Functionalized additive for rate type sodium ion battery, negative electrode slurry, negative electrode pole piece and sodium ion battery
By using functional additives formed by condensation of carbon materials containing carboxyl or hydroxyl groups with alkaline sodium compounds or organic sodium salt amides, the problem of poor rate performance of sodium ion batteries is solved, the conduction and migration rate of sodium ions is improved, and the High-rate discharge retention rate of the battery.
Patent Information
- Application Number
- CN202310636939.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2023-05-31
- Publication Date
- 2024-11-22
AI Technical Summary
The rate performance of sodium ion batteries is poor, mainly due to the large radius of sodium ions, which lead to difficulty in diffusion and migration in the negative electrode material. Existing functional additives such as graphene or carbon nanotubes cannot effectively solve this problem.
Carbon materials containing carboxyl or hydroxyl groups are used to react with alkaline sodium compounds or condense with amino and sulfonic acid organic sodium salt amides to form functional additives, increase sodium ion conduction and migration rate, and improve the rate performance of the battery.
Through functional additives, the rate performance of sodium ion batteries is significantly improved, the migration rate of sodium ions and battery capacity of batteries are improved, the kinetic process of electrochemical reactions is enhanced, and the high rate discharge retention rate of the battery is enhanced.
Smart Images

Figure CN119008946A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and more specifically, to a functionalized additive for a rate-type sodium ion battery, a negative electrode slurry, a negative electrode sheet and a sodium ion battery. Background Art
[0002] The performance of the battery is closely related to the positive electrode sheet, negative electrode sheet, separator and electrolyte, especially the positive and negative electrode sheets play a key role in the overall performance of the battery. The negative electrode sheet is mainly obtained by drying the current collector and the negative electrode slurry coated on the current collector. The negative electrode slurry includes negative electrode active material, conductive agent, adhesive and solvent. And an excellent conductive agent needs to have high conductivity to increase the migration rate of electrons to improve the cycle performance of the battery. At present, the commonly used conductive agents for lithium-ion batteries include carbon black, conductive graphite, carbon fiber, etc., but the conductivity of these conductive agents is poor. Generally, graphene and carbon nanotubes are needed as functional additives together with conventional conductive agents to improve the conductivity of the conductive agent, or graphene and carbon nanotubes are directly used as conductive agents to improve the cycle performance of lithium-ion batteries.
[0003] However, lithium resources are limited and unevenly distributed, causing its price to continue to rise, so non-lithium batteries are urgently needed as a supplement; sodium resources are abundant and low-cost, attracting more and more attention. Sodium-ion batteries have a similar working principle to lithium-ion batteries, but sodium ions have a larger radius. During high-rate charge and discharge, it is difficult for them to diffuse and migrate quickly and timely in the negative electrode material (hard carbon or soft carbon), resulting in poor rate performance of sodium-ion batteries, and existing conventional functional additives (graphene or carbon nanotubes) cannot solve this problem. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects and shortcomings of the existing sodium ion negative electrode, such as poor electronic conductivity and low sodium ion diffusion rate, and to provide a functional additive for rate-type sodium ion batteries.
[0005] Another object of the present invention is to provide a negative electrode slurry for a rate-type sodium ion battery.
[0006] Another object of the present invention is to provide a method for preparing a negative electrode slurry for a rate-type sodium ion battery.
[0007] Another object of the present invention is to provide a negative electrode sheet made from the above-mentioned battery negative electrode slurry for a rate-type sodium ion battery.
[0008] Another object of the present invention is to provide a sodium ion battery comprising the above-mentioned negative electrode plate.
[0009] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0010] The present invention protects a functionalized additive used in a rate-type sodium ion battery. The functionalized additive is obtained by reacting a carbon material containing a carboxyl group or a hydroxyl group with an alkaline sodium compound; and / or, is obtained by condensing a carbon material containing a carboxyl group with an organic sodium salt amide containing an amino group and a sulfonic acid group.
[0011] The above functional additives are made of carbon materials through Na + The modified carbon material contains a large number of oxygen-containing functional groups (such as -COOH or -OH), which can not only undergo a neutralization reaction with alkaline sodium compounds to form -COONa or -ONa, thereby increasing the sodium ion conductivity while playing a sodium supplementing role, thereby improving the capacity of the sodium ion battery; it can also undergo an amide condensation reaction with alkane organic sodium salts containing amino and sulfonic acid functional groups, and graft sulfonic acid groups with higher electronegativity on the surface of the carbon material, further increasing the migration rate of sodium ions, promoting the kinetic process of the electrochemical reaction, and thereby improving the rate performance of the sodium ion battery.
