Solid electrolyte based on dual-functional MOF three-dimensional nanofiber material and preparation method and application thereof

By using dual-functional MOF three-dimensional nanofiber materials to construct a three-dimensional network structure in lithium metal solid-state batteries, the problem of uneven lithium ion transmission and deposition is solved, the cycle stability and safety of the battery are improved, and high energy density and Improved safety performance.

CN119009102APending Publication Date: 2024-11-22HENGYANG NORMAL UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411294361.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The lithium metal solid-state batteries have unclear lithium ion transmission mechanisms, difficulty in building solid electrolyte structures, uneven deposition of lithium ions and uncontrollable growth of lithium dendrites, resulting in poor cycle stability and safety problems.

Method used

Using dual-functional metal organic frame (MOF) three-dimensional nanofiber material, the MOF material modified by open metal sites and functional groups is formed by in-situ growth, a three-dimensional network structure is constructed, lithium salts and polymers are filled to form high ionic conductivity and mechanical Solid-state electrolyte with excellent performance.

Benefits of technology

It realizes continuous and rapid transmission of lithium ions, improves the cycle stability and safety of the battery, inhibits the growth of lithium dendrites, and improves energy density and safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009102A_ABST
    Figure CN119009102A_ABST
Patent Text Reader

Abstract

The invention provides a solid electrolyte based on a bifunctional MOF (Metal Organic Framework) three-dimensional nanofiber material, which is obtained by filling a lithium salt and a polymer after bifunctional MOF grows on the surface of the three-dimensional nanofiber material in situ, wherein the bifunctional MOF is composed of a metal salt and an organic ligand material, the metal salt provides an open metal site, and the organic ligand material provides functional group modification. The MOF material modified by open metal sites and organic ligand functional groups grows on a three-dimensional network structure in situ in an in-situ growth mode, dissociation of lithium salt can be enhanced, continuous and uniform transmission of lithium ions to a negative electrode is promoted, uniform deposition of the lithium ions is promoted, and the electrochemical cycle stability of the battery is improved. In addition, the polymer / lithium salt is filled into the bifunctional MOF three-dimensional network structure, so that the solid electrolyte with high ionic conductivity, good mechanical property, low interface impedance, high magnification and stable long circulation is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid electrolytes, and in particular to a solid electrolyte based on a dual-functional MOF three-dimensional nanofiber material and a preparation method and application thereof. Background Art

[0002] Since Sony first launched commercial lithium-ion batteries (LIBs), they have been widely used in various portable electronic products such as laptops and mobile phones. However, with the rapid development of society, higher requirements have been placed on the energy density and safety of energy storage devices. At present, the energy density of the most advanced lithium-ion batteries assembled with ternary high-nickel positive electrode (NCM811) and graphite negative electrode is difficult to exceed 300Wh / kg.

[0003] As a high-energy-density, high-safety secondary battery system, lithium metal solid-state batteries have a theoretical capacity of up to 3860mAh / g and a minimum potential (-3.04V vs. SHE). At the same time, the non-flammability and high Young's modulus of solid electrolytes make them the next generation energy storage system with the most development and application prospects. However, in the practical application of lithium metal solid-state batteries, they still face severe challenges: ① The transmission mechanism of lithium ions between electrodes / solid electrolytes is still unclear; ② How to construct a solid electrolyte structure with the function of fast lithium ion transmission; ③ The uneven deposition of lithium ions and the uncontrollable growth of lithium dendrites lead to poor cycle stability of the battery, causing serious safety issues.

[0004] Based on this, it is urgent to propose a technical solution to solve the above-mentioned problems. Summary of the invention

[0005] In view of the above problems, the present invention provides a solid electrolyte based on a dual-functional metal organic framework (MOF) three-dimensional nanofiber material and its preparation method and application. The present invention grows a MOF material with open metal sites and modified organic ligand functional groups on a three-dimensional nanofiber material in situ through an in-situ growth method to form a three-dimensional continuous lithium ion fast transmission channel, and further fills the polymer / lithium salt into the dual-functional MOF three-dimensional nanofiber material to prepare a solid electrolyte with high ion conductivity, good mechanical properties, low interface impedance, high rate and long cycle stability.

