Sodium battery positive electrode material and preparation method and application thereof
By doping Ni, Cu, Zn, Mg, Fe, Co, and Cr elements in the sodium electropositive electrode material, the conductivity and multi-electron redox reaction of sodium batteries are improved, and the capacity and magnification of sodium phosphate sodium electropositive electrode material are solved. The problem of poor capability has significantly improved the charging and discharging performance and rate performance of sodium batteries.
Patent Information
- Application Number
- CN202410972466.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-22
AI Technical Summary
The existing sodium phosphate electropositive electrode materials have insufficient reversible capacity and poor magnification capacity under high current density, resulting in poor charging and discharging performance of sodium batteries.
Carbon-doped Na3+yMn1-xAxTi1-yBy(PO4)3 is used as the sodium-electrode material, and the electron/ion transport of the material is adjusted by doping Ni, Cu, Zn, Mg and Ca elements as well as Fe, Co, and Cr elements. Transport properties, increase conductivity and multi-electron redox reactions, and inhibit Jahn-Teller distortion.
The charge and discharge specific capacity of sodium batteries, the first-time Coulomb efficiency and rate performance are improved, and the discharge voltage platform and capacity are enhanced.
Smart Images

Figure CN119008934A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of batteries, and particularly to a sodium battery cathode material, a preparation method thereof and an application thereof. Background Art
[0002] The low cost and abundant sodium resources of sodium-ion batteries make them an ideal choice for stationary energy storage. Among sodium battery cathode materials, polyanion compounds have attracted much attention due to their inherent structural stability, especially the sodium + superionic conductor (NASICON) structure cathode, whose ultrafast three-dimensional (3D) sodium + transport channels and high stability show broad application prospects.
[0003] However, existing sodium phosphate battery cathode materials have disadvantages such as low electronic conductivity, Jahn-Teller distortion or high sodium + diffusion barriers, resulting in insufficient reversible capacity and poor rate performance of the batteries prepared using the above-mentioned sodium phosphate battery cathode materials at high current densities. Summary of the Invention
[0004] In view of this, the present invention provides a sodium battery cathode material, a preparation method thereof and an application thereof to solve the problems of insufficient specific capacity and poor rate performance of the batteries prepared using existing sodium phosphate battery cathode materials.
[0005] In a first aspect, the present invention provides a sodium battery cathode material.
[0006] In an alternative embodiment, the sodium battery cathode material comprises carbon-doped Na 3+y Mn 1-x A x Ti 1-y B y (PO4)3;
[0007] wherein, 0.01 < x ≤ 0.3, 0.01 < y ≤ 0.5, A is selected from one or more combinations of Ni, Cu, Zn, Mg and Ca, B is selected from one or more combinations of Ni, Cu, Fe, Co and Cr, and A is different from B.
[0008] In an alternative embodiment, the sodium battery cathode material comprises carbon-doped Na 3.3 Mn 0.8 Ni 0.2 Ti 0.7 Cr 0.3 (PO4)3, carbon-doped Na 3.3 Mn 0.8 Cu 0.2 Ti 0.7 Fe 0.3(PO4)3 and carbon-doped Na 3.3 Mn 0.8 Ni 0.2 Ti 0.7 Co 0.3 (PO4)3 or a combination of two or more thereof.
[0009] In a second aspect, the present invention provides a method for preparing the sodium battery positive electrode material.
[0010] In an optional embodiment, the method for preparing the sodium positive electrode material comprises: mixing a sodium source, a manganese source, a titanium source, a phosphorus source, a dopant containing A, a dopant containing B and a carbon source in water to obtain a precursor slurry;
[0011] The precursor slurry is dried and then calcined in an inactive gas to obtain the sodium positive electrode material.
[0012] In an optional embodiment, the method for preparing the sodium positive electrode material satisfies at least one of the following (1)-(7):
[0013] (1) The sodium source includes one or a combination of two or more of sodium acetate, sodium oxalate, sodium carbonate, sodium bicarbonate and sodium hydroxide;
[0014] (2) the manganese source includes one or a combination of two or more of manganese acetate, manganese oxalate and manganese nitrate;
[0015] (3) The titanium source includes one or a combination of two or more of titanium dioxide, titanium oxalate, tetrabutyl titanate and dihydroxybis(ammonium lactate)titanium;
[0016] (4) the phosphorus source includes one or a combination of two or more of diammonium phosphate, diammonium hydrogen phosphate and phosphoric acid;
[0017] (5) The carbon source includes one or a combination of two or more of carbon nanofibers, carbon nanotubes, graphene, graphene oxide, acetylene black, citric acid, glucose, and sucrose;
[0018] (6) The A-containing dopant includes one or a combination of two or more of nickel acetate, copper acetate, zinc acetate, magnesium acetate, calcium acetate, nickel oxalate, copper oxalate, zinc oxalate, magnesium oxalate and calcium oxalate;
[0019] (7) The B-containing dopant includes one or a combination of two or more of ferric acetate, cobalt acetate, chromium acetate, ferric oxalate, cobalt oxalate and chromium oxalate.