[0012] It should also be noted that the above-mentioned basic sodium compound refers to a substance that can react with a carboxyl group or a hydroxyl group on a carbon material to generate -COONa or -ONa.
[0013] Specifically, the carbon material containing carboxyl or hydroxyl groups is one or more of graphene oxide, oxidized carbon nanotubes and oxidized carbon fibers. Optionally, the oxidized carbon nanotubes are oxidized single-walled carbon nanotubes and / or oxidized multi-walled carbon nanotubes.
[0014] Specifically, the alkaline sodium compound is one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate and sodium ethoxide. Optionally, the organic sodium salt is sodium aminobenzenesulfonate and / or sodium m-aminobenzenesulfonate.
[0015] Specifically, the mass ratio of the carbon material containing carboxyl or hydroxyl groups to the alkaline sodium compound is 1:(0.5-1.2), and the reaction temperature is 50-60°C.
[0016] The present invention also protects a battery negative electrode slurry for a rate-type sodium ion battery, comprising a negative electrode active material, a thickener, a conductive agent, an adhesive and the above-mentioned functional additive.
[0017] Specifically, based on the total mass fraction of the negative electrode active material, the thickener, the conductive agent, the binder and the functional additive being 100%, the mass fraction of the functional additive is 0.1% to 1%.
[0018] The present invention can better enhance both electronic conduction and ion conduction by regulating the ratio of the functional additive and other components in the negative electrode slurry of the sodium ion battery, thereby significantly improving the rate performance of the sodium ion battery.
[0019] Preferably, the mass fraction of the functional additive is 0.1% to 0.5%, and more preferably, the mass fraction is 0.25% to 0.5%.
[0020] Specifically, the graphene oxide can be prepared by a modified Hummer method, and the oxidized carbon nanotubes or oxidized carbon fibers can be prepared by a mixed acid oxidation method.
[0021] In a specific embodiment, the mass ratio of the negative electrode active material, the thickener, the conductive agent and the binder is (92-95):(0-2):(1-3):(2-3).
[0022] Optionally, the negative electrode active material is amorphous carbon; and the thickener is carboxymethyl cellulose.
[0023] Specifically, the conductive agent is one or more of conductive graphite, carbon black, acetylene black, Ketjen black, carbon nanotubes, carbon fiber and graphene; the binder is at least one of styrene-butadiene rubber, polyacrylate resin, sodium alginate, polyimide resin and polyacrylonitrile resin.
[0024] The present invention also protects a method for preparing the above-mentioned rate-type sodium ion battery negative electrode slurry, comprising the following steps:
[0025] The negative electrode active material, thickener, conductive agent, adhesive, functional additive and organic solvent are uniformly mixed to form a mixture with a solid content of 40% to 55%, thereby obtaining a negative electrode slurry for a rate-type sodium ion battery.
[0026] A negative electrode plate comprises a current collector and a negative electrode active layer, wherein the negative electrode active layer is prepared from the above-mentioned battery negative electrode slurry for a rate-type sodium ion battery.
[0027] A sodium ion battery including the above-mentioned negative electrode plate is also within the protection scope of the present invention.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The invention provides a new functionalized additive, which is obtained by reacting a carbon material containing a carboxyl group with an alkaline sodium compound, and / or by condensing a carbon material containing a carboxyl group with an organic sodium salt amide containing an amino group and a sulfonic acid group; the functionalized additive is mainly composed of graphene, carbon nanotubes or carbon fibers, and Na+ or Na+-containing functional groups are grafted on the surface thereof, wherein Na can supplement sodium, increase sodium ion conduction, and improve capacity; the sulfonic acid group has a large electronegativity, can accelerate the migration rate of sodium ions, promote the kinetic process of electrochemical reactions, and simultaneously improve electronic and ion conduction, thereby improving the rate performance of the battery.
[0030] Based on the application of new functional additives in rate-type sodium ion batteries, the present invention further provides a negative electrode slurry for sodium ion batteries, which uses graphene oxide, oxidized carbon nanotubes or oxidized carbon fibers as carriers, reacts with alkaline sodium compounds and alkane organic sodium salts containing amino and sulfonic acid functional groups, and grafts Na+ or Na+ functional groups on the surface to form functional additives, which not only increases sodium ion conduction while playing a sodium supplementing role, thereby improving the capacity of the sodium ion battery; it can also undergo an amide condensation reaction with alkane organic sodium salts containing amino and sulfonic acid functional groups, and graft sulfonic acid groups with larger electronegativity on the surface of the carbon material, further increasing the migration rate of sodium ions, promoting the kinetic process of the electrochemical reaction, and thereby improving the rate performance of the sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 1 is the AC impedance diagram of the sodium ion battery of Comparative Example 1 and Example 1.