[0006] The present invention first designs and prepares a dual-functional MOF from the molecular structure level, anchors anions (open metal sites) and improves electrochemical stability (halogen functional groups); secondly, a three-dimensional network structure (three-dimensional nanofiber material) with high mechanical strength, high antioxidant potential and cation superconductivity is constructed from the structural design, and is committed to providing a solid electrolyte with excellent performance. Among them, the MOF open metal site can bind lithium salt anions and improve lithium ion transmission; functional group modification can regulate the charge distribution inside the MOF pores, promote lithium ion transmission, and achieve high ionic conductivity. At the same time, MOF forms a continuous three-dimensional network structure on the three-dimensional nanofiber material, which can enhance the dissociation of lithium salts, promote the continuous and uniform transmission of lithium ions to the negative electrode, promote the uniform deposition of lithium ions, and improve the electrochemical cycle stability of the battery; in addition, the three-dimensional network structure is highly interconnected, which can enhance the mechanical strength of the electrolyte, improve the antioxidant potential and improve the safety of lithium metal solid-state batteries.

[0007] The solid electrolyte of the present invention can provide a continuous and fast transmission channel for lithium ions under the synergistic effect of open metal sites, functional group modification and highly interconnected three-dimensional network structure of MOFs, thereby realizing lithium ion superconductivity. At the same time, the selection of three-dimensional network fiber materials with high mechanical strength and high oxidation potential can not only effectively inhibit the growth of lithium dendrites and improve battery safety, but also match high-voltage positive electrode materials to improve battery energy density.

[0008] The term "open metal site" of the present invention means that the site where the metal cation coordination is unsaturated in MOF is called an open metal site. The unsaturated metal cation can combine with the lithium salt anion to limit the transmission of the anion and improve the mobility of the lithium ion.

[0009] One object of the present invention is to provide a solid electrolyte based on a bifunctional MOF three-dimensional nanofiber material, wherein the solid electrolyte based on a bifunctional MOF three-dimensional nanofiber material is obtained by in-situ growth of a bifunctional MOF on the surface of the three-dimensional nanofiber material and then filling lithium salt and polymer;

[0010] in,

[0011] The bifunctional MOF is composed of metal salt and organic ligand material.

[0012] The metal salt provides an open metal site,

[0013] The organic ligand material provides functional group modification.

[0014] Furthermore, the metal salt is selected from one or more salts composed of cerium ions, zirconium ions, manganese ions, nickel ions, cobalt ions, copper ions, aluminum ions or zinc ions.

[0015] Furthermore, the functional group of the organic ligand material is selected from one or more of -F, -Cl, -Br, -I, -SO3Li, -NH2 or -NO2.

[0016] Furthermore, the bifunctional MOF is selected from one or more of Ce-UIO-66-4F, Ce-UIO-66-4Cl, Ce-UIO-66-4Br, Ce-UIO-66-SO3Li, Ce-UIO-66-NH2, and Ce-UIO-66-NO2.

[0017] Furthermore, the three-dimensional nanofiber material is selected from one or more of polyacrylonitrile (PAN), polyimide (PI), polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PA) or bacterial cellulose (BC).

[0018] Furthermore, the lithium salt is selected from one or more of lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium difluorooxalatoborate (LiODFB), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4) or lithium perchlorate (LiClO4).

[0019] Furthermore, the polymer is selected from one or more of polyethylene oxide (PEO), polyacrylonitrile, polycarbonate (PC), polyvinylidene fluoride (PVDF) or polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP).

[0020] Furthermore, the mass ratio of the lithium salt to the polymer is (0.5-5):1.

[0021] Another object of the present invention is to provide a method for preparing the above-mentioned solid electrolyte based on the bifunctional MOF three-dimensional nanofiber material, wherein the method for preparing the solid electrolyte based on the bifunctional MOF three-dimensional nanofiber material comprises the following steps:

[0022] S1. Add metal salt and organic ligand material to a solvent, and stir ultrasonically to obtain a mixed solution; then add a three-dimensional nanofiber material treated with ozone plasma, synthesize a bifunctional MOF three-dimensional network structure by a hydrothermal method, purify, and dry to obtain a bifunctional MOF three-dimensional nanofiber material;

[0023] S2. Blend a lithium salt, a polymer and an organic solvent, stir to obtain a lithium salt-polymer solution; apply the lithium salt-polymer solution on a substrate, then place the bifunctional MOF three-dimensional nanofiber material, and then apply the lithium salt-polymer solution, and use negative pressure to assist filling so that the lithium salt-polymer solution is fully filled into the bifunctional MOF three-dimensional nanofiber material, dry, and obtain a solid electrolyte based on the bifunctional MOF three-dimensional nanofiber material.

[0024] Furthermore, in step S1, the reaction temperature of the hydrothermal method is 100-120° C., and the reaction time is 10-40 h.

