scope of the present invention should be determined by the technical ideas of the claims.
[0079] The specific example described in the embodiment is only one embodiment and does not limit the scope of the embodiment in any way. In addition, if there is no specific description of "essential", "important", etc., it may not be a component that is essential to the application of the present invention.
[0080] In the specification of the embodiment (especially in the claims), the use of the term "said" and similar indicative terms can correspond to both the singular and the plural. In addition, in the embodiment, when the range is recorded, it includes the invention of each value belonging to the above range (unless otherwise recorded to the contrary), and is the same as the various values that constitute the above range recorded in the detailed description. Finally, when the order is clearly recorded for the steps constituting the method according to the embodiment or there is no opposite record, the steps can be performed in an appropriate order. The embodiment is not necessarily limited to the order of recording the steps. In the embodiment, the use of all examples or exemplary terms (for example, etc.) is only used to describe the embodiment in detail, unless limited by the claims, the scope of the embodiment is not limited by the examples or exemplary terms. In addition, those skilled in the art can know that in the scope of the claims or their equivalents, various modifications, combinations and changes can be made according to design conditions and factors.
Claims
1. A negative electrode active material composition for a lithium secondary battery, comprising a carbon-based negative electrode active material and a silicon-based negative electrode active material, in, The carbon-based negative electrode active material has an orientation degree I of 2.85 or less measured by X-ray diffraction (XRD). 004 / I 110 , where I 004 is the peak intensity of the (004) plane when XRD measurement is performed on the carbon-based negative electrode active material, I 110 It is the peak intensity of the (110) plane when performing XRD measurement on the carbon-based negative electrode active material.
2. The negative electrode active material composition for lithium secondary battery according to claim 1, wherein The silicon-based negative electrode active material comprises SiC or SiO x , where 0 <x<2。 3. The negative electrode active material composition for lithium secondary battery according to claim 2, wherein: Based on the total weight of the negative electrode active material composition, the content of the silicon-based negative electrode active material is greater than 2 weight %.
4. The negative electrode active material composition for lithium secondary battery according to claim 1, wherein The silicon-based negative electrode active material includes SiC having a porous structure.
5. The negative electrode active material composition for lithium secondary battery according to claim 4, wherein The silicon-based negative electrode active material comprises: carbon-based particles comprising pores; and A silicon-based coating is formed on the pores or surfaces of the carbon-based particles.
6. A negative electrode for a lithium secondary battery, comprising: Anode current collector; and a negative electrode mixture layer formed on at least one side of the negative electrode current collector, The negative electrode mixture layer comprises the negative electrode active material composition for lithium secondary battery according to any one of claims 1 to 5, a negative electrode conductive material and a negative electrode binder.
7. The negative electrode for a lithium secondary battery according to claim 6, wherein: The negative electrode mixture layer is provided in two or more layers on the negative electrode collector. 8 . A lithium secondary battery comprising the negative electrode for a lithium secondary battery according to claim 6 .
Citation Information
Patent Citations
Silicon-carbon negative electrode slurry, preparation method, negative electrode plate and lithium ion battery
CN110444746A
Negative active material for lithium secondary battery and lithium secondary battery including same
CN115966662A