Electrolyte and battery comprising same

By using a specific proportion of acrylate polymer and lithium difluorosulfonimide in lithium-ion battery electrolyte, the insufficient performance of the electrolyte under high and low temperature conditions is solved, and the safety of the battery is improved and the dissolution properties of lithium salts.

CN119009135APending Publication Date: 2024-11-22ZHUHAI COSMX BATTERY CO LTD

Patent Information

Application Number
CN202411130918.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing lithium-ion battery electrolyte has poor performance under high and low temperature conditions, is flammable and has a high solubility to lithium salts affected by temperature, resulting in insufficient safety performance.

Method used

A eutectic solution is formed using acrylate polymers with a specific mass ratio and lithium difluorosulfonimide as part of the electrolyte, thereby improving the thermal stability of the electrolyte and the dissolution performance of the lithium salt.

Benefits of technology

It significantly improves the high and low temperature performance and safety performance of the battery, reduces the solidification temperature and viscosity of the electrolyte, and enhances the safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004997785030000021
    Figure BDA0004997785030000021
  • Figure BDA0004997785030000022
    Figure BDA0004997785030000022
  • Figure BDA0004997785030000041
    Figure BDA0004997785030000041
Patent Text Reader

Abstract

The invention provides an electrolyte and a battery comprising the electrolyte. The electrolyte comprises an acrylate polymer and a lithium salt, the lithium salt comprises lithium bis (fluorosulfonyl) imide, and the mass ratio of the acrylate polymer to the lithium bis (fluorosulfonyl) imide is (1-10): 1. The acrylate polymer and the lithium bis (fluorosulfonyl) imide in a specific mass ratio are mixed to form a eutectic solution, so that the safety performance, the high-temperature performance and the low-temperature performance of the battery can be obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to an electrolyte and a battery comprising the electrolyte. Background Art

[0002] In recent years, the lithium-ion battery industry has developed very rapidly, which has also driven the development of electrolytes. However, the electrolytes on the market are still mainly based on traditional carbonate solvents. However, this type of electrolyte is flammable and combustible. When external force puncture or short circuit caused by lithium precipitation occurs, the battery temperature will rise rapidly, causing the electrolyte to burn violently and causing serious safety accidents.

[0003] Eutectic solvent refers to a solvent obtained by mixing hydrogen bond donors and hydrogen bond acceptors. The melting point of the mixture is lower than the melting point of any of the substances. Eutectic solvents have most of the advantages of ionic liquids, such as good thermal stability, wide electrochemical window, low vapor pressure and high electrolyte conductivity. At the same time, eutectic solvents have more obvious advantages than ionic liquid solvents, such as simple preparation, low cost and non-toxicity. Therefore, compared with traditional electrolytes, eutectic solvents have the advantages of non-flammability and low melting point, which can significantly improve the safety performance of batteries.

[0004] At present, the eutectic solvents commonly used in electrolytes are organic solvents such as amides, carboxylic acids, and phenol-naphthalene. However, the stability and properties of these eutectic solvents are limited by specific temperature conditions, especially the solubility of lithium salts is greatly affected by temperature. In addition, alkaline or acidic eutectic solvents such as amides and carboxylic acids are not conducive to the long-term stability of internal battery materials, increase the risk of corrosion and oxidation inside the battery, and may cause battery failure, leakage or even short circuit, thereby causing safety problems.

[0005] Therefore, how to improve the performance of the electrolyte at high and low temperatures and enhance the temperature tolerance of the electrolyte is a technical problem that needs to be solved urgently in this field. Summary of the invention

[0006] The invention provides an electrolyte, wherein an acrylic acid ester polymer and lithium bis(fluorosulfonyl)imide in a specific mass ratio are added to the electrolyte, and the two can form a eutectic solution after compounding, so that both the low-temperature performance and the high-temperature performance of the electrolyte are significantly improved.

[0007] The present invention also provides a battery. Since the battery includes the electrolyte, the battery has excellent high and low temperature performance and safety performance.

[0008] A first aspect of the present invention provides an electrolyte comprising an acrylate polymer and a lithium salt, wherein the lithium salt comprises lithium bis(fluorosulfonyl)imide, and the mass ratio of the acrylate polymer to the lithium bis(fluorosulfonyl)imide is (1-10):1.

