High-entropy sodium ferric fluorophosphate positive electrode material as well as preparation method and application thereof

By using high-entropy sodium ferrophosphate positive electrode material in Na2FePO4F electrode material, the problem of poor conductivity of the material is solved through the combination of multiple elements and the conductive carbon layer coating technology, the rate performance and cycle stability are significantly improved, and the rate performance and cycle stability are achieved. Excellent performance in sodium ion batteries.

CN119008889APending Publication Date: 2024-11-22BEIJING NADONG NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411093456.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The rate performance and cycle stability of Na2FePO4F electrode materials in sodium ion batteries are poor, and existing modification methods such as carbon coating and transition metal doping effects are limited.

Method used

High-entropy sodium ferric phosphate positive electrode material is used to perform high-entropy replacement of body phase in the Na2FePO4F crystal structure through the combination of various elements, and a conductive carbon layer is wrapped on the surface of the active nanoparticles to enhance the interface and body phase conductivity of the material.

Benefits of technology

It significantly improves the rate performance and cycle stability of the material, extends the service life of the battery, and shows good conductivity and high gram capacity at room temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008889A_ABST
    Figure CN119008889A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of battery materials, and particularly discloses a high-entropy sodium ferric fluorophosphate positive electrode material and a preparation method and application thereof. The high-entropy sodium ferric fluorophosphate positive electrode material comprises active nanoparticles and a conductive carbon layer wrapping the surfaces of the active nanoparticles, the chemical general formula of the active nanoparticles is Na2FexMyPO4F, x ranges from 0.95 to 0.96, y ranges from 0.01 to 0.02, and M is one or more of Mg, Cu, Ni, Co, Mn, Al and Ti. The intrinsic conductivity of the material is improved through a bulk phase high-entropy substitution strategy, the interface conductivity of the material is further improved by combining surface carbon coating, the problem that the overall conductivity of the sodium ferric fluorophosphate positive electrode material is poor is solved, and the gram volume, the rate capability and the cycling stability of the material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of battery materials, and more specifically, to a high-entropy sodium iron fluorophosphate positive electrode material and a preparation method and application thereof. Background Art

[0002] Sodium cathode material refers to the material used as cathode in sodium ion batteries. As a new energy storage technology, sodium ion batteries are rich in resources, low in cost, and environmentally friendly. They are considered to be a substitute for sodium ion batteries and are suitable for electric vehicle power supplies and large-scale energy storage power stations. LiFePO4, as a cathode material for sodium ion batteries, has the advantages of high theoretical specific capacity, stable cycle performance, low iron cost, and abundant resources, making iron-based phosphates the most popular cathode material in the field of sodium ion batteries.

[0003] Among them, the theoretical specific capacity of the fluorine-phosphorus compound Na2FePO4F is 124 mAh﹒ g -1 , has a simple two-dimensional sodium ion pathway and a good working voltage (3 V), but has very low intrinsic electronic conductivity, resulting in poor cycling stability and rate performance, which in turn inhibits its electrochemical performance in sodium ion batteries.

[0004] Common modification methods include carbon coating and transition metal doping. Patent CN114242968A uses carbon coating to improve the conductivity of the material, thereby improving the electrochemical performance. Patent CN117878277A uses Cr to partially replace the Fe in Na2FePO4F. The introduction of Cr shortens the PO bond length and enhances the stability of the material structure, thereby effectively improving the electrochemical performance of sodium ion batteries. However, ordinary carbon coating can only improve the conductivity of the surface of the material particles, but cannot improve the conductivity of the bulk phase of the material. Although single transition metal substitution can improve the material performance to a certain extent, it has limited effects on the rate performance and cycle stability of the material. In patent CN117457874A, Na2Fe was prepared. 0.2 Mn 0.2 Ni 0.2 Mg 0.2 Cu 0.2 PO4F electrode material, but the improvement on the material's cycle stability is limited. Summary of the invention

[0005] In order to improve the problems of poor rate performance and cycle stability of Na2FePO4F electrode materials, the present application provides a high entropy sodium iron fluorophosphate positive electrode material and a preparation method and application thereof.

