Composite solid electrolyte for secondary battery and preparation method thereof

By using composite solid electrolytes in secondary batteries, combining ionic conductive ceramics and polymers, and immersing liquid electrolytes in composite films, the problem of low stability of liquid electrolytes in lithium secondary batteries is solved, and high thermal stability is achieved and low interface impedance improve the electrochemical characteristics and stability of the battery.

CN119009082APending Publication Date: 2024-11-22SEVEN KING ENERGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411221347.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2016-09-21
Filing Date
2016-10-06
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The use of liquid electrolytes in existing lithium secondary batteries has problems of high flammability and low stability. Ceramic solid electrolytes have low ion conductivity and high interface impedance with the electrode at room temperature, resulting in poor battery stability and electrochemical characteristics.

Method used

By using a composite solid electrolyte, a composite film is formed by mixing 60 to 100 parts by weight of ionic conductive ceramics with 1 to 40 parts by weight of polymers, and a solution containing lithium ions or sodium ions in the liquid electrolyte is immersed therein to form a solution having a liquid electrolyte with lithium ions or sodium ions. Electrolytes with high thermal stability and low interfacial impedance.

Benefits of technology

Thermal stability above 400°C and electrochemical oxidation stability above 6V are achieved, which significantly reduces the interface impedance and improves the stability and electrochemical characteristics of the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009082A_ABST
    Figure CN119009082A_ABST
Patent Text Reader

Abstract

A composite solid electrolyte according to one embodiment of the present invention comprises: a composite thin film comprising 70 to 100 parts by weight of an ion-conductive ceramic and 1 to 30 parts by weight of a polymer; and an ionic liquid electrolyte containing lithium ions or sodium ions, the ionic liquid electrolyte being impregnated in the composite thin film. The composite solid electrolyte for a secondary battery according to the present invention and the method for preparing the same can provide a secondary battery having improved stability and electrochemical characteristics by applying an electrolyte having low interface impedance and high stability.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application based on the Chinese patent application with application number 201680089445.9 (international application number PCT / KR2016 / 011180), application date October 6, 2016, and invention name “Composite solid electrolyte for secondary battery and preparation method thereof”. Technical Field

[0002] The invention relates to a composite solid electrolyte for a secondary battery and a preparation method thereof, which can improve the stability and electrochemical characteristics of the battery. Background Art

[0003] Recently, large batteries used for power storage purposes, such as automotive batteries and stationary batteries, have attracted much attention. The reason is that the demand for large batteries used for electric vehicle stationary storage batteries has increased dramatically compared to the small batteries used for mobile phones, which have been the mainstream so far.

[0004] As the demand for large-sized batteries becomes higher, more improved performance than current secondary batteries is required in terms of ensuring the stability of secondary batteries and increasing battery life.

[0005] Although liquid electrolytes are widely used in commercialized secondary batteries such as lithium secondary batteries, the liquid electrolytes have high flammability and low stability, thereby causing a problem of reducing the stability of the battery.

[0006] In order to improve the stability of the above-mentioned lithium secondary batteries, research is being conducted on solid electrolytes that can replace liquid electrolytes. For example, although ceramic solid electrolytes are light in weight, have no electrolyte leakage, and have excellent variability, they have low ion conductivity at room temperature and high interface impedance with electrodes, resulting in the problem that the battery characteristics are not obvious. Summary of the invention

[0007] Technical Problems to be Solved by the Invention

[0008] The object of the present invention is to provide a composite solid electrolyte and a preparation method thereof which is made by applying ion conductive ceramics together with polymer and liquid electrolyte in order to improve the stability and electrochemical characteristics of the battery.

[0009] Technical Solution

[0010] In order to achieve the above-mentioned purpose, a composite solid electrolyte according to one embodiment of the present invention includes: a composite film, which includes 60 to 100 parts by weight of ion conductive ceramics and 1 to 40 parts by weight of a polymer; and a liquid electrolyte, which contains a solution mixed with lithium ions or sodium ions and a solvent, and the above-mentioned liquid electrolyte is impregnated in the above-mentioned composite film.