[0020] In an optional embodiment, the content of the carbon source is 5-15wt% of the total content of the sodium source, the manganese source, the titanium source, the phosphorus source, the A-containing dopant and the B-containing dopant, in terms of weight percentage;
[0021] And / or, in terms of weight percentage, the amount of water added is 10%-50% of the total weight of the sodium source, the manganese source, the titanium source, the phosphorus source, the A-containing dopant and the B-containing dopant.
[0022] In an optional embodiment, the molar ratio of the sodium element in the sodium source, the manganese element in the manganese source, the titanium element in the titanium source, the phosphorus element in the phosphorus source, the A element in the A-containing dopant, and the B element in the B-containing dopant is (3+y):(1-x):x:(1-y):y; wherein 0.01 <x≤0.3,0.01<y≤0.5;
[0023] Optionally, the molar ratio of the sodium element in the sodium source, the manganese element in the manganese source, the titanium element in the titanium source, the phosphorus element in the phosphorus source, the A element in the A-containing dopant and the B element in the B-containing dopant is 3.3:0.8:0.2:0.7:0.3:3.
[0024] In an optional embodiment, the drying is spray drying, and during the spray drying process, the feed rate is 1-5 L / h;
[0025] and / or, the air inlet temperature is 180-220°C;
[0026] And / or, the air outlet temperature is 90-110°C.
[0027] In an optional embodiment, the calcination temperature is 200-800°C;
[0028] The calcination is divided into two stages, including:
[0029] In the first stage, the temperature is raised to 200°C-350°C, and the holding time is 1h-5h; optionally, the heating rate in the first stage is 1°C / min-5°C / min;
[0030] The second stage is to heat up to 600°C-800°C, and the heat preservation time is 6h-15h; optionally, the heating rate of the second stage is 0.5°C / min-1°C / min.
[0031] In an optional embodiment, the inactive gas includes nitrogen and / or an inert gas;
[0032] Optionally, the inert gas includes one or a combination of two or more of helium, neon, argon, krypton, xenon and radon.
[0033] In a third aspect, the present invention also provides an application of the sodium-ion positive electrode material or the sodium-ion positive electrode material obtained by the preparation method in a sodium-ion battery.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] The present invention provides a sodium battery cathode material, which comprises carbon-doped Na 3+y Mn 1- x A x Ti 1-y B y (PO4)3; wherein, 0.01 < x ≤ 0.3, 0.01 < y ≤ 0.5, A is selected from one or more combinations of Ni, Cu, Zn, Mg, and Ca, B is selected from one or more combinations of Ni, Cu, Fe, Co, and Cr, and A is different from B. Doping and substituting with two or more elements increases the conductivity of the sodium battery cathode material, simultaneously increases the multi-electron redox reaction, improves the discharge voltage platform and capacity, and inhibits the Jahn-Teller distortion, thereby improving the charge-discharge specific capacity, initial Coulomb efficiency, and rate performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the specific embodiments of the present application or the technical solutions in the prior art, the following will briefly introduce the drawings required for the description of the specific embodiments or the prior art. Obviously, the drawings in the following description are some embodiments of the present application. For those of ordinary skill in the art, without creative efforts, other drawings can also be obtained based on these drawings.
[0037] Figure 1 is the scanning electron microscope image of the Na 3.3 Mn 0.8 Ni 0.2 Ti 0.7 Cr 0.3 (PO4)3 / C cathode material in Example 1. DETAILED DESCRIPTION OF THE EMBODIMENTS
[0038] The following embodiments are provided to better further understand the present invention. It is not limited to the best embodiment, and does not limit the content and protection scope of the present invention. Any product that is the same as or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior art features falls within the protection scope of the present invention.
[0039] Unless otherwise stated or there is a contradiction, the terms or phrases used herein have the following meanings:
[0040] In the present application, the selection scope involving "and / or", "or / and", and "and / or" includes any one of two or more related listed items, and also includes any and all combinations of the related listed items, and the any and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items.
[0041] In the present application, the term “preferred” is only used to describe an implementation method or example with better effects, and it should be understood that it does not constitute a limitation on the scope of protection of the present application.
[0042] In this application, "optionally" refers to optional, that is, it refers to any one of the two parallel solutions of "yes" or "no". If there are multiple "options" in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "option" is independent.
[0043] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0044] In the present application, when referring to a numerical interval (i.e., a numerical range), unless otherwise specified, the optional numerical distribution within the above numerical interval is deemed to be continuous and includes the two numerical endpoints of the numerical range (i.e., the minimum value and the maximum value), and every numerical value between the two numerical endpoints.
[0045] In the present application, the percentage content, unless otherwise specified, refers to mass percentage for solid-liquid mixing and solid-solid mixing, and refers to volume percentage for liquid-liquid mixing.