[0006] In the first aspect, the present application provides a high entropy sodium iron fluorophosphate cathode material, which adopts the following technical scheme: a high entropy sodium iron fluorophosphate cathode material, comprising active nanoparticles and a conductive carbon layer wrapped on the surface of the active nanoparticles, wherein the chemical formula of the active nanoparticles is Na2Fe x M y PO4F, x is 0.95-0.96, y is 0.01-0.02, and M is one or more of Mg, Cu, Ni, Co, Mn, Al, and Ti.

[0007] By adopting the above technical solution and combining multiple elements, it is possible to have a certain influence on the electronic state in the Na2FePO4F crystal structure. Through the bulk high entropy substitution strategy, that is, partially replacing the iron position with multiple atypical transition metal elements, the conductivity of the electrode material interface and bulk phase can be synergistically improved, thereby improving the material's rate performance and cycle stability.

[0008] Optionally, the chemical formula of the active nanoparticles is Na2Fe 0.96 (MgCuAlTi) 0.01 PO4F, in which the amounts of Mg, Cu, Al and Ti substances account for 0.5-2% respectively.

[0009] By adopting the above technical solution, M is further limited to Mg, Cu, Al, and Ti, and the obtained high-entropy sodium iron fluorophosphate positive electrode material has good crystal structure stability, and the cycle stability of the electrode material is significantly improved.

[0010] Optionally, the mass of the conductive carbon layer accounts for 5-30% of the total mass of the positive electrode material.

[0011] By adopting the above technical solution, the amount of conductive carbon layer is limited, and the interfacial conductivity of the material is further improved. Carbon coating can reduce the charge transfer resistance and increase the diffusion rate of sodium ions inside the particles, thereby improving the electrochemical properties of the material, including improving the discharge capacity and cycle stability, and extending the service life of the battery.

[0012] Further preferably, the mass of the conductive carbon layer accounts for 20% of the total mass of the positive electrode material.

[0013] By adopting the above technical solution, the amount of the conductive carbon layer is further limited. The carbon coating layer helps to form an effective conductive network between the positive electrode material particles and between the binder and the conductive additive, which is beneficial to improving the rate performance of the electrode material and maintaining good electrochemical properties at high current density.

[0014] Optionally, the raw material for preparing the conductive carbon layer is a carbon source, and the carbon source is one of glucose, ascorbic acid, citric acid, sucrose, polyvinyl pyrrolidone, and polyvinyl alcohol.

[0015] By adopting the above technical scheme, the carbon source can be decomposed during the heat treatment process to form a carbon coating layer, which covers the surface of the positive electrode material, thereby improving the conductivity and structural stability of the material; it can also form a conductive network, thereby improving the electronic conductivity of the positive electrode material, reducing the charge transfer resistance, and improving the rate performance of the battery, effectively preventing the structural changes of the positive electrode material during the charging and discharging process, improving the structural stability and cycle performance of the material, and extending the service life of the battery.

[0016] Further preferably, the carbon source is polyvinyl pyrrolidone.

[0017] By adopting the above technical solution, polyvinyl pyrrolidone is used as a carbon source to provide carbon atoms, and the formed carbon coating layer helps the diffusion of sodium ions in the positive electrode material and increases the migration rate of sodium ions, thereby improving the charge and discharge rate and energy density of the battery.

[0018] Optionally, the raw materials for preparing the high entropy sodium iron fluorophosphate positive electrode material include an iron source, a magnesium source, a copper source, an aluminum source and a titanium source, the iron source is ferrous oxalate, the magnesium source is magnesium acetate, the copper source is copper acetate, the aluminum source is aluminum acetate or aluminum nitrate, and the titanium source is tetrabutyl titanate or titanium isopropoxide, and the doping amounts of the magnesium source, copper source, aluminum source and titanium source are 1-2% each.