[0011] The composite thin film and the liquid electrolyte may be included in a weight ratio of 60 to 100:1 to 40.

[0012] The liquid electrolyte may be a solution in which 0.1 M or more of a lithium salt or a sodium salt is dissolved in a solvent.

[0013] The solvent may include an ionic liquid. Also, the solvent may be formed of an ionic liquid.

[0014] The thickness of the composite solid electrolyte may be less than 30 micrometers, and the thickness of the composite solid electrolyte may be between 0.1 micrometers and less than 30 micrometers.

[0015] The composite solid electrolyte may have a thermal stability above 400°C.

[0016] A secondary battery according to another embodiment of the present invention includes the above-mentioned composite solid electrolyte.

[0017] According to another embodiment of the present invention, a method for preparing a composite solid electrolyte comprises: a step (1) of preparing a mixture slurry by mixing 60 to 100 parts by weight of an ion conductive ceramic and 1 to 40 parts by weight of a polymer; a step (2) of preparing a composite film by molding the mixture slurry into a film form; and a step (3) of preparing a composite solid electrolyte by absorbing a liquid electrolyte in the composite film.

[0018] In the liquid electrolyte used for absorption in the step (3), the solvent may include an ionic liquid, or the solvent may be formed of an ionic liquid.

[0019] In the above step (3), the above composite film and the above liquid electrolyte may be provided in a weight ratio of 60 to 100:1 to 40 to perform the above absorption.

[0020] Hereinafter, the present invention will be described in more detail.

[0021] The inventors of the present invention are aware of the following disadvantages: although the ceramic solid electrolyte has high ion conductivity and lithium (or sodium) ion transport rate, the interface impedance is high, which has the disadvantage of reducing the electrochemical characteristics of the secondary battery. Although the polymer solid electrolyte has excellent variability, it has the disadvantages of low ion conductivity and electrochemical oxidation stability at room temperature and large interface impedance with the electrode. Thereafter, the inventors studied composite polymer electrolytes that improve the above-mentioned disadvantages and improve the stability of the secondary battery, while having high ion conductivity at room temperature and improving the electrochemical characteristics of the battery by reducing the interface impedance with the electrode. As a result, a composite solid electrolyte with thermal stability of more than 400 degrees (°C), electrochemical oxidation stability of more than 6V and low interface impedance was prepared through the structure of the present invention to complete the present invention.

[0022] A composite solid electrolyte according to an embodiment of the present invention comprises: a composite film comprising ion conductive ceramics and polymers; and a liquid electrolyte comprising a solution of lithium ions or sodium ions and a solvent. The liquid electrolyte exists in a state of being absorbed and impregnated in the composite film.

[0023] The above-mentioned ion conductive ceramics may include Al2O3 type, SiO2 type, BaTiO3 type, TiO2 type and Li as ion conductive ceramics. 1.3 Al 0.3 Ti 1.7 (PO4)3(LTAP), Li7La3Zr2O 12 (LLZO), Li5La3Ta2O 12 , Li9SiAlO8 lithium oxides, such as Li 10 GeP2S 12 , Li2S-P2S5, Li2S-Ga2S3-GeS2 lithium sulfides, such as Na3Zr2Si2PO 12 In addition, it can be applied to amorphous ionic conductive materials (phosphorus-based glass, oxide-based glass, oxide / sulfide based glass), sodium superionic conductor (Na superionic conductor, NASICON), sodium sulfide solid electrolytes, such as Na3Zr2Si2PO 12 Any one selected from the group consisting of sodium oxide-based solid electrolytes and combinations thereof.