[0046] In this application, when it comes to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.
[0047] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0048] Among sodium cathode materials, polyanionic compounds have attracted much attention due to their inherent structural stability, especially Na + The superionic conductor (NASICON) structure cathode has an ultrafast three-dimensional (3D) Na + The transport channel and high stability show broad application prospects.
[0049] Na3V2(PO4)3 (NVP) has a high theoretical capacity (117 mAh / g) and is a rising star among NASICON cathodes. However, the high cost and toxicity of vanadium resources have hindered the practical application of NVP. Considerable efforts have been made to improve the energy density of NVP and reduce its toxicity. Strategies to achieve this goal include reducing or eliminating vanadium, increasing the working voltage, and activating multi-electron reactions. Na3MnTi(PO4)3 is considered an ideal cathode material due to its low cost and low toxicity.
[0050] However, the disadvantages of Na3MnTi(PO4)3 are rather obvious, mainly including low electronic conductivity, Jahn-Teller distortion, and high Na + diffusion energy barrier, resulting in insufficient reversible capacity and poor rate performance at high current densities.
[0051] To solve the problems existing in the above related technologies, according to the first aspect of the present invention, a sodium cathode material is provided, and the sodium cathode material comprises carbon-doped Na 3+y Mn 1-x A x Ti 1-y B y (PO4)3;
[0052] wherein, 0.01 < x ≤ 0.3, 0.01 < y ≤ 0.5, A is selected from one or more combinations of Ni, Cu, Zn, Mg, and Ca, B is selected from one or more combinations of Ni, Cu, Fe, Co, and Cr, and A is different from B.
[0053] In some embodiments, the sodium cathode material comprises one or more combinations of carbon-doped Na 3.3 Mn 0.8 Ni 0.2 Ti 0.7 Cr 0.3 (PO4)3, carbon-doped Na 3.3 Mn 0.8 Cu 0.2 Ti 0.7 Fe 0.3 (PO4)3, and carbon-doped Na 3.3 Mn 0.8 Ni 0.2 Ti 0.7 Co 0.3 (PO4)3.
[0054] In order to solve the problem of insufficient specific capacity and poor rate capability of Na3MnTi(PO4)3, metal doping and substitution are effective methods to adjust the crystal structure and thus change the inherent properties of electron / ion transport. The present invention adopts two or more elements for doping and substitution, which increases the conductivity of the sodium positive electrode material, increases the multi-electron redox reaction, improves the discharge voltage platform and capacity, and suppresses Jahn-Teller distortion, thereby improving the charge and discharge specific capacity, first coulomb efficiency and rate performance of the battery.
[0055] B is selected from one or a combination of two or more of Ni, Cu, Fe, Co and Cr, and the redox potential is higher than that of Ti 3+ / Ti 4+ Ni, Cu, Fe, Co and Cr can all undergo redox reactions in sodium manganese titanium phosphate materials. Doping with B elements can not only replace part of Ti, but also increase multi-electron redox reactions during the charge and discharge process, which can increase the voltage platform of the material and provide capacity through redox reactions.
[0056] A element is selected from one or a combination of two or more of Ni, Cu, Zn, Mg and Ca, which can replace part of Mn 2+ The main function is to reduce the Mn content, reduce the Jahn-Teller effect of Mn, and enhance the cyclic stability of the material.
[0057] In a second aspect, the present invention provides a method for preparing the sodium battery positive electrode material.
[0058] In some embodiments, the method for preparing the sodium positive electrode material comprises: mixing a sodium source, a manganese source, a titanium source, a phosphorus source, a dopant containing A, a dopant containing B, and a carbon source in water to obtain a precursor slurry;
[0059] The precursor slurry is dried and then calcined in an inactive gas to obtain the sodium positive electrode material.
[0060] A is selected from one or a combination of two or more of Ni, Cu, Zn, Mg and Ca, B is selected from one or a combination of two or more of Ni, Cu, Fe, Co and Cr, and A is different from B.
[0061] The inactive gas refers to a gas that does not react with carbon.
[0062] In some embodiments, the method for preparing the sodium positive electrode material satisfies at least one of the following (1)-(7):
[0063] (1) The sodium source includes one or a combination of two or more of sodium acetate, sodium oxalate, sodium carbonate, sodium bicarbonate and sodium hydroxide; preferably sodium acetate and sodium oxalate, and no other impurities are introduced;
[0064] (2) the manganese source includes one or a combination of two or more of manganese acetate, manganese oxalate and manganese nitrate; preferably manganese oxalate and manganese oxalate, which will not introduce other impurities;
[0065] (3) The titanium source includes one or a combination of two or more of titanium dioxide, titanium oxalate, tetrabutyl titanate and dihydroxybis(ammonium lactate) titanium; titanium oxalate is preferred, as it will not introduce other impurities;
[0066] (4) the phosphorus source includes one or a combination of two or more of diammonium phosphate, diammonium hydrogen phosphate and phosphoric acid;
[0067] (5) The carbon source includes one or a combination of two or more of carbon nanofibers, carbon nanotubes, graphene, graphene oxide, acetylene black, citric acid, glucose, and sucrose; preferably carbon nanotubes, which have better electrical conductivity;
[0068] (6) The A-containing dopant includes one or a combination of two or more of nickel acetate, copper acetate, zinc acetate, magnesium acetate, calcium acetate, nickel oxalate, copper oxalate, zinc oxalate, magnesium oxalate and calcium oxalate;
[0069] (7) The B-containing dopant includes one or a combination of two or more of ferric acetate, cobalt acetate, chromium acetate, ferric oxalate, cobalt oxalate and chromium oxalate.