[0009] The electrolyte as described above, wherein the acrylic acid ester polymer has a structural unit shown in Formula 1:

[0010]

[0011] In Formula 1, R1, R2, and R3 are each independently selected from H, halogen, cyano, C1-C6 alkyl, C1-C6 alkoxy, C2-C6 alkenyl, or C6-C10 aryl;

[0012] Preferably, the structural unit is selected from at least one of the following structures:

[0013]

[0014] The electrolyte as described above, wherein the lithium salt further comprises at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium bis(trifluoromethylsulfonyl)imide, lithium difluorobis(oxalatophosphate), lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium hexafluoroantimonate, lithium hexafluoroarsenate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, tris(trifluoromethylsulfonyl)methyl lithium and lithium bis(trifluoromethylsulfonyl)imide;

[0015] Preferably, the mass content of other lithium salts in the electrolyte is 1% to 18%.

[0016] The electrolyte as described above, wherein, based on the total mass of the electrolyte, the mass content of the lithium salt is h%, and the mass content of the acrylic ester polymer is c%, wherein 0.025≤h / (c+20)≤0.5.

[0017] The electrolyte as described above, wherein, based on the total mass of the electrolyte, 5≤h≤25, and / or, 20≤c≤50.

[0018] The electrolyte as described above, wherein the electrolyte further comprises an additive, and the additive comprises one or more of fluoroethylene carbonate, vinylene carbonate, vinyl sulfate, 1,3-propylene sultone, vinylethylene carbonate, succinonitrile, adiponitrile, and 1,3,6-hexanetrinitrile;

[0019] Preferably, the content of the additive in the electrolyte is 0wt% to 20wt%.

[0020] The second aspect of the present invention provides a battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the electrolyte is selected from the electrolyte described in the first aspect of the present invention, and the separator comprises a base film and a glue layer arranged on at least one surface of the base film.

[0021] The battery as described above, wherein the glue layer comprises polyvinylidene fluoride, and / or the glue layer has a thickness of t μm, wherein 0.5<t<3;

[0022] Preferably, 3.5≤c / t≤50.

[0023] The battery as described above, wherein the negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector;

[0024] The tensile toughness of the negative electrode current collector is s joules, where 50≤980s+c≤125;

[0025] Preferably, 0.03≤s≤0.1.

[0026] The battery as described above, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector;

[0027] The positive electrode active material layer includes a lithium cobalt oxide material. Preferably, the lithium cobalt oxide material includes doping elements, and the doping elements include one or more of Mn, Ni, Mg, Al, W, Zn, Ca, Fe, Ba, Sr, B, Cr, V, Zr, Ti, Sn, Mo, Ru, Si, Sb, Nb, and Te.

[0028] The implementation of the present invention has at least the following advantages:

[0029] The present invention adds an acrylate polymer and lithium bis(fluorosulfonyl)imide in a specific mass ratio into an electrolyte, wherein the acrylate polymer serves as a hydrogen bond donor and the lithium bis(fluorosulfonyl)imide serves as a hydrogen bond acceptor. The two can form a eutectic solution after mixing. The eutectic solution has the advantages of good thermal stability, non-flammability, low melting point, good solubility in lithium salts, etc., which is not only beneficial to improving the thermal stability of the electrolyte, but also can reduce the solidification temperature of the electrolyte, so that the electrolyte maintains a low viscosity and internal resistance at low temperatures, thereby allowing the battery to have both excellent high and low temperature performance and safety performance. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] A first aspect of the present invention provides an electrolyte, comprising an acrylate polymer and a lithium salt, wherein the lithium salt comprises lithium bis(fluorosulfonyl)imide, and the mass ratio of the acrylate polymer to the lithium bis(fluorosulfonyl)imide is (1 to 10): 1. Exemplarily, the mass ratio of the acrylate polymer to the lithium bis(fluorosulfonyl)imide may be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1 or a range formed by any two of the mass ratios above.

[0032] The electrolyte of the present invention includes an acrylic polymer and lithium bis(fluorosulfonyl)imide in a specific mass ratio, wherein the acrylic polymer is a hydrogen bond donor and the lithium bis(fluorosulfonyl)imide is a hydrogen bond acceptor. After the two are mixed, the O atom region of the acrylic polymer with strong electronegativity has a tendency to coordinate with the positive charge region around the lithium ions in the lithium bis(fluorosulfonyl)imide. This coordination tendency makes the two have lower energy and uniform molecular electrostatic potential energy surface distribution after mixing. Therefore, after the two are mixed, a eutectic solution system with a stable structure can be formed. The solution is not flammable, so that the safety performance and high temperature performance of the battery are improved. In addition, the melting point of the two after mixing is lower than the melting point of the two existing independently, which not only shows excellent solubility performance for lithium salts in the electrolyte, but also reduces the solidification temperature of the electrolyte, so that the electrolyte maintains a low viscosity and internal resistance at low temperatures, thereby improving the low temperature performance of the battery.