[0024] Specifically, the ion conductive ceramic may include: lithium oxide ceramic, which is composed of Li 1.3 Al 0.3 Ti 1.7(PO4)3, Li7La3Zr2O 12 、Li5La3Ta2O 12 , Li9SiAlO8 and combinations thereof; lithium sulfide ceramics, which are selected from Li 10 GeP2S 12 , Li2S-P2S5, Li2S-Ga2S3-GeS2 and combinations thereof; a sodium superionic conductor (NASICON); a sodium sulfide ceramic, which is any one selected from the group consisting of Na2S-SiS2, Na2S-GeS2 and combinations thereof; or a sodium compound ceramic, which is any one selected from the group consisting of NaTi2(PO4)3, NaFe2(PO4)3, Na2(SO4)3, Na3Zr2Si2PO 12 Any one selected from the group consisting of and combinations thereof. As the above-mentioned ion conductive ceramic, Li 1.3 Al 0.3 Ti 1.7 (PO4)3(LTAP) or Na3Zr2Si2PO 12 , in this case, it can be easily prepared and the ionic conductivity can be further improved.

[0025] The polymer can be selected from polyvinylidene fluoride (PVdF) polymers, polyvinylidene fluoride-trifluoroethylene copolymer (P(VDF-TrFE)) polymers, polyethylene glycol (PEO) polymers, polyacrylonitrile (PAN) polymers, polymethyl methacrylate (PMMA) polymers, polyvinyl chloride (PVC) polymers, polyvinylpyrrolidone (PVP) polymers, polyimide (PI) polymers, polyethylene (PE) polymers, polyurethane (PU) polymers, polypropylene (PP) polymers, polypropylene oxide (PPO) polymers, polyethyleneimine (PE) polymers, polyurethane (PU) polymers, polypropylene oxide (PP) polymers, polypropylene oxide (PPO ... imine (PEI), polyethylene sulfide (PES), polyvinyl acetate (PVAc), polyethylene succinate (PESc), polyester (Polyester), polyamine (Polyamine), polysulfide (Polysulfide), silicon-based (Siloxane-based) polymers and combinations thereof. Specifically, as the above-mentioned polymer, a polymer including polyvinylidene fluoride (PVdF) can be used. In this case, the ionic conductivity and the thermal and electrochemical stability are improved, and a composite solid electrolyte that can fully absorb the liquid electrolyte described below and maintain a state of being immersed in the composite film can be obtained.

[0026] For the above-mentioned ion conductive ceramic and the above-mentioned polymer, the ratio of 60 to 100 parts by weight of the ion conductive ceramic to 1 to 40 parts by weight of the polymer can be adopted, and the ratio of 60 to 78 parts by weight of the ion conductive ceramic to 22 to 40 parts by weight of the polymer can be adopted, and the ratio of 95 to 85 parts by weight of the ion conductive ceramic to 5 to 15 parts by weight of the polymer can be adopted. When the above-mentioned ion conductive ceramic and the above-mentioned polymer are mixed in the above-mentioned weight parts, a sufficient amount of the ion conductive ceramic is dispersed in the composite film, and the binding effect due to the polymer or the effect that the liquid electrolyte applied later can be fully impregnated without leakage can be fully obtained, and at the same time, the excellent stability of the composite solid electrolyte and the high ion conductivity at room temperature can be obtained.

[0027] The ion conductive ceramic and the polymer are mixed with each other and molded into a mixture to be used as a composite film. At this time, if necessary, a suitable solvent can be added to the mixture (or mixture slurry) for mixing. For example, as the solvent, N-methyl-2-pyrrolidone (NMP): acetone (aceton) (1:3 vol) can be used, but it is not limited to this.

[0028] The above-mentioned composite film includes ion conductive ceramics and polymers, and thus acts as a solid electrolyte with excellent ion conductivity itself. However, in order to ensure better electrochemical performance of the battery, it is impregnated with a liquid electrolyte and used as a composite solid electrolyte in a state where the above-mentioned liquid electrolyte is absorbed in the composite film.