[0025] Another object of the present invention is to provide application of the above-mentioned solid electrolyte based on bifunctional MOF three-dimensional nanofiber material in the field of lithium batteries.

[0026] Furthermore, the application in the field of lithium batteries is application in lithium metal negative electrode secondary batteries.

[0027] The present invention has the following beneficial effects:

[0028] (1) The preparation method of the solid electrolyte based on the dual-functional MOF three-dimensional nanofiber material of the present invention is to design and synthesize a MOF material with open metal sites and functional group modification. X=F, Cl, Br, I) has a suitable pore size, which can effectively bind lithium salt anions and limit the transmission of lithium salt anions; and the open metal sites of Ce-UIO-66 combine with lithium salt anions through Lewis acid-base interaction, further limiting the transmission of lithium salt anions and increasing the number of lithium ion migration. At the same time, the present invention prepares Ce-UIO-66-X (X=F, Cl, Br, I) by modifying the functional groups of organic ligands and grafting halogens on the organic ligands. Halogen modification can adjust the electron distribution in the channel, promote ion transmission, and achieve high ionic conductivity. In addition, MOF materials have an ordered pore structure, which can promote the uniform deposition of lithium ions and improve the electrochemical cycle stability of the battery.

[0029] (2) The present invention designs a composite solid electrolyte with high mechanical strength, high antioxidant potential and fast lithium ion transmission channel from the perspective of structural design. The present invention selects polyimide (PI) with high mechanical strength and high antioxidant potential. The high mechanical strength can effectively inhibit the growth of lithium dendrites and improve the safety performance of the battery; at the same time, the high antioxidant potential of PI can match high-voltage positive electrode materials and improve the energy density of the battery; in addition, by in-situ growing tightly connected Ce-UIO-66-X materials on PI three-dimensional network fibers, a continuous and fast transmission channel is provided for lithium ions from the perspective of the structural design of the solid electrolyte, thereby greatly improving the ionic conductivity of the solid electrolyte at room temperature, the lithium ion migration number and the battery cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The scanning electron microscope image of the dual-functionalized MOF in Example 1 is shown.

[0031] Figure 2 The powder diffraction pattern of the dual-functionalized MOF in Example 1 is shown.

[0032] Figure 3 The scanning electron microscope image of the dual-functional MOF on the three-dimensional nanofiber material in Example 1 is shown.

[0033] Figure 4 A scanning electron microscope image of the solid electrolyte based on the dual-functional MOF three-dimensional nanofiber material in Example 1 is shown.

[0034] Figure 5 A schematic diagram of the preparation of a solid electrolyte based on a dual-functional MOF three-dimensional nanofiber material of the present invention is shown.

[0035] Figure 6 The Li||Li symmetric battery based on the solid electrolyte of the bifunctional MOF three-dimensional nanofiber material in Example 1 is shown at a current density of 0.5 mA / cm 2 、0.5mAh / cm 2 , long cycle performance diagram at 30℃.

[0036] Figure 7 A comparison chart of the cycling performance of the NCM111||Li battery assembled with a solid electrolyte based on a bifunctional MOF three-dimensional nanofiber material in Example 1 at a current density of 0.5C and 30°C is shown. DETAILED DESCRIPTION

[0037] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0038] Unless otherwise stated, the raw materials, reactions and post-treatment methods mentioned in the examples are common raw materials on the market and technical methods well known to those skilled in the art.

[0039] The PI in the examples and comparative examples of the present invention is PI80, which was purchased from Jiangxi Xiancai Nanofiber Technology Co., Ltd.

[0040] The molecular weight of PVDF-HFP in the examples and comparative examples of the present invention is 500,000 and is purchased from Clamart Reagent Company.

[0041] The PVDF in the test example of the present invention is polyvinylidene fluoride, with a molecular weight of 600,000, purchased from Clamart Reagent Company.

[0042] The NMP of the present invention is N-methylpyrrolidone, which is purchased from Tianjin Zhiyuan Chemical Reagent Co., Ltd.

[0043] Example 1

[0044] A solid electrolyte based on a dual-functional MOF three-dimensional nanofiber material, wherein the solid electrolyte based on the dual-functional MOF three-dimensional nanofiber material is obtained by in-situ growth of the dual-functional MOF on the surface of a PI membrane and filling LiTFSI and PVDF-HFP;

[0045] in,

[0046] The bifunctional MOF is composed of ammonium cerium nitrate and tetrafluoroterephthalic acid.