[0033] Compared with amide, carboxylic acid, and urea compounds used as hydrogen bond acceptors in eutectic solutions in traditional electrolytes, acrylate polymers have the following advantages as hydrogen bond donors:

[0034] 1. Low vapor pressure and high stability: Acrylic polymers have a high molecular weight and a very low vapor pressure, which allows them to remain relatively stable at room temperature and not easily evaporate, which is conducive to the formation and stability of eutectic solutions.

[0035] 2. Wide temperature range: In the eutectic solution, acrylic polymers can exist in liquid form in the range of -20°C to 80°C and maintain good stability. They can dissolve lithium salts and additives under low temperature conditions.

[0036] 3. Excellent solubility: Acrylate polymers can significantly improve the solubility of electrolyte additives, especially for additives with low solubility in conventional carbonate or carboxylate solvents.

[0037] In summary, the present application can significantly improve the safety performance, high temperature performance and low temperature performance of the battery by adding a specific mass ratio of acrylic acid ester polymer and lithium bis(fluorosulfonyl)imide to the electrolyte.

[0038] In a preferred embodiment, the acrylic acid ester polymer has a structural unit shown in Formula 1:

[0039]

[0040] In Formula 1, R1, R2, and R3 are each independently selected from H, halogen, cyano, C1-C6 alkyl, C1-C6 alkoxy, C2-C6 alkenyl, or C6-C10 aryl.

[0041] The halogen can be F, Cl, Br, I.

[0042] The C1-C6 alkyl group may be a straight-chain alkyl group or a branched-chain alkyl group having 1 to 6 carbon atoms, for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, n-hexyl, etc.

[0043] The C1-C6 alkoxy group may be a straight chain alkoxy group or a branched chain alkoxy group having 1 to 6 carbon atoms, for example, methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, tert-butoxy, n-pentoxy, n-hexoxy, etc.

[0044] The C2-C6 alkenyl group may be a straight-chain alkenyl group or a branched alkenyl group having 2 to 6 carbon atoms, for example, vinyl, n-propenyl, isopropenyl, n-butenyl, isobutenyl, etc.

[0045] The C6-C10 aryl group may be phenyl or naphthyl.

[0046] Selecting acrylic polymers within the above general formula is conducive to compounding with lithium bis(fluorosulfonyl)imide to form a eutectic solution;

[0047] Preferably, the structural unit represented by Formula 1 is selected from at least one of the following structures:

[0048]

[0049] In a preferred embodiment, the molecular weight of the acrylic polymer is 100,000 to 3 million, preferably 500,000 to 2.7 million. For example, the molecular weight of the acrylic polymer can be 100,000, 300,000, 500,000, 700,000, 900,000, 1.1 million, 1.3 million, 1.5 million, 1.7 million, 1.9 million, 2.1 million, 2.3 million, 2.5 million, 2.7 million, 3 million, or a range consisting of any two of the above values. Acrylic polymers with larger molecular weights usually have better solubility because their molecular chains can provide more sites for solvent molecules to interact with other compounds, thereby helping to enhance solubility; acrylic polymers with too small molecular weights have fewer hydrogen bonds and poor eutectic ability; however, when the molecular weight of the acrylic polymer is too large, the longer and more complex its molecular chain is, the worse the ionic conductivity of the electrolyte will be, directly affecting the diffusion rate and conductivity of the electrolyte.

[0050] In a specific embodiment, in order to facilitate the eutectic formation of the acrylic ester polymer and the lithium salt after mixing, the mixture of the two can be heated and stirred at 50-100° C. until the liquid becomes clear and transparent. For example, the heating temperature can be 50° C., 60° C., 70° C., 80° C., 90° C., 100° C., or a range consisting of any two of the above values.

[0051] Lithium salt is an important component of the electrolyte. It can dissociate lithium ions in the electrolyte and provide the lithium ions necessary for the battery to work. It can also adjust the charge balance inside the battery to avoid overcharging or over-discharging. The appropriate type and concentration of lithium salt can also improve the battery's power density, battery capacity and other performance.

[0052] In addition to lithium bisfluorosulfonyl imide, the lithium salt of the present invention also includes other lithium salts, including lithium hexafluorophosphate (LiPF6), (fluorosulfonyl) (trifluoromethanesulfonyl) imide, lithium difluorophosphate (LiPO2F2), difluorooxalato lithium borate (LiDFOB), lithium bisfluorosulfonyl imide (LiTFSI), bistrifluoromethylsulfonyl imide, difluorobisoxalato lithium phosphate, lithium tetrafluoroborate, bisoxalato borate, lithium hexafluoroantimonate, lithium hexafluoroarsenate, lithium bis(trifluoromethylsulfonyl) imide, lithium bis(pentafluoroethylsulfonyl) imide, tris(trifluoromethylsulfonyl) methyl lithium and one or more of lithium bis(trifluoromethylsulfonyl) imide and lithium (fluorosulfonyl) (trifluoromethanesulfonyl) imide.