[0070] In some embodiments, the carbon source is present in an amount of 5-15 wt % of the total amount of the sodium source, the manganese source, the titanium source, the phosphorus source, the A-containing dopant, and the B-containing dopant;
[0071] And / or, in terms of weight percentage, the amount of water added is 10%-50% of the total weight of the sodium source, the manganese source, the titanium source, the phosphorus source, the A-containing dopant and the B-containing dopant.
[0072] In some embodiments, the molar ratio of the sodium element in the sodium source, the manganese element in the manganese source, the titanium element in the titanium source, the phosphorus element in the phosphorus source, the A element in the A-containing dopant, and the B element in the B-containing dopant is (3+y):(1-x):x:(1-y):y; wherein 0.01 <x≤0.3,0.01<y≤0.5;
[0073] Optionally, the molar ratio of the sodium element in the sodium source, the manganese element in the manganese source, the titanium element in the titanium source, the phosphorus element in the phosphorus source, the A element in the A-containing dopant and the B element in the B-containing dopant is 3.3:0.8:0.2:0.7:0.3:3.
[0074] In some embodiments, the drying is spray drying, and during the spray drying process, the feed rate is 1-5 L / h;
[0075] and / or, the air inlet temperature is 180-220°C;
[0076] And / or, the air outlet temperature is 90-110°C.
[0077] The carbon source and other raw materials are spray-dried, and the product after calcination is in the form of microspherical particles with minimal agglomeration, which is conducive to high-density stacking. At the same time, the carbon coating on the surface of the spherical particles forms a fast conductive network, which significantly improves the electronic conductivity. The prepared positive electrode material has a high rate performance.
[0078] In some embodiments, the calcination temperature is 200-800°C;
[0079] The calcination is divided into two stages, including:
[0080] In the first stage, the temperature is raised to 200°C-350°C, and the holding time is 1h-5h; optionally, the heating rate in the first stage is 1°C / min-5°C / min;
[0081] The second stage is to heat up to 600°C-800°C, and the heat preservation time is 6h-15h; optionally, the heating rate of the second stage is 0.5°C / min-1°C / min.
[0082] In some embodiments, the inert gas includes nitrogen and / or an inert gas;
[0083] Optionally, the inert gas includes one or a combination of two or more of helium, neon, argon, krypton, xenon and radon.
[0084] In a third aspect, the present invention also provides an application of the sodium-ion positive electrode material or the sodium-ion positive electrode material obtained by the preparation method in a sodium-ion battery.
[0085] The present invention is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed by the present invention.
[0086] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0087] Example 1
[0088] This embodiment provides a sodium positive electrode material, and the preparation method thereof is as follows:
[0089] (1) Sodium acetate, manganese acetate, nickel acetate, titanium oxalate, chromium acetate, and ammonium dihydrogen phosphate are weighed respectively according to a molar ratio of 3.4:0.8:0.2:0.7:0.3:3, wherein the amount of sodium acetate is slightly excessive on the basis of the theoretical molar amount to supplement the volatilization of the sodium element during high-temperature calcination; then 10 wt% of the total mass of the above raw materials, carbon nanotubes, sodium acetate, manganese acetate, nickel acetate, titanium oxalate, chromium acetate, ammonium dihydrogen phosphate and carbon nanotubes are weighed, and sodium acetate, manganese acetate, nickel acetate, titanium oxalate, chromium acetate, ammonium dihydrogen phosphate and carbon nanotubes are fully stirred and dissolved in pure water (wherein the total mass of sodium acetate, manganese acetate, nickel acetate, titanium oxalate, chromium acetate, and ammonium dihydrogen phosphate accounts for 30% of the mass of pure water) to obtain a precursor slurry;
[0090] (2) conveying the precursor slurry in step (1) to a spray dryer with an inlet air temperature of 190° C. and an outlet air temperature of 105° C. at a preset feeding rate of 3 L / h, and spray drying to obtain a gray precursor powder;
[0091] (3) The precursor powder in step (2) was heated to 300°C at a heating rate of 2°C / min under nitrogen conditions, and calcined at 300°C for 3 hours, and then heated to 650°C at a heating rate of 1°C / min, and calcined at 650°C for 10 hours. After sintering, the precursor powder was naturally cooled in the furnace to obtain Na 3.3 Mn 0.8 Ni 0.2 Ti 0.7 Cr 0.3 (PO4)3 / C cathode material (carbon-doped Na 3.3 Mn 0.8 Ni 0.2 Ti 0.7 Cr 0.3 (PO4)3); Figure 1 Yes 3.3 Mn 0.8 Ni 0.2 Ti 0.7 Cr 0.3 Scanning electron microscope image of (PO4)3 / C positive electrode material.