[0019] By adopting the above technical scheme, the iron source is one of the basic elements constituting the high entropy sodium iron fluorophosphate positive electrode material. Its main function is to provide iron ions, participate in the formation of the main structure of the material, and have an important influence on the electrochemical properties of the material. The introduction of the magnesium source can improve the structural stability of the material, optimize the electrochemical properties of the material, improve the cycle stability and rate performance, and at the same time, the doping of magnesium ions helps to improve the conductivity of the material and the sodium ion diffusion performance. The doping of the copper source can improve the electronic conductivity of the material and improve the conductive network of the material, thereby improving the rate performance and energy density of the battery. At the same time, the introduction of copper ions helps to optimize the structure of the material and improve the cycle stability.

[0020] Doping with aluminum sources can improve the structural stability and thermal stability of materials, reduce structural changes in materials during the charge and discharge process, and extend the service life of the battery. Doping with aluminum ions can also help improve the electrochemical properties of materials, improve cycle stability and rate performance. Doping with titanium sources can improve the structural stability and thermal stability of materials. At the same time, the introduction of titanium ions can help optimize the electrochemical properties of materials, improve cycle stability and rate performance. The use of titanium sources can also improve the sodium ion diffusion performance of materials, thereby improving the charge and discharge rate and energy density of the battery.

[0021] In a second aspect, the present application provides a method for preparing a high entropy sodium iron fluorophosphate positive electrode material, comprising the following steps: (1) ball milling ferrous oxalate, aluminum acetate, copper acetate, magnesium acetate, tetrabutyl titanate, ammonium dihydrogen phosphate and sodium fluoride for 5-15 hours at a rotation speed of 300-700 r / min to obtain a precursor; (2) Under an inert atmosphere, heat treating the precursor obtained in step (1) at 300-400° C. for 2-12 h to obtain a pretreated precursor; (3) dispersing the pretreated precursor obtained in step (2) in anhydrous ethanol, adding 5-30% by weight of polyvinyl pyrrolidone, stirring to dissolve, and drying to obtain a powder; (4) Pressing the powder obtained in step (3) into tablets, and heat treating the tablets at 550-800° C. for 4-12 h under an inert atmosphere to obtain a high entropy sodium iron fluorophosphate positive electrode material.

[0022] By adopting the above technical solution and the above preparation method, the prepared high-entropy sodium iron fluorophosphate positive electrode material has good cycle stability, and the active nanoparticles are combined with the surface carbon coating to accelerate the electronic conduction at the material interface and improve the interface conductivity.

[0023] In addition, the doping of multiple elements in the bulk structure improves the stability of the material's crystal structure, thereby significantly improving the cycle stability of its electrode material.

[0024] Further preferably, in step (1), the rotation speed is 500 r / min.

[0025] Further preferably, in step (2), heat treatment is performed at 350° C. for 4 h.

[0026] Further preferably, in step (4), heat treatment is performed at 600° C. for 8 h.

[0027] Optionally, in step (3), the stirring rate is 300-350 r / min, and the stirring time is 1-4 h; the drying temperature is 50-80° C., and the drying time is 2-3 h.

[0028] By adopting the above technical solution, the stirring and drying conditions are further limited, so that the carbon coating is uniform, and the obtained high-entropy sodium iron fluorophosphate positive electrode material has better comprehensive performance.

[0029] In a third aspect, the present application provides a sodium ion battery, wherein the positive electrode material is the above-mentioned high-entropy sodium iron fluorophosphate positive electrode material, or the high-entropy sodium iron fluorophosphate positive electrode material prepared by the above-mentioned preparation method.

[0030] By adopting the above technical scheme, the high entropy sodium iron fluorophosphate positive electrode material prepared in the present application is used as the positive electrode material of the sodium ion battery, which has good conductivity, high gram capacity, cycle stability and rate performance at room temperature, and has good application prospects.

[0031] In summary, this application has the following beneficial effects: 1. In this application, the intrinsic conductivity of the material is improved through the bulk high entropy substitution strategy, and the interfacial conductivity of the material is further improved by combining the surface carbon coating, thereby overcoming the problem of poor overall conductivity of the sodium iron fluorophosphate positive electrode material and improving the gram capacity, rate performance and cycle stability of the material.