[0032] Figure 2 This is a rate performance diagram of the sodium ion battery of Comparative Example 1 and Example 1. DETAILED DESCRIPTION
[0033] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0034] Example 1
[0035] A sodium ion battery negative electrode slurry is obtained by the following preparation method:
[0036] The negative electrode active material (hard carbon), thickener (carboxymethyl cellulose), conductive agent (conductive carbon black), adhesive (styrene-butadiene rubber), and functional additive (modified graphene I) are uniformly mixed with deionized water in a mass ratio of 93:2:1.5:3:0.5 to form a mixture with a solid content of 45%, thereby obtaining a negative electrode slurry for a sodium ion battery.
[0037] Wherein, the above functional additive is prepared by the following preparation method:
[0038] First, NaOH (sodium carbonate, sodium bicarbonate or sodium ethoxide) is dissolved in deionized water to prepare a 0.5-1.2M dilute solution, and then 50-100 mg of graphene oxide powder is added, and ultrasonic dispersion is performed for 2 hours to make it evenly dispersed, and then stirred at a temperature of 50-60°C overnight, filtered, washed, and dried to obtain modified graphene I.
[0039] Example 2
[0040] A sodium ion battery negative electrode slurry is obtained by the following preparation method:
[0041] The negative electrode active material (hard carbon), thickener (carboxymethyl cellulose), conductive agent (conductive carbon black), adhesive (styrene-butadiene rubber), and functional additive are uniformly mixed with deionized water in a mass ratio of 92.5:2:1.5:3:1 to form a mixture with a solid content of 40%, thereby obtaining a negative electrode slurry for a sodium ion battery.
[0042] Among them, the above-mentioned functional additive is the same as that in Example 1, which is modified graphene I.
[0043] Example 3
[0044] A sodium ion battery negative electrode slurry is obtained by the following preparation method:
[0045] The negative electrode active material (hard carbon), thickener (carboxymethyl cellulose), conductive agent (conductive carbon black), adhesive (styrene-butadiene rubber), and functional additive are uniformly mixed with deionized water in a mass ratio of 93.25:2:1.5:3:0.25 to form a mixture with a solid content of 45%, thereby obtaining a negative electrode slurry for a sodium ion battery.
[0046] Among them, the above-mentioned functional additive is the same as that in Example 1, which is modified graphene I.
[0047] Example 4
[0048] A sodium ion battery negative electrode slurry is obtained by the following preparation method:
[0049] The negative electrode active material (hard carbon), thickener (carboxymethyl cellulose), conductive agent (conductive carbon black), adhesive (styrene-butadiene rubber), and functional additive are uniformly mixed with deionized water in a mass ratio of 93.4:2:1.5:3:0.1 to form a mixture with a solid content of 45%, thereby obtaining a negative electrode slurry for a sodium ion battery.
[0050] Among them, the above-mentioned functional additive is the same as that in Example 1, which is modified graphene I.
[0051] Example 5
[0052] A sodium ion battery negative electrode slurry is obtained by the following preparation method:
[0053] The negative electrode active material (hard carbon), thickener (carboxymethyl cellulose), conductive agent (conductive carbon black), adhesive (styrene-butadiene rubber), and functional additives are uniformly mixed with deionized water in a mass ratio of 92.0:2:1.5:3:1.5 to form a mixture with a solid content of 45%, thereby obtaining a negative electrode slurry for a sodium ion battery.
[0054] Among them, the above-mentioned functional additive is the same as that in Example 1, which is modified graphene I.
[0055] Example 6
[0056] A sodium ion battery negative electrode slurry is obtained by the following preparation method:
[0057] The negative electrode active material (hard carbon), thickener (carboxymethyl cellulose), conductive agent (conductive carbon black), adhesive (styrene-butadiene rubber), and functional additive are uniformly mixed with deionized water in a mass ratio of 93:2:1.5:3:0.5 to form a mixture with a solid content of 45%, thereby obtaining a negative electrode slurry for a sodium ion battery.
[0058] Wherein, the above functional additive is prepared by the following preparation method:
[0059] S1. Add 0.5 g of single-walled carbon nanotubes (SWCNT) to 100 mL of concentrated sulfuric acid, and disperse them by ultrasonication at room temperature for 2 h. Then slowly add 50 mL of concentrated nitric acid to the mixture, and stir and react for 30 min at room temperature. Then transfer the mixture to a hydrothermal reactor and react at 150 ° C for 14 h. After the reaction solution is cooled, dilute it with deionized water, filter it, and vacuum dry it at 60 ° C for 24 h to obtain oxidized carbon nanotubes.