[0092] Embodiment 2:
[0093] This embodiment provides a sodium positive electrode material, and the preparation method thereof is as follows:
[0094] (1) Sodium oxalate, manganese oxalate, copper acetate, titanium dioxide, ferric acetate, and ammonium dihydrogen phosphate are weighed respectively according to a molar ratio of 3.3:0.9:0.1:0.8:0.2:3, wherein the amount of sodium oxalate is slightly excessive on the basis of the theoretical molar amount to supplement the volatilization of the sodium element during high-temperature calcination; 10 wt% of the total mass of the above raw materials is weighed for nano-carbon fibers, and the above raw materials and nano-carbon fibers are fully stirred and dissolved in pure water (wherein the total mass of each raw material accounts for 30 wt.% of the mass of pure water) to obtain a precursor slurry;
[0095] (2) conveying the precursor slurry in step (1) to a spray dryer with an inlet air temperature of 180° C. and an outlet air temperature of 90° C. at a preset feeding rate of 3 L / h, and spray drying to obtain a gray precursor powder;
[0096] (3) The precursor powder in step (2) is heated to 200°C at a heating rate of 1°C / min under helium conditions, and is calcined at 200°C for 5 h, and then heated to 600°C at a heating rate of 0.5°C / min, and is calcined at 600°C for 15 h. After sintering, the precursor powder is naturally cooled in the furnace to obtain Na 3.2 Mn 0.9 Cu 0.1 Ti 0.8 Fe 0.2 (PO4)3 / C cathode material (carbon-doped Na 3.2 Mn 0.9 Cu 0.1 Ti 0.8 Fe 0.2 (PO4)3).
[0097] Embodiment 3:
[0098] This embodiment provides a sodium positive electrode material, and the preparation method thereof is as follows:
[0099] (1) Sodium carbonate, manganese nitrate, nickel acetate, tetrabutyl titanate, cobalt acetate, and diammonium hydrogen phosphate are weighed respectively according to a molar ratio of 3.5:0.7:0.3:0.6:0.4:3, wherein the amount of sodium carbonate is slightly excessive on the basis of the theoretical molar amount to supplement the volatilization of the sodium element during high-temperature calcination; 10 wt% of the total mass of the above raw materials and graphene are weighed, and the above raw materials and graphene are fully stirred and dissolved in pure water (wherein the total mass of each raw material accounts for 30% of the mass of pure water) to obtain a precursor slurry;
[0100] (2) conveying the precursor slurry in step (1) to a spray dryer with an inlet air temperature of 220° C. and an outlet air temperature of 110° C. at a preset feeding rate of 3 L / h, and spray drying to obtain a gray precursor powder;
[0101] (3) The precursor powder in step (2) was heated to 350°C at a heating rate of 2°C / min under argon conditions, and calcined at 350°C for 1 hour, then heated to 800°C, and calcined at 800°C for 6 hours. After sintering, the precursor powder was naturally cooled in the furnace to obtain Na4Mn 0.7 Ni 0.3 Ti 0.6 Co 0.4 (PO4)3 / C cathode material (carbon-doped Na4Mn 0.7 Ni 0.3 Ti 0.6 Co 0.4 (PO4)3).
[0102] Embodiment 4:
[0103] This embodiment provides a sodium positive electrode material, and the preparation method thereof is as follows:
[0104] (1) Sodium bicarbonate, manganese acetate, magnesium acetate, dihydroxy di(ammonium lactate) titanium, nickel acetate, and diammonium hydrogen phosphate are weighed respectively in a molar ratio of 3.3:0.9:0.1:0.8:0.2:3, wherein the amount of sodium bicarbonate is slightly excessive on the basis of the theoretical molar amount to supplement the volatilization of the sodium element during high-temperature calcination; acetylene black accounting for 10 wt% of the total mass of the above raw materials is weighed, and the above raw materials and acetylene black are fully stirred and dissolved in pure water (wherein the total mass of each raw material accounts for 30% of the mass of pure water) to obtain a precursor slurry;
[0105] (2) conveying the precursor slurry in step (1) to a spray dryer with an inlet air temperature of 220° C. and an outlet air temperature of 110° C. at a preset feeding rate of 3 L / h, and spray drying to obtain a gray precursor powder;
[0106] (3) The precursor powder in step (2) was heated to 350° C. at a heating rate of 2° C. / min under argon gas, and calcined at 350° C. for 1 h, then heated to 800° C., and calcined at 800° C. for 6 h. After sintering, the precursor powder was naturally cooled in the furnace to obtain Na 3.2 Mn 0.9 Mg 0.1 Ti 0.8 Ni 0.2 (PO4)3 / C cathode material (carbon-doped Na 3.2 Mn 0.9 Mg 0.1 Ti 0.8 Ni 0.2 (PO4)3).