[0032] 2. The combination of multiple elements in this application can have a certain influence on the electronic state in the Na2FePO4F crystal structure. Through the bulk high entropy substitution strategy, that is, partially replacing the iron position with multiple heterovalent transition metal elements, the conductivity of the electrode material interface and bulk phase is synergistically improved, thereby improving the material's rate performance and cycle stability.

[0033] 3. The high entropy sodium iron fluorophosphate positive electrode material in this application, as a positive electrode material for sodium ion batteries, has good conductivity, high gram capacity, cycle stability and rate performance at room temperature, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 X-ray diffraction (XRD) diagrams of the positive electrode materials prepared in Example 1 and Comparative Example 1, wherein NFPF is the sample corresponding to Comparative Example 1, and HE-NFPF is the sample corresponding to Example 1; Figure 2 The scanning electron microscope (SEM) images of the positive electrode materials prepared in Example 1 and Comparative Example 1; Figure 3 The rate performance diagram of the 2032-type button battery prepared in Example 1 and Comparative Example 1; Figure 4 This is a cycle performance diagram of the 2032-type button battery prepared in Example 1 and Comparative Example 1. DETAILED DESCRIPTION Example

[0035] Example 1 A method for preparing a high entropy sodium iron fluorophosphate positive electrode material comprises the following steps: (1) 10 g of ferrous oxalate, aluminum acetate, copper acetate, magnesium acetate, tetrabutyl titanate, 10 g of ammonium dihydrogen phosphate and 10 g of sodium fluoride were placed in a ball mill and ball milled for 10 h at a speed of 500 r / min to obtain a precursor; wherein the amount of aluminum source, magnesium source, copper source and titanium source substances accounted for 1% respectively, and 1% was based on the amount of Fe substance; (2) Under an inert atmosphere, heat treating the precursor obtained in step (1) in a tube furnace at 350° C. for 4 h to obtain a pretreated precursor; (3) Disperse the pretreated precursor obtained in step (2) in 5 mL of anhydrous ethanol, add 20% by mass of polyvinyl pyrrolidone, stir to dissolve, and dry to obtain a powder; wherein the stirring rate is 300 r / min and the stirring time is 2 h; the drying temperature is 70° C. and the drying time is 2 h; the mass ratio of 20% means that the mass of polyvinyl pyrrolidone accounts for 20% of the mass of the pretreated precursor.

[0036] (4) The powder obtained in step (3) is pressed into a tablet, and heat treated at 600° C. for 8 h in a tube furnace under an inert atmosphere to obtain a high entropy sodium iron fluorophosphate positive electrode material with a chemical formula of Na2Fe 0.96 (MgCuAlTi) 0.01 PO4F.

[0037] Example 2 A high entropy sodium iron fluorophosphate positive electrode material, which is different from Example 1 in that it comprises the following steps: (1) 12 g of ferrous oxalate, aluminum acetate, copper acetate, magnesium acetate, tetrabutyl titanate, 12 g of ammonium dihydrogen phosphate and 12 g of sodium fluoride were placed in a ball mill and ball milled for 5 h at a speed of 300 r / min to obtain a precursor; wherein the amount of aluminum source, magnesium source, copper source and titanium source each accounted for 2%; (2) Under an inert atmosphere, heat-treating the precursor obtained in step (1) in a tube furnace at 300° C. for 12 h to obtain a pretreated precursor; (3) Disperse the pretreated precursor obtained in step (2) in 8 mL of anhydrous ethanol, add 5% by mass of polyvinyl pyrrolidone, stir to dissolve, and dry to obtain a powder; wherein the stirring rate is 350 r / min, the stirring time is 4 h, the drying temperature is 50°C, and the drying time is 3 h.

[0038] (4) The powder obtained in step (3) is pressed into tablets, and heat treated at 550° C. for 12 h in a tube furnace under an inert atmosphere to obtain a high entropy sodium iron fluorophosphate positive electrode material.