[0060] S2. Dissolve NaOH in deionized water to prepare a 0.5-1.2M dilute solution, add 50-100 mg of oxidized carbon nanotubes, and disperse them evenly by ultrasonic dispersion for 2 hours. Then stir at 50-60°C overnight, filter, wash, and dry to obtain modified carbon nanotubes.
[0061] Example 7
[0062] A sodium ion battery negative electrode slurry is obtained by the following preparation method:
[0063] The negative electrode active material (hard carbon), thickener (carboxymethyl cellulose), conductive agent (conductive carbon black), adhesive (styrene-butadiene rubber), and functional additive are uniformly mixed with deionized water in a mass ratio of 93:2:1.5:3:0.5 to form a mixture with a solid content of 45%, thereby obtaining a negative electrode slurry for a sodium ion battery.
[0064] Wherein, the above functional additive is prepared by the following preparation method:
[0065] S1. Add 0.5 g of carbon fiber to 100 mL of concentrated sulfuric acid, and ultrasonically disperse it at room temperature for 2 hours. Then slowly add 50 mL of concentrated nitric acid to the mixture, and stir and react for 30 minutes at room temperature. Then transfer it to a hydrothermal reactor and react at 150°C for 14 hours. After the reaction liquid is cooled, dilute it with deionized water, filter it, and vacuum dry it at 60°C for 24 hours to obtain oxidized carbon fiber.
[0066] S2. Dissolve NaOH in deionized water to prepare a 0.5-1.2M dilute solution, add 50-100 mg of oxidized carbon fiber, and disperse it evenly by ultrasonic dispersion for 2 hours. Then stir it at 50-60°C overnight, filter, wash and dry to obtain the modified carbon fiber.
[0067] Example 8
[0068] A sodium ion battery negative electrode slurry is obtained by the following preparation method:
[0069] The negative electrode active material (hard carbon), thickener (carboxymethyl cellulose), conductive agent (conductive carbon black), adhesive (styrene-butadiene rubber), and functional additive (modified graphene II) are uniformly mixed with deionized water in a mass ratio of 93:2:1.5:3:0.5 to form a mixture with a solid content of 45%, thereby obtaining a negative electrode slurry for a sodium ion battery.
[0070] Wherein, the above functional additive is prepared by the following preparation method:
[0071] First, 50-100 mg of graphene oxide powder and condensation agent EDC are added to 100 mL of deionized water, and ultrasonic dispersion is performed for 2 hours to make it evenly dispersed. Then, NaOH is added to adjust the pH of the solution to 8, and then a 0.5-1.2 M ethanol dilute solution of sodium aminobenzenesulfonate is added. After mixing evenly, the mixture is stirred at a temperature of 50-60° C. overnight. After suction filtration, washing, and drying, the modified graphene II is obtained.
[0072] Comparative Example 1
[0073] A sodium ion battery negative electrode slurry is obtained by the following preparation method:
[0074] The negative electrode active material (hard carbon), thickener (carboxymethyl cellulose), conductive agent (conductive carbon black), and adhesive (styrene-butadiene rubber) are uniformly mixed with deionized water in a mass ratio of 93.5:2:1.5:3 to form a mixture with a solid content of 45%, thereby obtaining a negative electrode slurry for a sodium ion battery.
[0075] Comparative Example 2
[0076] A sodium ion battery negative electrode slurry, the preparation method of which is basically the same as that of Example 1, except that the functionalized additive is graphene.
[0077] Results
[0078] The negative electrode slurries of the sodium ion battery in the above-mentioned Examples 1 to 8 and Comparative Examples 1 to 2 are respectively coated on the surface of aluminum foil, dried, and rolled to obtain the negative electrode sheet of the sodium ion battery. At the same time, the conventional positive electrode slurry of the sodium ion battery is coated on the surface of the aluminum foil, dried, and rolled to obtain the positive electrode sheet of the sodium ion battery, and the positive electrode sheet is assembled with the above-mentioned negative electrode sheet, separator and electrolyte into a 1Ah soft-pack battery cell, and the impedance of the battery cell at 50% SOC is tested, and the test frequency is 0.01Hz to 10000Hz.
[0079] The positive electrode active material in the above-mentioned conventional sodium ion battery positive electrode slurry is a layered transition metal oxide (other positive electrode active materials can also be used in the present invention, such as polyanion materials, etc.), and the positive electrode active material: binder: conductive carbon are uniformly mixed with NMP in a mass ratio of 95:2:3 to form a mixture with a solid content of 58% to 62%, thereby obtaining a sodium ion battery positive electrode slurry.