[0107] Embodiment 5:
[0108] This embodiment provides a sodium positive electrode material, and the preparation method thereof is as follows:
[0109] (1) Sodium hydroxide, manganese acetate, zinc acetate, dihydroxy di(ammonium lactate) titanium, ferrous oxalate, and diammonium hydrogen phosphate were weighed respectively according to a molar ratio of 3.2:0.9:0.1:0.9:0.1:3, wherein the amount of sodium hydroxide was slightly excessive on the basis of the theoretical molar amount to supplement the volatilization of the sodium element during high-temperature calcination; glucose accounting for 10 wt% of the total mass of the above raw materials was weighed, and the above raw materials and glucose were fully stirred and dissolved in pure water (wherein the total mass of each raw material accounted for 30% of the mass of pure water) to obtain a precursor slurry;
[0110] (2) conveying the precursor slurry in step (1) to a spray dryer with an inlet air temperature of 220° C. and an outlet air temperature of 110° C. at a preset feeding rate of 3 L / h, and spray drying to obtain a gray precursor powder;
[0111] (3) The precursor powder in step (2) was heated to 350° C. at a heating rate of 2° C. / min under argon gas, and calcined at 350° C. for 1 h, then heated to 800° C., and calcined at 800° C. for 6 h. After sintering, the precursor powder was naturally cooled in the furnace to obtain Na 3.1 Mn 0.9 Zn 0.1 Ti 0.9 Fe 0.1 (PO4)3 / C cathode material (carbon-doped Na 3.1 Mn 0.9 Zn 0.1 Ti 0.9 Fe 0.1 (PO4)3).
[0112] Comparative Example 1:
[0113] This comparative example provides a sodium positive electrode material, and the preparation method thereof is as follows:
[0114] (1) Sodium acetate, manganese acetate, titanium oxalate, and ammonium dihydrogen phosphate are weighed respectively according to a molar ratio of 3.1:1:1:3, wherein the amount of sodium acetate is slightly excessive on the basis of the theoretical molar amount to supplement the volatilization of the sodium element during high-temperature calcination; 10 wt% of the total weight of the above raw materials is weighed, and the above raw materials and carbon nanotubes are fully stirred and dissolved in pure water (wherein the total weight of each raw material accounts for 30% of the weight of pure water) to obtain a precursor slurry;
[0115] (2) conveying the precursor slurry in step (1) to a spray dryer with an inlet air temperature of 190° C. and an outlet air temperature of 105° C. at a preset feeding rate of 3 L / h, and spray drying to obtain a gray precursor powder;
[0116] (3) The precursor powder in step (2) is heated to 300°C at a heating rate of 2°C / min under nitrogen conditions, and is calcined at 300°C for 3 hours, then heated to 650°C, and calcined at 650°C for 10 hours. After sintering, it is naturally cooled in the furnace to obtain Na3MnTi(PO4)3 / C positive electrode material.
[0117] Comparative Example 2:
[0118] This comparative example provides a sodium positive electrode material, and the preparation method thereof is as follows:
[0119] (1) Sodium acetate, manganese acetate, titanium oxalate, chromium acetate, and ammonium dihydrogen phosphate are weighed respectively in a molar ratio of 3.4:1.0:0.7:0.3:3, wherein the amount of sodium acetate is slightly excessive on the basis of the theoretical molar amount to supplement the volatilization of the sodium element during high-temperature calcination; 10 wt% of the total weight of the above raw materials is weighed, and the above raw materials and carbon nanotubes are fully stirred and dissolved in pure water (wherein the total weight of each raw material accounts for 30% of the weight of pure water) to obtain a precursor slurry;
[0120] (2) conveying the precursor slurry in step (1) to a spray dryer with an inlet air temperature of 190° C. and an outlet air temperature of 105° C. at a preset feeding rate of 3 L / h, and spray drying to obtain a gray precursor powder;
[0121] (3) The precursor powder in step (2) was heated to 300°C at a heating rate of 2°C / min under nitrogen conditions, and calcined at 300°C for 3 hours, then heated to 650°C, and calcined at 650°C for 10 hours. After sintering, the precursor powder was naturally cooled in the furnace to obtain Na 3.3 MnTi 0.7 Cr 0.3 (PO4)3 / C cathode material (carbon-doped Na 3.3 MnTi 0.7 Cr 0.3 (PO4)3).