[0047] The ammonium cerium nitrate provides an open metal site,

[0048] The tetrafluoroterephthalic acid provides functional group modification.

[0049] The preparation method of the solid electrolyte based on the bifunctional MOF three-dimensional nanofiber material comprises the following steps:

[0050] S1. Add 548 mg of ammonium cerium nitrate and 476 mg of tetrafluoroterephthalic acid to a mixture of 3 ml of acetic acid and 45 ml of deionized water, stir ultrasonically, and add to a reactor after dissolution to obtain a mixed solution; cut the PI film irradiated with ozone plasma into 4×4 cm 2The size was placed in the reactor and reacted at 110°C for 13h to obtain a dual-functional MOF three-dimensional network structure, and then the PI membrane was taken out, washed three times with deionized water and anhydrous ethanol respectively, and vacuum dried at 120°C for 24h to obtain an open metal site and halogen functional group dual-functional MOF three-dimensional nanofiber material (Ce-UIO-66-4F / PI);

[0051] S2. Blend PVDF-HFP, LiTFSI and NMP (m / m / m=1:2:25), stir at room temperature for 24 hours to obtain a PVDF-HFP / LiTFSI solution; use a 200μm scraper to coat a layer of PVDF-HFP / LiTFSI solution on a glass plate, stick the Ce-UIO-66-4F / PI thereon, then use a 400μm scraper to coat a layer of PVDF-HFP / LiTFSI solution, and use negative pressure to assist filling multiple times to ensure that the PVDF-HFP / LiTFSI solution is fully filled into the Ce-UIO-66-4F / PI skeleton; place the glass plate at 80°C for vacuum drying for 24 hours, then tear off the membrane and put it into a glove box, and dry it at 60°C for 24 hours, then dry it for 3 days, cut it into a circular membrane with a diameter of 16 mm, and obtain a solid electrolyte (Ce-UIO-66-4F / PI / PVDF-HFP) based on a dual-functional MOF three-dimensional nanofiber material.

[0052] Figure 1 The scanning electron microscope image of the dual-functionalized MOF (ie, Ce-UIO-66-4F) in Example 1 is shown.

[0053] Figure 2 The powder diffraction pattern of the dual-functionalized MOF in Example 1 is shown; Figure 2 It can be seen that the bifunctionalized MOF has an octahedral crystal structure, indicating that the modification of the open metal sites and organic ligand functional groups did not change the crystal structure of the material.

[0054] Figure 3 The scanning electron microscope image of the dual-functional MOF on the three-dimensional nanofiber material in Example 1 is shown.

[0055] Figure 4 A scanning electron microscope image of the solid electrolyte based on the dual-functional MOF three-dimensional nanofiber material in Example 1 is shown.

[0056] Figure 5 A schematic diagram of the preparation of a solid electrolyte based on a dual-functional MOF three-dimensional nanofiber material of the present invention is shown.

[0057] Depend on Figure 5It can be seen that the in situ growth technology evenly distributes the bifunctional MOF material with open metal sites and functional group modifications on the polymer fibers to construct a three-dimensional network support, forming a bifunctional three-dimensional continuous lithium ion rapid transmission channel with cation superconductivity and anion anchoring, and further fills the polymer / lithium salt into the bifunctional MOF three-dimensional support structure to prepare a solid electrolyte with high ionic conductivity, good mechanical properties and low interface impedance.

[0058] Example 2

[0059] A solid electrolyte based on a dual-functional MOF three-dimensional nanofiber material, wherein the solid electrolyte based on the dual-functional MOF three-dimensional nanofiber material is obtained by in-situ growth of the dual-functional MOF on the surface of a PI membrane and filling LiTFSI and PVDF-HFP;

[0060] in,

[0061] The bifunctional MOF is composed of ammonium cerium nitrate and tetrachloroterephthalic acid.

[0062] The ammonium cerium nitrate provides an open metal site,

[0063] The tetrachloroterephthalic acid provides functional group modification.