[0029] The liquid electrolyte contains a solution in which lithium ions or sodium ions are dissolved in a solvent. In this case, the lithium ions or sodium ions may be derived from a lithium salt or sodium salt suitable for a secondary battery, and any salt suitable for a secondary battery may be used.

[0030] The above-mentioned lithium salt is any one selected from the group consisting of LiClO4, LiPF6, LiBF4, CF3SO2NLiSO2CF3 (LiTFSI), LiB(C2O4)2, Li[N(SO2F)2](LiFSI), Li[B(C2O4)2], LiAsF6 and combinations thereof, and the above-mentioned sodium salt can be any one selected from the group consisting of NaClO4, NaBF4, NaPF4, NaPF6, NaAsF6, CF3SO2NNaSO2CF3 (NaTFSI), NaB(C2O4)2, Na[(C2F5)3PF3], Na[B(C2O4)2], Na[N(SO2F)2](NaFSI), NaN[SO2C2F5]2 and combinations thereof.

[0031] The above-mentioned solvent can be a non-aqueous organic solvent. The above-mentioned non-aqueous organic solvent can be any one selected from the group consisting of carbonates, esters, ethers, ketones, alcohols and combinations thereof. Aprotic solvents can also be used.

[0032] The above-mentioned solvent may be an ionic liquid, in which case, it has the advantage of being able to further improve the stability (especially thermal stability) of the electrolyte. Specifically, for the above-mentioned ionic liquid, imidazolium-based ionic liquids, pyridinium-based ionic liquids, pyrrolidinium-based ionic liquids, ammonium-based ionic liquids, and piperidinium-based ionic liquids can be used as solvents.

[0033] More specifically, the ionic liquid may include any one cation selected from the group consisting of imidazolium, pyridinium, pyrrolidinium, ammonium, piperidinium, and combinations thereof, and any one cation selected from the group consisting of BF4 - PF6 - 、AsF6 - 、SbF6 - 、AlCl4 - 、HSO4 - 、ClO4 - , Cl - Br - ,I - 、SO4 - CF3SO3 - CF3CO2 - 、(C2F5SO2)(CF3SO2)N - 、NO3 - 、Al2Cl7 - 、CH3COO - 、[N(SO2F)2] - 、CH3SO3 - Any anion selected from CF3SO3 and combinations thereof.

[0034] More specifically, the ionic liquid may be selected from N-methyl-N-butyl pyrrolidinium bis(trifluoromethylsulfonyl)imide, N-methyl-N-propylpyrrolidiniumbis(trifluoromethanesulfonyl)imide, N-butyl-N-methylpyrrolidium bis(3-trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide and 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide. Any one selected from the group consisting of bis(trifluoromethylsulfonyl)imide) and combinations thereof, in this case, the stability of the prepared composite solid electrolyte can be further improved.

[0035] The above-mentioned liquid electrolyte is suitable for the above-mentioned composite solid electrolyte in the form of lithium ions or sodium ions included in a solvent and absorbed in the composite film, which alleviates the high interface impedance of ion-conductive ceramics and compensates for the low ionic conductivity of polymers at room temperature. Since the liquid electrolyte is absorbed in the composite film containing the polymer, the problems of the liquid electrolyte itself, such as flammability and possibility of leakage, are almost not generated, so that an electrolyte with high thermal stability and low interface impedance can be prepared.

[0036] The liquid electrolyte may be a solution containing 0.1 M or more of a lithium salt or a sodium salt in a solvent, and may be a solution containing 0.1 M to 2 M of a lithium salt or a sodium salt.

[0037] The weight ratio of the composite film and the liquid electrolyte may be 60 to 100: 1 to 40, and the weight ratio may be 70 to 80: 10 to 20. If a large amount of the liquid electrolyte is added compared to the composite film, the liquid electrolyte may be wasted, and if the amount added is small, the effect of using the liquid electrolyte may not be obvious.