[0122] Comparative Example 3:
[0123] This comparative example provides a sodium positive electrode material, and the preparation method thereof is as follows:
[0124] (1) Sodium acetate, manganese acetate, nickel acetate, titanium oxalate, and ammonium dihydrogen phosphate are weighed respectively according to a molar ratio of 3.1:0.8:0.2:1.0:3, wherein the amount of sodium acetate is slightly excessive on the basis of the theoretical molar amount to supplement the volatilization of the sodium element during high-temperature calcination; then 10 wt% of the total mass of the above raw materials is weighed, and the sodium acetate, manganese acetate, nickel acetate, titanium oxalate, ammonium dihydrogen phosphate and carbon nanotubes are fully stirred and dissolved in pure water (wherein the total mass of each raw material accounts for 30% of the mass of pure water) to obtain a precursor slurry;
[0125] (2) conveying the precursor slurry in step (1) to a spray dryer with an inlet air temperature of 190° C. and an outlet air temperature of 105° C. at a preset feeding rate of 3 L / h, and spray drying to obtain a gray precursor powder;
[0126] (3) The precursor powder in step (2) was heated to 300°C at a heating rate of 2°C / min under nitrogen conditions, and calcined at 300°C for 3 hours, and then heated to 650°C at a heating rate of 1°C / min, and calcined at 650°C for 10 hours. After sintering, the precursor powder was naturally cooled in the furnace to obtain Na3Mn 0.8 Ni 0.2 Ti(PO4)3 / C cathode material (carbon-doped Na3Mn 0.8 Ni 0.2 Ti(PO4)3).
[0127] Test Example 1 Electrical Performance Test
[0128] Test method:
[0129] (1) The positive electrode materials, PVDF and SP obtained in Examples 1-3 and Comparative Examples 1-2 were mixed in a ratio of 80 (positive electrode material): 10 (PVDF): 10 (SP), and the mixture was homogenized, coated, dried and cut in N-methylpyrrolidone (solvent) to form a positive electrode sheet, a metal Na sheet was used as a counter electrode, a glass fiber was used as a separator, and 1 mol / L NaPF6 was mixed in a solution of ethylene carbonate (EC) / dimethyl carbonate (DMC) / ethyl methyl carbonate (EMC) (volume ratio 1:1:0.5) as an electrolyte. During the test, a CR2032 button cell was assembled consisting of a positive electrode sheet, a glass fiber separator, a Na sheet, a gasket and a spring.
[0130] (2) Place the button cell into the blue battery test system for electrical performance testing.
[0131] First, activate the battery: voltage range 1.5V-4.3V, charge and discharge once at 0.05C / 0.05C;
[0132] Then, capacity test: voltage range 1.5V-4.3V, first cycle 0.1C / 0.1C charge and discharge for specific capacity test;
[0133] Finally, rate performance test: voltage range 1.5V-4.3V, charge and discharge cycle once at 0.1C / 0.1C, 0.2C / 0.2C, 0.5C / 0.5C, 1C / 1C, 2C / 2C, 4C / 4C rates for rate performance test.
[0134] Test results:
[0135] The first cycle 0.1C / 0.1C charge-discharge specific capacity test results are shown in Table 1, and the rate performance test results are shown in Table 2.
[0136] Table 1 First cycle charge and discharge specific capacity test results
[0137]
[0138]
[0139] Table 2 Rate performance test results
[0140]
[0141] As can be seen from Table 1, the battery prepared using the sodium-based positive electrode material of the present application has a first-cycle 0.1C / 0.1C charge capacity of more than 163.4 mAh / g, a first-cycle 0.1C / 0.1C discharge capacity of more than 157.8 mAh / g, and a first coulombic efficiency of more than 96.1%. The charge and discharge capacity and first coulombic efficiency of the battery prepared using the sodium-based positive electrode material of the present application are higher than those of Comparative Example 1, Comparative Example 2 or Comparative Example 3, indicating that the present application can significantly improve the charge and discharge capacity and first coulombic efficiency of the battery by doping elements A and B on the basis of Na3MnTi(PO4)3. As can be seen from Table 2, the 0.2C / 0.2C discharge specific capacity, 0.5C / 0.5C discharge specific capacity, 1C / 1C discharge specific capacity, 2C / 2C discharge specific capacity, and 4C / 4C discharge specific capacity of the battery prepared using the sodium-based positive electrode material of the present application are significantly higher than those of the battery prepared using the sodium-based positive electrode material of Comparative Example 1 or Comparative Example 2, indicating that the present application can significantly improve the rate performance of the battery by doping elements A and B on the basis of Na3MnTi(PO4)3.
[0142] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A sodium positive electrode material, characterized in that: The sodium positive electrode material includes carbon-doped Na 3+y Mn 1-x A x Ti 1-y B y (PO4)3; Among them, 0.01 < x ≤ 0.3, 0.01 < y ≤ 0.5, A is selected from one or more combinations of Ni, Cu, Zn, Mg, and Ca, B is selected from one or more combinations of Ni, Cu, Fe, Co, and Cr, and A is different from B.