[0080] The above 1Ah soft-pack battery was fully charged at room temperature with a charging current of 0.5C, and discharged at 0.2C, 1C, 3C, and 5C respectively. The discharge capacity at 0.2C was taken as the initial capacity, and the capacity retention rate relative to the initial capacity at 1C, 3C, and 5C was tested respectively. Capacity retention rate = discharge capacity at different rates / initial capacity*100%.
[0081] Table 1
[0082]
[0083] It can be seen from Examples 1 to 5 that the capacity retention rate of the sodium ion battery under high rate (1C\3C\5C) conditions shows a trend of first increasing and then decreasing with the increase in the relative content of the functional additive in the negative electrode slurry of the sodium ion battery. It can be found from Examples 1 and 6 to 8 that, except for modified graphene I, when modified carbon nanotubes, modified carbon fibers and modified graphene II are used as functional additives, the sodium ion battery has excellent capacity retention rate under high rate conditions; it can be seen from Comparative Example 2 and Example 1 that when graphene is used as a functional additive, it is difficult to effectively improve the rate performance of the sodium ion battery. At the same time, Figure 1 and Figure 2 It can be seen that functional additives can significantly reduce the impedance of the battery cell and promote the migration of sodium ions, so that the battery cell has a 5C high-rate discharge retention rate of 94.4% at room temperature, while the battery cell without functional additives has a discharge capacity retention rate of only 89.6% at 5C rate at room temperature.
[0084] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A functional additive for a rate-type sodium ion battery, characterized in that: It is obtained by reacting a carbon material containing carboxyl or hydroxyl groups with an alkaline sodium compound; and / or, it is obtained by condensing a carbon material containing carboxyl groups with an organic sodium salt amide containing amino groups and sulfonic acid groups.
2. The functional additive according to claim 1, characterized in that: The carbon material containing carboxyl or hydroxyl groups is one or more of graphene oxide, carbon nanotube oxide and carbon fiber oxide.
3. The functional additive according to claim 1, characterized in that: The alkaline sodium compound is one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate and sodium ethoxide; The organic sodium salt is sodium aminobenzenesulfonate and / or sodium meta-aminobenzenesulfonate.
4. According to the functional additive according to claim 1, it is characterized in that: The mass ratio of the carbon material containing carboxyl or hydroxyl groups to the alkaline sodium compound is 1:(0.5-1.2).
5. A negative electrode slurry for a rate-type sodium ion battery, characterized in that: The invention comprises a negative electrode active material, a thickener, a conductive agent, an adhesive and the functional additive according to any one of claims 1 to 4.
6. The negative electrode slurry for a rate-type sodium ion battery according to claim 5, characterized in that: Based on the total mass fraction of the negative electrode active material, thickener, conductive agent, adhesive and functional additive being 100%, the mass fraction of the functional additive is 0.1% to 1%.
7. The negative electrode slurry for a rate-type sodium ion battery according to claim 6, characterized in that: The mass fraction of the functional additive is 0.1% to 0.5%.
8. The negative electrode slurry for a rate-type sodium ion battery according to claim 5, characterized in that: The mass ratio of the negative electrode active material, thickener, conductive agent and adhesive is (92-95):(0-2):(1-3):(2-3).
9. The negative electrode slurry for a rate-type sodium ion battery according to claim 5, characterized in that: The negative electrode active material is amorphous carbon; and the thickener is carboxymethyl cellulose.
10. The negative electrode slurry for a rate-type sodium ion battery according to claim 9, characterized in that: The conductive agent is one or more of conductive graphite, carbon black, acetylene black, Ketjen black, carbon nanotubes, carbon fiber and graphene; the binder is at least one of styrene-butadiene rubber, polyacrylate resin, sodium alginate, polyimide resin and polyacrylonitrile resin.
11. A method for preparing a negative electrode slurry for a rate-type sodium ion battery according to any one of claims 5 to 10, characterized in that: The following steps are involved: The negative electrode active material, thickener, conductive agent, adhesive, functional additive and organic solvent are uniformly mixed to form a mixture with a solid content of 40% to 55%, thereby obtaining a negative electrode slurry for a rate-type sodium ion battery.
12. A negative electrode sheet, comprising a current collector and a negative electrode active layer, characterized in that: The negative electrode active layer is prepared from the negative electrode slurry for a rate-type sodium ion battery according to any one of claims 5 to 10.
13. A sodium ion battery, characterized in that: Including the negative electrode sheet as described in claim 12.
Citation Information
Cited By
Isolating membrane for sodium-ion battery and preparation method of isolating membrane
CN120432813A