[0038] The thickness of the composite solid electrolyte can be less than 30 microns. The stability (especially thermal stability) of the composite solid electrolyte of the present invention is further improved, so that the thickness can be prepared to be less than 30 microns for use, and has stability suitable for secondary batteries.

[0039] Specifically, the composite solid electrolyte may also have excellent thermal stability at a temperature above 400°C.

[0040] Furthermore, the composite solid electrolyte has excellent electrochemical stability and has the characteristic of having electrochemical stability of 6V or more.

[0041] At the same time, the composite solid electrolyte significantly reduces the interface impedance, specifically, can have an interface impedance of less than 800Ω.

[0042] For the composite solid electrolyte of the present invention, i) ion (Li or Na) conductive ceramics improve ion conductivity and ion (Li or Na) transport rate, ii) polymers enable ceramic particles to achieve very good bonding, and iii) liquid electrolytes improve ion conductivity and reduce interface impedance between ceramic particles and between electrodes and electrolytes. The composite solid electrolyte manufactured in this way has excellent thermal and electrochemical stability due to ceramics and polymers, and a small amount of liquid electrolyte can improve the electrochemical characteristics of the secondary battery by reducing interface impedance.

[0043] A secondary battery according to another embodiment of the present invention includes an anode, a cathode, and the composite solid electrolyte located between the anode and the cathode.

[0044] As long as it is applicable to the anode or cathode of a lithium secondary battery or a sodium secondary battery, it can be applied to the above anode and the above cathode, so the detailed description is omitted. In addition, since the above composite solid electrolyte overlaps with the above description, its description is omitted.

[0045] Specifically, for lithium secondary batteries, LiFePO4 is used as the anode and Li metal is used as the cathode, and the composite solid electrolyte of the present invention can be used as the electrolyte. At this time, while having excellent thermal and electrochemical stability, the interface impedance is reduced, thereby obtaining a high capacity of more than 150 mAh / g.

[0046] Furthermore, for sodium secondary batteries, NaFePO4 is used as the anode and Na metal is used as the cathode. The composite solid electrolyte of the present invention can be used as the electrolyte. At this time, while having excellent thermal and electrochemical stability, the interface impedance is reduced, thereby obtaining an excellent discharge capacity of more than 135 mAh / g.

[0047] According to another embodiment of the present invention, a method for preparing a composite solid electrolyte includes: a step (1) of preparing a mixture slurry by mixing 60 to 100 parts by weight of an ion conductive ceramic and 1 to 40 parts by weight of a polymer; a step (2) of preparing a composite film by molding the mixture slurry into a film form; and a step (3) of preparing a composite solid electrolyte by absorbing a small amount of liquid electrolyte in the composite film.

[0048] The contents of the ion conductive ceramic, polymer, their mixing ratio, composite film, liquid electrolyte and its solvent, etc. are repeated in the above description, and thus the description thereof is omitted.

[0049] In the use of printing or blade coating After the mixture slurry is coated in a manner, a composite film can be prepared by a drying method. Any method that can prepare the slurry into a film form can be applied without particular limitation.

[0050] Regarding the liquid electrolyte used for absorption in the step (3), the solvent may include an ionic liquid. Since the specific type and content of the ionic liquid are the same as those described above, the description thereof is omitted.

[0051] Also, the absorption may be performed by providing the composite thin film and the liquid electrolyte at a weight ratio of 60 to 100:1 to 40, and detailed description of portions overlapping with the above description will be omitted.

[0052] Beneficial Effects

[0053] The composite solid electrolyte for secondary battery of the present invention and the preparation method thereof can provide a secondary battery with improved battery stability and electrochemical characteristics. The present invention can be prepared by a relatively simple method, and can be applied to lithium secondary battery or sodium secondary battery with excellent discharge capacity, low interface impedance and high stability, thereby improving the stability and electrochemical characteristics of the secondary battery at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 is a conceptual diagram of a composite solid electrolyte according to an embodiment of the present invention.