[0064] The preparation method of the solid electrolyte based on the bifunctional MOF three-dimensional nanofiber material comprises the following steps:

[0065] S1. Add 548 mg of ammonium cerium nitrate and 604 mg of tetrachloroterephthalic acid to a mixture of 3 ml of acetic acid and 45 ml of deionized water, stir ultrasonically, and add to a reactor to obtain a mixed solution after dissolution; cut the PI film irradiated with ozone plasma into 4×4 cm 2 The size was placed in the reactor and reacted at 110°C for 13h to obtain a dual-functional MOF three-dimensional network structure, and then the PI membrane was taken out, washed three times with deionized water and anhydrous ethanol respectively, and vacuum dried at 120°C for 24h to obtain an open metal site and halogen functional group dual-functional MOF three-dimensional nanofiber material (Ce-UIO-66-4Cl / PI);

[0066] S2. PVDF-HFP, LiTFSI and NMP are mixed (m / m / m=1:2:25), stirred at room temperature for 24 hours to obtain a PVDF-HFP / LiTFSI solution; a layer of PVDF-HFP / LiTFSI solution is coated on a glass plate with a 200 μm scraper, the Ce-UIO-66-4Cl / PI is attached thereto, and then a layer of PVDF-HFP / LiTFSI solution is coated with a 400 μm scraper, and negative pressure is used for multiple auxiliary fillings to fully fill the PVDF-HFP / LiTFSI solution into the Ce-UIO-66-4Cl / PI skeleton; the glass plate is placed in a vacuum dryer at 80°C for 24 hours, and then the membrane is torn off and placed in a glove box, and dried at 60°C for 24 hours, followed by drying for 3 days, and cut into a circular membrane with a diameter of 16 mm to obtain a solid electrolyte (Ce-UIO-66-4Cl / PI / PVDF-HFP) based on a dual-functional MOF three-dimensional nanofiber material.

[0067] Example 3

[0068] A solid electrolyte based on a dual-functional MOF three-dimensional nanofiber material, wherein the solid electrolyte based on the dual-functional MOF three-dimensional nanofiber material is obtained by in-situ growth of the dual-functional MOF on the surface of a PI membrane and filling LiTFSI and PVDF-HFP;

[0069] in,

[0070] The bifunctional MOF is composed of ammonium cerium nitrate and tetrabromoterephthalic acid.

[0071] The ammonium cerium nitrate provides an open metal site,

[0072] The tetrabromoterephthalic acid provides functional group modification.

[0073] The preparation method of the solid electrolyte based on the bifunctional MOF three-dimensional nanofiber material comprises the following steps:

[0074] S1. Add 548 mg of ammonium cerium nitrate and 963 mg of tetrabromoterephthalic acid to a mixture of 3 ml of acetic acid and 45 ml of deionized water, stir ultrasonically, and add to a reactor after dissolution to obtain a mixed solution; cut the PI film irradiated with ozone plasma into 4×4 cm 2 The size was placed in the reactor and reacted at 110°C for 13h to obtain a dual-functional MOF three-dimensional network structure, and then the PI membrane was taken out, washed three times with deionized water and anhydrous ethanol respectively, and vacuum dried at 120°C for 24h to obtain an open metal site and halogen functional group dual-functional MOF three-dimensional nanofiber material (Ce-UIO-66-4Br / PI);

[0075] S2. Blend PVDF-HFP, LiTFSI and NMP (m / m / m=1:2:25), stir at room temperature for 24 hours to obtain a PVDF-HFP / LiTFSI solution; use a 200μm scraper to coat a layer of PVDF-HFP / LiTFSI solution on a glass plate, stick the Ce-UIO-66-4Br / PI thereon, then use a 400μm scraper to coat a layer of PVDF-HFP / LiTFSI solution, and use negative pressure to assist filling multiple times to ensure that the PVDF-HFP / LiTFSI solution is fully filled into the Ce-UIO-66-4Br / PI skeleton; place the glass plate at 80°C for vacuum drying for 24 hours, then tear off the membrane and put it into a glove box, and dry it at 60°C for 24 hours, then dry it for 3 days, cut it into a circular membrane with a diameter of 16 mm, and obtain a solid electrolyte (Ce-UIO-66-4Br / PI / PVDF-HFP) based on a dual-functional MOF three-dimensional nanofiber material.

[0076] Example 4

[0077] A solid electrolyte based on a dual-functional MOF three-dimensional nanofiber material, wherein the solid electrolyte based on the dual-functional MOF three-dimensional nanofiber material is obtained by in-situ growth of the dual-functional MOF on the surface of a PI membrane and filling LiTFSI and PVDF-HFP;

[0078] in,

[0079] The bifunctional MOF is composed of ammonium cerium nitrate and tetraiodoterephthalic acid.

[0080] The ammonium cerium nitrate provides an open metal site,

[0081] The tetraiodoterephthalic acid provides functional group modification.