[0039] Example 3 A high entropy sodium iron fluorophosphate positive electrode material, which is different from Example 1 in that it comprises the following steps: (1) 8 g of ferrous oxalate, aluminum acetate, copper acetate, magnesium acetate, tetrabutyl titanate, 8 g of ammonium dihydrogen phosphate and 8 g of sodium fluoride were placed in a ball mill and ball milled for 15 h at a speed of 700 r / min to obtain a precursor; wherein the amount of aluminum source, magnesium source, copper source and titanium source each accounted for 0.5%; (2) Under an inert atmosphere, heat-treating the precursor obtained in step (1) in a tube furnace at 400° C. for 2 h to obtain a pretreated precursor; (3) Disperse the pretreated precursor obtained in step (2) in 6 mL of anhydrous ethanol, add 30% by mass of polyvinyl pyrrolidone, stir to dissolve, and dry to obtain a powder; wherein the stirring rate is 300 r / min, the stirring time is 1 h, the drying temperature is 50°C, and the drying time is 3 h.

[0040] (4) The powder obtained in step (3) is pressed into tablets, and heat treated at 800° C. for 4 h in a tube furnace under an inert atmosphere to obtain a high entropy sodium iron fluorophosphate positive electrode material.

[0041] Example 4 A high entropy sodium iron fluorophosphate positive electrode material, which is different from Example 1 in that the amount of aluminum source, magnesium source, copper source and titanium source substances each accounts for 0.1%.

[0042] Example 5 A high entropy sodium iron fluorophosphate positive electrode material, which is different from Example 1 in that the amount of aluminum source, magnesium source, copper source and titanium source substances each accounts for 2.5%.

[0043] Example 6 A high entropy sodium iron fluorophosphate positive electrode material, which differs from Example 1 in that, in step (3), 2% by mass of polyvinyl pyrrolidone is added.

[0044] Example 7 A high entropy sodium iron fluorophosphate positive electrode material, which differs from Example 1 in that, in step (3), 35% by mass of polyvinyl pyrrolidone is added.

[0045] Example 8 A high entropy sodium iron fluorophosphate positive electrode material, which is different from Example 1 in that only an aluminum source is added, and the amount of the substance accounts for 1% each.

[0046] Example 9 A high entropy sodium iron fluorophosphate positive electrode material, which is different from Example 1 in that only a magnesium source is added, and the amount of the substance accounts for 1% each.

[0047] Example 10 A high entropy sodium iron fluorophosphate positive electrode material, which is different from Example 1 in that only a copper source is added, and the amount of the substance accounts for 1% each.

[0048] Embodiment 11 A high entropy sodium iron fluorophosphate positive electrode material, which differs from Example 1 in that only a titanium source is added, and the amount of the substance accounts for 1% each.

[0049] Comparative Example Comparative Example 1 A high entropy sodium iron fluorophosphate positive electrode material, which is different from Example 1 in that no aluminum source, magnesium source, copper source, or titanium source is added.

[0050] Performance testing The high entropy sodium iron fluorophosphate positive electrode materials prepared in Examples 1-11 and Comparative Example 1 were assembled into batteries, and the following performance tests were performed; the specific steps of battery assembly are as follows: the positive electrode materials prepared in the Examples and Comparative Examples, conductive carbon black (Super P) and polyvinylidene fluoride (PVDF) were weighed in a mass ratio of 7:2:1, and they were fully ground and mixed and then dissolved in 400uL N-methylpyrrolidone (NMP) solution. After magnetic stirring for 4 hours, a uniform slurry was formed. The slurry was evenly applied on aluminum foil using a scraper method. After drying at 80°C for 12 hours under a vacuum environment, it was cut into pole pieces as the positive electrode; the sodium sheet was used as the negative electrode, the electrolyte was 1M sodium perchlorate (NaClO4) dissolved in a volume ratio of 1:1 ethylene carbonate / propylene carbonate (EC / PC) system, and 5wt% of fluoroethylene carbonate (FEC) was added at the same time, the diaphragm was glass fiber, and it was assembled into a 2032 type button battery in a glove box filled with argon.