[0055] Figure 2 It is the scanning electron microscope-X-ray energy dispersive spectrometer (SEM-EDX) analysis data of the surface and cross-section of the composite solid electrolyte prepared in Example 1 and Example 2 of the present invention (upper side: lithium ion conductive electrolyte, lower side: sodium ion conductive electrolyte).

[0056] Figure 3This is the thermal stability evaluation result of the lithium ion conductive composite solid electrolyte prepared in Example 1 of the present invention [Thermogravimetric (TG) curve].

[0057] Figure 4 These are the results of evaluating the electrochemical stability of the lithium ion conductive composite solid electrolyte prepared in Example 1 of the present invention (LVS).

[0058] Figure 5 This is a graph confirming the interfacial impedance characteristics of a battery to which the lithium ion conductive composite solid electrolyte prepared in Example 1 of the present invention is applied.

[0059] Figure 6 1 is a charge-discharge curve when a secondary battery is constructed by the lithium ion conductive composite solid electrolyte prepared in Example 1 of the present invention and a LiFePO4 electrode.

[0060] Figure 7 is a charge-discharge curve of a sodium battery composed of the sodium ion conductive composite solid electrolyte prepared in Example 2 of the present invention and a NaFePO4 electrode.

[0061] Figure 8 This is a scanning electron microscope (SEM) photograph of the entire cross section of the lithium ion conductive composite solid electrolyte prepared in Example 3 of the present invention.

[0062] Fig. 9 The graph is a result of evaluating the thermal stability of the lithium ion conductive composite solid electrolyte (red) prepared in Example 3 of the present invention and the lithium ion conductive composite solid electrolyte (black) prepared in Example 1 (TG curve graph). DETAILED DESCRIPTION

[0063] Hereinafter, multiple embodiments of the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily implement the present invention. However, the present invention can be implemented in various different ways and is not limited to the embodiments described herein.

[0064] In the examples of the present invention, conductive ceramics, polymers, and liquid electrolytes were mixed and a composite solid electrolyte having excellent stability, good variability, and excellent electrochemical characteristics was prepared by the following method, and its physical properties were evaluated.

[0065] Preparation and performance evaluation of composite solid electrolytes and batteries

[0066] After preparing a mixture by mixing 70 parts by weight of conductive ceramic and 15 parts by weight of polymer in a solvent of N-methylpyrrolidone (NMP): acetone (aceton) (1:3 vol), the slurry is spread by printing or doctor blade coating, and a composite film is prepared by phase separation. 15 parts by weight of liquid electrolyte (or ionic liquid electrolyte) is absorbed in 85 parts by weight of the above composite film to prepare a Figure 1 A composite solid electrolyte of the morphology disclosed in the conceptual diagram.

[0067] Furthermore, in order to analyze the electrochemical characteristics of secondary batteries to which the prepared composite electrolytes were applied, interfacial impedance and charge-discharge tests were performed.

[0068] <Example 1>

[0069] 1) Preparation of lithium ion conductive composite solid electrolyte

[0070] The lithium conductive ceramic uses 70 parts by weight of Li 1.3 Al 0.3 Ti 1.7 (PO4)3(LTAP) porcelain, the polymer uses 15 parts by weight of polyvinylidene fluoride (PVdF). The liquid electrolyte is prepared by dissolving 1M LiPF6 in a mixed solvent of ethylene carbonate (EC) / dimethyl carbonate (DMC), and 15 parts by weight of the liquid electrolyte is used for every 85 parts by weight of the composite film to form a lithium ion conductive composite solid electrolyte.

[0071] 2) Physical property evaluation of lithium ion conductive composite solid electrolyte

[0072] Figure 2 are the SEM-EDX analysis data of the surface and cross section of the composite solid electrolyte prepared in the embodiment of the present invention, such as Figure 2 As shown, EDX confirmed that LTAPO and the polymer were uniformly mixed in the composite solid electrolyte prepared to a thickness of 30 microns (top: refer to the data of the lithium ion conductive electrolyte).