[0082] S1. Add 548 mg of ammonium cerium nitrate and 1.35 g of tetraiodoterephthalic acid to a mixture of 3 ml of acetic acid and 45 ml of deionized water, stir ultrasonically, and add to a reactor to obtain a mixed solution after dissolution; cut the PI film irradiated with ozone plasma into 4×4 cm 2 The size was placed in the reactor and reacted at 110°C for 13h to obtain a dual-functional MOF three-dimensional network structure, and then the PI membrane was taken out, washed three times with deionized water and anhydrous ethanol respectively, and vacuum dried at 120°C for 24h to obtain an open metal site and halogen functional group dual-functional MOF three-dimensional nanofiber material (Ce-UIO-66-4I / PI);

[0083] S2. PVDF-HFP, LiTFSI and NMP were mixed (m / m / m=1:2:25), stirred at room temperature for 24 hours to obtain a PVDF-HFP / LiTFSI solution; a layer of PVDF-HFP / LiTFSI solution was coated on a glass plate with a 200 μm scraper, the Ce-UIO-66-4I / PI was attached thereto, and then a layer of PVDF-HFP / LiTFSI solution was coated with a 400 μm scraper, and negative pressure was used for multiple auxiliary fillings to fully fill the PVDF-HFP / LiTFSI solution into the Ce-UIO-66-4I / PI skeleton; the glass plate was placed in a vacuum dryer at 80°C for 24 hours, and then the film was torn off and placed in a glove box, and dried at 60°C for 24 hours, followed by drying for 3 days, and cut into a circular film with a diameter of 16 mm, thereby obtaining a solid electrolyte (Ce-UIO-66-4I / PI / PVDF-HFP) based on a dual-functional MOF three-dimensional nanofiber material.

[0084] Example 5

[0085] A solid electrolyte based on a dual-functional MOF three-dimensional nanofiber material, wherein the solid electrolyte based on the dual-functional MOF three-dimensional nanofiber material is obtained by in-situ growth of the dual-functional MOF on the surface of a PI membrane and filling LiTFSI and PVDF-HFP;

[0086] in,

[0087] The bifunctional MOF is composed of ammonium cerium nitrate and monosodium disulfonate terephthalate.

[0088] The ammonium cerium nitrate provides an open metal site,

[0089] The monosodium disulfonate terephthalate salt provides functional group modification.

[0090] The preparation method of the solid electrolyte based on the bifunctional MOF three-dimensional nanofiber material comprises the following steps:

[0091] S1. Add 1.88 g of ammonium cerium nitrate and 0.90 g of monosodium disulfonate terephthalate to a mixture of 10 ml of acetic acid and 90 ml of DMF, stir ultrasonically, and add to a reactor to obtain a mixed solution after dissolution; cut the PI film irradiated with ozone plasma into 4×4 cm 2size, placed in the reactor, reacted at 120°C for 40h to obtain a dual-functional MOF three-dimensional network structure, then took out the PI membrane, washed it three times with DMF and anhydrous ethanol respectively, and dried it at 120°C in vacuum for 24h to obtain Ce-UIO-66-SO3Na / PI; immersed the Ce-UIO-66-SO3Na / PI in 1mol / L LiOH for 72h to obtain an open metal site and a single lithium ion conductor dual-functional MOF three-dimensional nanofiber material (Ce-UIO-66-SO3Li / PI);

[0092] S2. Blend PVDF-HFP, LiTFSI and NMP (m / m / m=1:2:25), stir at room temperature for 24 hours to obtain a PVDF-HFP / LiTFSI solution; use a 200μm scraper to coat a layer of PVDF-HFP / LiTFSI solution on a glass plate, stick the Ce-UIO-66-SO3Li / PI thereon, then use a 400μm scraper to coat a layer of PVDF-HFP / LiTFSI solution, and use negative pressure to assist filling multiple times to ensure that the PVDF-HFP / LiTFSI solution is fully filled into the Ce-UIO-66-SO3Li / PI skeleton; place the glass plate at 80°C for vacuum drying for 24 hours, then tear off the membrane and put it into a glove box, and dry it at 60°C for 24 hours, then dry it for 3 days, cut it into a circular membrane with a diameter of 16 mm, and obtain a solid electrolyte (Ce-UIO-66-SO3Li / PI / PVDF-HFP) based on a dual-functional MOF three-dimensional nanofiber material.

[0093] Example 6

[0094] A solid electrolyte based on a dual-functional MOF three-dimensional nanofiber material, wherein the solid electrolyte based on the dual-functional MOF three-dimensional nanofiber material is obtained by in-situ growth of the dual-functional MOF on the surface of a PI membrane and filling LiTFSI and PVDF-HFP;

[0095] in,

[0096] The bifunctional MOF is composed of ammonium cerium nitrate and 2-aminoterephthalic acid.