[0051] Test conditions: The sodium ion battery was tested for (constant current) charge and discharge interval cycle performance and rate performance. The cycle performance test was carried out on the Land battery tester with a test voltage range of (2-4.3V), and the battery's first discharge capacity and capacity retention rate after 200 cycles at 1C current were recorded. The test results are shown in Table 1.

[0052] Table 1 Test data of embodiments and comparative examples from Figure 1 The XRD results show that the cathode material prepared in Comparative Example 1 is Na2FePO4F, without any extra peaks, indicating that the sample is pure. The XRD characteristic peaks of the sample prepared in Example 1 are basically consistent with those in Comparative Example 1, indicating that the doping of multiple transition metals does not cause changes in the bulk structure, and the peak position slightly shifts to a lower angle, indicating that the transition metals are successfully doped into the structure.

[0053] from Figure 2 From the SEM, it can be seen that the sample particles of Example 1 and Comparative Example 1 are obvious, uniform in size, and are all irregular nano-scale particles.

[0054] from Figure 3 It can be seen that under the condition of 0.1C rate, Example 1 has 118 mAh﹒ g -1 The initial capacity of the comparative example is only 107 mAh﹒ g -1 After rapid charge and discharge at different current densities, it can be found that the capacity of the comparative example is always lower than that of Example 1. This proves that Example 1 has excellent rate performance.

[0055] from Figure 4 It can be seen that when the cycle stability is tested at a current density of 1C, the initial discharge specific capacities of Example 1 and Comparative Example 1 are (107, 104) mAh﹒ g respectively at 1C. -1 After 200 cycles, the discharge capacity is (83, 65) mAh﹒ g -1 , the capacity retention rates were 77.6% and 62.5%.

[0056] Example 2-3 changes the amount of each raw material in the preparation process of high entropy sodium iron fluorophosphate positive electrode material. As shown in Table 1, at 1C, the initial discharge specific capacities of Example 2 and Example 3 are (100.8, 98) mAh﹒ g respectively. -1 After 200 cycles, the discharge capacity is (71.7, 69.8) mAh﹒ g -1 The capacity retention rates are 71.1% and 71.2%, and the gram capacity, rate performance and cycle stability are still good.

[0057] Example 4-5 changes the proportion of aluminum source, magnesium source, copper source and titanium source in the preparation process of high entropy sodium iron fluorophosphate positive electrode material. As shown in Table 1, at 1C, the initial discharge specific capacities of Example 4 and Example 5 are (101, 103.4) mAh﹒ g respectively. -1 After 200 cycles, the discharge capacity is (63, 62.5) mAh﹒ g -1 The capacity retention rates were 62.4% and 60.4%, and the gram capacity, rate performance and cycle stability decreased significantly, indicating that when the proportions of aluminum source, magnesium source, copper source and titanium source are limited within a certain range, the obtained electrode material has better comprehensive performance.

[0058] In Examples 6 and 7, the amount of polyvinyl pyrrolidone added during the preparation of the high entropy sodium iron fluorophosphate positive electrode material was changed. As shown in Table 1, at 1C, the initial discharge specific capacities of Examples 6 and 7 were (103.4, 105) mAh﹒ g, respectively. -1 After 200 cycles, the discharge capacity is (65.6, 74.5) mAh﹒ g -1 , the capacity retention rates were 63.4% and 71.0%, and the gram capacity, rate performance and cycle stability decreased significantly, indicating that limiting the amount of polyvinyl pyrrolidone within a certain range can ensure the electrochemical properties of the material, including improving the discharge capacity and cycle stability, and extending the service life of the battery.

[0059] In Examples 8-11, only aluminum source, magnesium source, copper source and titanium source were added respectively. As shown in Table 1, at 1C, the initial discharge specific capacities were (101.3, 102, 103.9, 102.6) mAh﹒ g -1After 200 cycles, the discharge specific capacity is (72.4, 69.8, 73.5, 75.8) mAh﹒ g -1 The capacity retention rates were 71.5%, 68.4%, 70.7% and 73.9%, and the gram capacity, rate performance and cycle stability decreased significantly, indicating that the combination of the iron source, magnesium source, copper source, aluminum source and titanium source in the present application has good crystal structure stability, and the cycle stability of the electrode material is significantly improved.