2. The sodium positive electrode material according to claim 1, characterized in that The sodium positive electrode material includes carbon-doped Na 3.3 Mn 0.8 Ni 0.2 Ti 0.7 Cr 0.3 (PO4)3, carbon-doped Na 3.3 Mn 0.8 Cu 0.2 Ti 0.7 Fe 0.3 (PO4)3 and carbon-doped Na 3.3 Mn 0.8 Ni 0.2 Ti 0.7 Co 0.3 (PO4)3 or a combination of two or more thereof.
3. A method for preparing a sodium positive electrode material according to claim 1 or 2, characterized in that: The method for preparing the sodium-based cathode material includes: mixing a sodium source, a manganese source, a titanium source, a phosphorus source, a dopant containing A, a dopant containing B, and a carbon source in water to obtain a precursor slurry; Drying the precursor slurry and then calcining it in an inert gas to obtain the sodium-based cathode material.
4. The method for preparing a sodium positive electrode material according to claim 3, characterized in that: The method for preparing the sodium-based cathode material satisfies at least one of the following (1)-(7): (1) The sodium source includes one or more combinations of sodium acetate, sodium oxalate, sodium carbonate, sodium bicarbonate, and sodium hydroxide; (2) The manganese source includes one or more combinations of manganese acetate, manganese oxalate, and manganese nitrate; (3) The titanium source includes one or more combinations of titanium dioxide, titanium oxalate, tetrabutyl titanate, and bis(ammonium lactate)titanium dihydroxide; (4) The phosphorus source includes one or more combinations of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and phosphoric acid; (5) The carbon source includes one or more combinations of nanofiber carbon, carbon nanotubes, graphene, graphene oxide, acetylene black, citric acid, glucose, and sucrose; (6) The dopant containing A includes one or more combinations of nickel acetate, copper acetate, zinc acetate, magnesium acetate, calcium acetate, nickel oxalate, copper oxalate, zinc oxalate, magnesium oxalate, and calcium oxalate; (7) The dopant containing B includes one or more combinations of iron acetate, cobalt acetate, chromium acetate, iron oxalate, cobalt oxalate, and chromium oxalate.
5. The method for preparing a sodium positive electrode material according to claim 3 or 4, characterized in that: By weight percentage, the content of the carbon source is 5-15 wt% of the total content of the sodium source, the manganese source, the titanium source, the phosphorus source, the dopant containing A, and the dopant containing B; and / or, by weight percentage, the addition amount of water is 10%-50% of the total weight of the sodium source, the manganese source, the titanium source, the phosphorus source, the dopant containing A, and the dopant containing B.
6. The method for preparing a sodium positive electrode material according to claim 5, characterized in that: The molar ratio of sodium element in the sodium source, manganese element in the manganese source, titanium element in the titanium source, phosphorus element in the phosphorus source, A element in the dopant containing A, and B element in the dopant containing B is (3 + y):(1 - x):x:(1 - y):y; where 0.01 < x ≤ 0.3, 0.01 < y ≤ 0.5; Optionally, the molar ratio of sodium element in the sodium source, manganese element in the manganese source, titanium element in the titanium source, phosphorus element in the phosphorus source, A element in the dopant containing A, and B element in the dopant containing B is 3.3:0.8:0.2:0.7:0.3:
3.
7. The method for preparing a sodium positive electrode material according to claim 3 or 4, characterized in that: The drying is spray drying, and during the spray drying process, the feeding speed is 1-5 L / h; and / or, the inlet air temperature is 180-220 °C; and / or, the outlet air temperature is 90-110 °C.
8. The method for preparing a sodium positive electrode material according to claim 3 or 4, characterized in that: The temperature of the calcination is 200-800 °C; The calcination is divided into two stages, including: The first stage is heated to 200 °C - 350 °C, and the holding time is 1 h - 5 h; optionally, the heating rate in the first stage is 1 °C / min - 5 °C / min; The second stage is to heat up to 600°C-800°C, and the heat preservation time is 6h-15h; optionally, the heating rate of the second stage is 0.5°C / min-1°C / min.
9. The method for preparing a sodium positive electrode material according to claim 3 or 4, characterized in that: The inactive gas includes nitrogen and / or an inert gas; Optionally, the inert gas includes one or a combination of two or more of helium, neon, argon, krypton, xenon and radon.
10. Use of the sodium positive electrode material according to claim 1 or 2 or the sodium positive electrode material obtained by the preparation method according to any one of claims 3 to 9 in a sodium ion battery.
Citation Information
Cited By
Sodium-rich polyanion positive electrode material and preparation method thereof
CN119481011A
Titanium-site copper-doped high-performance titanium-manganese-sodium phosphate sodium-ion battery positive electrode material as well as preparation method and application thereof
CN120033241A