[0073] Figure 3 and Figure 4 The thermal stability evaluation results (TG curve graph) and electrochemical stability evaluation results (LSV) of the lithium ion conductive composite solid electrolyte are shown respectively.

[0074] The liquid electrolyte used as a comparative example decomposes at a temperature of 120 degrees (°C). Although the composite solid electrolyte has a slight weight loss due to the liquid electrolyte absorbed at a temperature of 180 degrees, it has a high thermal stability of over 400 degrees as a whole. Figure 4 The linear scanning method curve graph is used as an experiment to analyze the electrochemical stability of the electrolyte, and it can be confirmed that the composite solid electrolyte exhibits a high stability of more than 6V.

[0075] 3) Preparation and physical property evaluation of batteries using lithium ion conductive composite solid electrolytes

[0076] A secondary battery was prepared using LiFePO4 as the anode, Li metal with the lowest potential as the cathode, and the lithium ion conductive composite solid electrolyte prepared above as the electrolyte, and the physical properties were evaluated.

[0077] The interfacial impedance of the battery using the composite solid electrolyte was measured and the results are shown in Figure 5 When the composite solid electrolyte is used, it can be confirmed that a low resistance of 800Ω or less is exhibited.

[0078] The charge-discharge characteristics of the battery using the composite solid electrolyte are shown in Figure 1. Figure 6 Reference is made to the use of lithium ion conductive ceramics (Li 1.3 Al 0.3 Ti 1.7 The results of the battery composed of a composite solid electrolyte of (PO4)3) and a LiFePO4 anode Figure 6 , showing a high capacity of 150mAh / g.

[0079] <Example 2>

[0080] 1) Preparation and physical property evaluation of sodium ion conductive composite solid electrolyte

[0081] The sodium conductive ceramic is 70 parts by weight of Na3Zr2Si2PO 12 The polymer uses 15 parts by weight of polyvinylidene fluoride (PVdF), and the liquid electrolyte is prepared by dissolving 1M NaCF3SO3 (sodium triflate) in tetraethylene glycol dimethyl ether (TEGDME) solvent, and 15 parts by weight of the liquid electrolyte is applied to every 85 parts by weight of the composite film to form a sodium ion conductive composite solid electrolyte.

[0082] The thickness of the composite solid electrolyte is 30 μm, and EDX shows that the ceramic and polymer are uniformly mixed (refer to Figure 2 (photo below).

[0083] 2) Preparation and physical property evaluation of batteries using sodium ion conductive composite solid electrolytes

[0084] A secondary battery was prepared using NaFePO4 as the anode, Na metal as the cathode, and the sodium ion conductive composite solid electrolyte prepared above as the electrolyte, and the physical properties were evaluated.

[0085] The charge-discharge characteristics of the battery using the composite solid electrolyte are shown in Figure 1. Figure 7 Reference is made to the sodium conductive ceramic (Na3Zr2Si2PO 12 The result of using a composite solid electrolyte and NaFePO4 anode to form a sodium battery Figure 7 , showing an excellent discharge capacity of 135 mAh / g.

[0086] <Example 3>

[0087] 1) Preparation of lithium ion conductive composite solid electrolyte using ionic liquid electrolyte

[0088] The lithium conductive ceramic uses 70 parts by weight of Li 1.3 Al 0.3 Ti 1.7 (PO4)3(LTAP), the polymer is 15 parts by weight of polyvinylidene fluoride (PVdF). 1M lithium bis(fluorosulfonyl)imide (LiFSI) is dissolved in the ionic liquid N-methyl-N-butylpyrrolidinium bis(trifluoromethylsulfonyl)imide (Py 14 An ionic liquid electrolyte is prepared by mixing 15 parts by weight of the prepared ionic liquid electrolyte with 85 parts by weight of the composite film to form a lithium ion conductive composite solid electrolyte.