[0060] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. After reading this specification, those skilled in the art can make non-creative modifications to the present embodiment as needed, but as long as it is within the scope of the claims of the present application, it is protected by the patent law.

Claims

1. A high entropy sodium iron fluorophosphate cathode material, It is characterized in that The invention comprises active nanoparticles and a conductive carbon layer wrapped on the surface of the active nanoparticles, wherein the chemical formula of the active nanoparticles is Na 2 Fe x M y PO 4 F, x is 0.95-0.96, y is 0.01-0.02, and M is one or more of Mg, Cu, Ni, Co, Mn, Al, and Ti.

2. A high entropy sodium iron fluorophosphate positive electrode material according to claim 1, It is characterized in that The chemical formula of the active nanoparticles is Na 2 Fe 0.96 (MgCuAlTi) 0.01 PO 4 F, in which the amounts of Mg, Cu, Al and Ti substances account for 0.5-2% respectively.

3. A high entropy sodium iron fluorophosphate positive electrode material according to claim 1, It is characterized in that The mass of the conductive carbon layer accounts for 5-30% of the total mass of the positive electrode material.

4. A high entropy sodium iron fluorophosphate positive electrode material according to claim 1, It is characterized in that The mass of the conductive carbon layer accounts for 20% of the total mass of the positive electrode material.

5. A high entropy sodium iron fluorophosphate positive electrode material according to claim 1, It is characterized in that The raw material for preparing the conductive carbon layer is a carbon source, and the carbon source is one of glucose, ascorbic acid, citric acid, sucrose, polyvinyl pyrrolidone, and polyvinyl alcohol.

6. A high entropy sodium iron fluorophosphate positive electrode material according to claim 1, It is characterized in that The carbon source is polyvinyl pyrrolidone.

7. A high entropy sodium iron fluorophosphate positive electrode material according to claim 2, It is characterized in that The raw materials for preparing the high entropy sodium iron fluorophosphate positive electrode material include an iron source, a magnesium source, a copper source, an aluminum source and a titanium source, wherein the iron source is ferrous oxalate, the magnesium source is magnesium acetate, the copper source is copper acetate, the aluminum source is aluminum acetate or aluminum nitrate, and the titanium source is tetrabutyl titanate or titanium isopropoxide, and the doping amounts of the magnesium source, copper source, aluminum source and titanium source each account for 1-2%.

8. A method for preparing a high entropy sodium iron fluorophosphate positive electrode material according to any one of claims 1 to 7, It is characterized in that The steps include: (1) ball milling ferrous oxalate, aluminum acetate, copper acetate, magnesium acetate, tetrabutyl titanate, ammonium dihydrogen phosphate and sodium fluoride for 5-15 hours at a rotation speed of 300-700 r / min to obtain a precursor; (2) Under an inert atmosphere, heat-treating the precursor obtained in step (1) at 300-400° C. for 2-12 h to obtain a pretreated precursor; (3) dispersing the pretreated precursor obtained in step (2) in anhydrous ethanol, adding 5-30% by weight of polyvinyl pyrrolidone, stirring to dissolve, and drying to obtain a powder; (4) The powder obtained in step (3) is pressed into tablets, and heat treated at 550-800° C. for 4-12 h under an inert atmosphere to obtain a high entropy sodium iron fluorophosphate positive electrode material.

9. A method for preparing a high entropy sodium iron fluorophosphate positive electrode material according to claim 8, It is characterized in that In step (3), the stirring rate is 300-350 r / min, and the stirring time is 1-4 h; the drying temperature is 50-80° C., and the drying time is 2-3 h.

10. A sodium ion battery, It is characterized in that The positive electrode material is the high entropy sodium iron fluorophosphate positive electrode material described in any one of claims 1 to 7, or the high entropy sodium iron fluorophosphate positive electrode material prepared by the preparation method described in claims 8 to 9.