[0097] The ammonium cerium nitrate provides an open metal site,

[0098] The 2-aminoterephthalic acid provides functional group modification.

[0099] The preparation method of the solid electrolyte based on the bifunctional MOF three-dimensional nanofiber material comprises the following steps:

[0100] S1. Add 0.548 g of ammonium cerium nitrate and 0.181 g of 2-aminoterephthalic acid into a mixture of 27 ml of deionized water and 18 ml of acetic acid, stir ultrasonically, and add to a reactor to obtain a mixed solution after dissolution; cut the PI film irradiated with ozone plasma into 4×4 cm 2 The size was placed in the reactor and reacted at 100°C for 24 hours to obtain a dual-functional MOF three-dimensional network structure, and then the PI membrane was taken out, washed three times with anhydrous ethanol, and vacuum dried at 120°C for 24 hours to obtain an open metal site and amino functional group dual-functional MOF three-dimensional nanofiber material (Ce-UIO-66-NH2 / PI);

[0101] S2. Blend PVDF-HFP, LiTFSI and NMP (m / m / m=1:2:25), stir at room temperature for 24 hours to obtain a PVDF-HFP / LiTFSI solution; use a 200μm scraper to scrape a layer of PVDF-HFP / LiTFSI solution on a glass plate, stick the Ce-UIO-66-NH2 / PI / PI on it, and then use a 400μm scraper to scrape a layer of PVDF-HFP / LiTFSI solution, and use negative pressure to assist filling multiple times to make the PVDF-HFP / LiTFSI solution fully fill into the Ce-UIO-66-NH2 / PI skeleton; place the glass plate at 80℃ for vacuum drying for 24 hours, then tear off the membrane and put it into a glove box, and dry it at 60℃ for 24 hours, then dry it for 3 days, cut it into a circular membrane with a diameter of 16mm, and obtain a solid electrolyte (Ce-UIO-66-NH2 / PI / PVDF-HFP) based on dual-functional MOF three-dimensional nanofiber material.

[0102] Test Case

[0103] The solid electrolyte (Ce-UIO-66-4F / PI / PVDF-HFP) based on the bifunctional MOF three-dimensional nanofiber material prepared in Example 1 was assembled into Li||Li symmetric batteries and Li|NCM111 batteries, and their various battery performances were tested.

[0104] Test method:

[0105] Li||Li symmetric battery test: In a glove box, lithium metal sheets were used as the positive and negative electrodes, and Ce-UIO-66-4F / PI / PVDF-HFP was used as the solid electrolyte membrane to assemble a lithium-lithium symmetric battery. The data was tested at 30°C using an electrochemical testing system.

[0106] Li||NCM111 battery test: NCM111 was mixed with Li400 and PVDF (m / m / m=80:12:8), and dispersed with N-methylpyrrolidone (NMP) solvent to prepare a slurry, which was coated on aluminum foil and dried in a vacuum oven at 60°C for 24 h; then it was cut into electrode discs with a diameter of 12 mm using a slicer, and prepared with scrapers of different thicknesses of 100 μm to form a slurry with a loading of 2 mg / cm 2 In a glove box, a CR-2032 button cell was assembled with the prepared electrode as the positive electrode, the lithium sheet as the negative electrode, and Ce-UIO-66-4F / PI / PVDF-HFP solid electrolyte, and the data was tested at 30°C using an electrochemical test system.

[0107] Figure 6 The Li||Li symmetric battery based on the solid electrolyte of the bifunctional MOF three-dimensional nanofiber material in Example 1 is shown at a current density of 0.5 mA / cm 2 、0.5mAh / cm 2 , long cycle performance diagram at 30℃.

[0108] Depend on Figure 6 It can be seen that the ionic conductivity of the composite solid electrolyte of the present invention at 30°C reaches 1.81×10 - 3 S / m 2 ; and Ce-UIO-66-4F / PI / PVDF-HFP at 0.5mA / cm 2 It can still cycle stably for 1000 h at a high current density, and the polarization is stable below 50 mV, indicating that the solid electrolyte supported by the Ce-UIO-66-4F / PI / PVDF-HFP dual-functional three-dimensional network can greatly improve the interface compatibility and effectively inhibit lithium dendrites, thereby protecting the lithium negative electrode.

[0109] Figure 7 A comparison chart of the cycling performance of the NCM111||Li battery assembled with a solid electrolyte based on a bifunctional MOF three-dimensional nanofiber material in Example 1 at a current density of 0.5C and 30°C is shown.