[0089] Figure 8 : is a SEM photograph of the entire cross section of the lithium ion conductive composite solid electrolyte prepared in Example 3 of the present invention. Figure 8 It can be confirmed that the prepared composite solid electrolyte is formed with a thickness of 30 μm or less, and the polymer and the conductive ceramic are fully mixed.

[0090] Fig. 9This is a TG curve diagram of the thermal stability of the composite solid electrolyte using an ionic liquid electrolyte as the liquid electrolyte according to Example 3. By comparing it with the composite solid electrolyte of Example 1 using a common liquid electrolyte, it can be confirmed that the composite solid electrolyte of Example 3 has better thermal stability (>400°C).

[0091] Although the preferred embodiments of the present invention have been described in detail above, the scope of the claims of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concepts of the present invention defined in the claims also fall within the scope of the claims of the present invention.

Claims

1. A composite solid electrolyte, It is characterized in that include: A composite film comprising 60 to 100 parts by weight of an ion conductive ceramic and 1 to 40 parts by weight of a polymer; as well as Liquid electrolyte, which contains a solution of lithium ions or sodium ions mixed with a non-aqueous organic solvent, The composite film and the liquid electrolyte are included in a weight ratio of 60 to 100:1 to 40, and the liquid electrolyte is impregnated in the composite film.

2. The composite solid electrolyte according to claim 1, It is characterized in that The ion conductive ceramic and the polymer are mixed in a solvent to prepare a mixture, the mixture is spread by a printing method or a doctor blade method, and the composite film is manufactured by a phase separation method.

3. The composite solid electrolyte according to claim 1, It is characterized in that The thickness of the composite solid electrolyte is less than 30 microns.

4. The composite solid electrolyte according to claim 1, It is characterized in that The polymer is any polymer selected from the group consisting of polyvinylidene fluoride polymers, polyvinylidene fluoride-trifluoroethylene copolymer polymers, polyethylene glycol polymers, polyacrylonitrile polymers, polymethyl methacrylate polymers, polyvinyl chloride polymers, polyvinyl pyrrolidone polymers, polyimide polymers, polyethylene polymers, polyurethane polymers, polypropylene polymers, polypropylene oxide polymers, polyethyleneimine polymers, polyethylene sulfide polymers, polyvinyl acetate polymers, polyethylene succinate polymers, polyester polymers, polyamine polymers, polysulfide polymers, silicon-based polymers and combinations thereof.

5. A secondary battery, It is characterized in that include: A composite solid electrolyte according to claim 1.

6. A method for preparing a composite solid electrolyte, It is characterized in that include: Step (1), preparing a mixture slurry by mixing 60 to 100 parts by weight of an ion conductive ceramic and 1 to 40 parts by weight of a polymer; Step (2), preparing a composite film by forming the mixture slurry into a film form; as well as Step (3) is to prepare a composite solid electrolyte by allowing the composite film to absorb a liquid electrolyte containing a solution mixed with lithium ions or sodium ions and a non-aqueous organic solvent so that the weight ratio of the composite film to the liquid electrolyte is 60 to 100:1 to 40.

7. A polymer electrolyte, It is characterized in that include: polymer; as well as a lithium ion or sodium ion liquid electrolyte contained in the polymer, Wherein, the weight ratio of the polymer to the liquid electrolyte is 1:2-20.

8. A polymer electrolyte, It is characterized in that include: A composite film comprising 60 to 75 parts by weight of an ion conductive ceramic and 100 to 400 parts by weight of a polymer; as well as Liquid electrolyte, which contains a solution of lithium ions or sodium ions mixed with a non-aqueous organic solvent, wherein the composite film and the liquid electrolyte are included in a weight ratio of 60 to 100:1 to 40, Furthermore, the liquid electrolyte is impregnated in the composite film.