[0110] Depend on Figure 7 It can be seen that the performance of the composite solid electrolyte based on MOF three-dimensional network support of the present invention is much higher than that of pure PI / PVDF-HFP solid electrolyte, indicating that the battery using solid electrolyte supported by Ce-UIO-66-4F / PI / PVDF-HFP three-dimensional network has very good cycle stability, and the capacity retention rate exceeds 91% after 300 cycles at 0.5C battery density.

[0111] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0112] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A solid electrolyte based on dual-functional MOF three-dimensional nanofiber materials, It is characterized in that The solid electrolyte based on the bifunctional MOF three-dimensional nanofiber material is obtained by in-situ growth of the bifunctional MOF on the surface of the three-dimensional nanofiber material and then filling it with lithium salt and polymer; in, The bifunctional MOF is composed of metal salt and organic ligand material. The metal salt provides an open metal site, The organic ligand material provides functional group modification.

2. The solid electrolyte based on bifunctional MOF three-dimensional nanofiber material according to claim 1, It is characterized in that The metal salt is selected from one or more salts composed of cerium ion, zirconium ion, manganese ion, nickel ion, cobalt ion, copper ion, aluminum ion or zinc ion.

3. The solid electrolyte based on bifunctional MOF three-dimensional nanofiber material according to claim 1, It is characterized in that The functional group of the organic ligand material is selected from -F, -Cl, -Br, -I, -SO 3 Li, -NH 2 or-NO 2 One or more of .

4. The solid electrolyte based on bifunctional MOF three-dimensional nanofiber material according to claim 1, It is characterized in that The three-dimensional nanofiber material is selected from one or more of polyacrylonitrile, polyimide, polyvinyl pyrrolidone, polyvinyl alcohol or bacterial cellulose.

5. The solid electrolyte based on bifunctional MOF three-dimensional nanofiber material according to claim 1, It is characterized in that The lithium salt is selected from one or more of bis(fluorosulfonyl)imide lithium salt, bis(trifluoromethanesulfonyl)imide lithium salt, difluorooxalatoborate lithium salt, lithium hexafluorophosphate, lithium tetrafluoroborate or lithium perchlorate.

6. The solid electrolyte based on bifunctional MOF three-dimensional nanofiber material according to claim 1, It is characterized in that The polymer is selected from one or more of polyethylene oxide, polyacrylonitrile, polycarbonate, polyvinylidene fluoride or polyvinylidene fluoride-hexafluoropropylene.

7. The solid electrolyte based on bifunctional MOF three-dimensional nanofiber material according to claim 1, It is characterized in that The mass ratio of the lithium salt to the polymer is (0.5-5):

1.

8. The method for preparing a solid electrolyte based on a dual-functional MOF three-dimensional nanofiber material according to any one of claims 1 to 7, It is characterized in that The preparation method of the solid electrolyte based on the dual-functional MOF three-dimensional nanofiber material comprises the following steps: S1. Add metal salt and organic ligand material to a solvent, and stir ultrasonically to obtain a mixed solution; then add a three-dimensional nanofiber material treated with ozone plasma, synthesize a bifunctional MOF three-dimensional network structure by a hydrothermal method, purify, and dry to obtain a bifunctional MOF three-dimensional nanofiber material; S2. Blend a lithium salt, a polymer and an organic solvent, stir to obtain a lithium salt-polymer solution; apply the lithium salt-polymer solution on a substrate, then place the bifunctional MOF three-dimensional nanofiber material, and then apply the lithium salt-polymer solution, and use negative pressure to assist filling so that the lithium salt-polymer solution is fully filled into the bifunctional MOF three-dimensional nanofiber material, dry, and obtain a solid electrolyte based on the bifunctional MOF three-dimensional nanofiber material.

9. The method for preparing a solid electrolyte based on a dual-functional MOF three-dimensional nanofiber material according to claim 8, It is characterized in that In step S1, the reaction temperature of the hydrothermal method is 100-120° C., and the reaction time is 10-40 h.

10. Application of the solid electrolyte based on bifunctional MOF three-dimensional nanofiber material according to any one of claims 1 to 7 in the field of lithium batteries.

Citation Information

Cited By

  • Composite electrolyte taking ZIF-8 coated cellulose membrane as skeleton and preparation method thereof

    CN119601765A

  • Cerium-doped modified MOFs-based composite solid electrolyte and preparation method and application thereof

    CN122455903A