[0053] High concentration of lithium bis(fluorosulfonyl)imide can easily corrode the battery aluminum foil and make the low-temperature performance of the battery poor. Appropriate addition of other lithium salts is beneficial to passivate the aluminum foil, reduce corrosion, and improve the low-temperature performance of the battery.

[0054] Preferably, the mass content of other lithium salts is 1% to 18%. Exemplarily, the mass content of other lithium salts can be 1%, 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18% or a range consisting of any two of the above values.

[0055] The content of lithium salt and the content of acrylic polymer in the electrolyte are also important factors affecting the performance of the electrolyte. In a specific embodiment, based on the total mass of the electrolyte, the mass content of lithium salt is h%, and the mass content of acrylic polymer is c%, wherein 0.025≤h / (c+20)≤0.5. Exemplarily, h / (c+20) can be 0.025, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5 or a range consisting of any two of the above values.

[0056] When h / (c+20) is less than 0.025, the content of lithium salt in the electrolyte is too little, resulting in a decrease in the ionic conductivity of the electrolyte; when h / (c+20) is greater than 0.5, the content of lithium salt in the electrolyte is too high, the solubility of lithium salt is poor, and it is easy to decompose in large quantities at high temperatures, resulting in an unstable interface between the electrolyte and the electrode, thereby reducing the safety performance of the battery.

[0057] Further, 5≤h≤25, and / or, 20≤c≤50. For example, the mass content of lithium salt in the electrolyte can be 5%, 10%, 13%, 15%, 18%, 20%, 25% or a range consisting of any two of the above values, and the mass content of acrylic acid ester polymer in the electrolyte can be 20%, 30%, 40%, 50% or a range consisting of any two of the above values.

[0058] The electrolyte of the present invention may also include other solvents, including propyl propionate, ethyl propionate, ethyl butyrate, ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, and the like.

[0059] The electrolyte of the present invention also includes additives, which may be negative electrode film-forming additives and / or positive electrode film-forming additives, specifically including but not limited to one or more of fluoroethylene carbonate, vinylene carbonate, vinyl sulfate, 1,3-propane sultone, 1,3-propylene sultone, vinyl ethylene carbonate, succinonitrile, adiponitrile, 1,3,6-hexanetrinitrile, and triphenyl phosphate.

[0060] Among them, fluoroethylene carbonate, vinylene carbonate, 1,3-propylene sultone, and vinylethylene carbonate are negative electrode film-forming additives that can ensure the stability of battery cycling.

[0061] Succinonitrile, adiponitrile, and 1,3,6-hexanetrinitrile are positive electrode film-forming additives that can complex transition metal ions in the positive electrode and inhibit the dissolution of metal ions under high voltage.

[0062] Preferably, the content of the additive in the electrolyte is 0wt% to 20wt%. Exemplarily, the content of the additive in the electrolyte can be 0wt%, 3wt%, 5wt%, 8wt%, 10wt%, 12wt%, 15wt%, 18wt%, 20wt% or a range consisting of any two of the above values. When the content exceeds 20wt%, it is easy to cause excessive growth of the positive and negative electrode interface protective film, thereby increasing the internal impedance of the battery.

[0063] The second aspect of the present invention provides a battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the electrolyte is selected from the electrolyte provided by the first aspect of the present invention, and the separator comprises a base film and a glue layer arranged on at least one surface of the base film.

[0064] Since the battery of the present invention includes the above-mentioned electrolyte, the battery has both excellent high and low temperature performance and safety performance.

[0065] Furthermore, the above-mentioned glue layer includes polyvinylidene fluoride (PVDF). During the first charge and discharge process of the battery, the acrylic polymer and lithium bis(fluorosulfonyl)imide in the electrolyte can form a SEI film on the surface of the negative electrode, and hydrogen bonds can be formed between the acrylic polymer in the SEI film and PVDF. Therefore, the PVDF layer of the separator has good compatibility with the negative electrode interface and can fit tightly, thereby shortening the lithium ion deintercalation distance and preventing the lithium plating and cycle diving problems caused by the broken bridge between the separator and the negative electrode due to long-term immersion in the electrolyte.

[0066] Furthermore, the thickness of the glue layer is tμm, wherein 3.5≤c / t≤50. Exemplarily, c / t can be 3.5, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50 or a range consisting of any two of the above values. When c / t<3.5, the content of acrylic polymer in the electrolyte is relatively low, and the content of PVDF in the diaphragm is excessive, resulting in increased density and reduced air permeability of the diaphragm; when c / t>50, the content of PVDF in the diaphragm is relatively low, and the content of acrylic polymer in the electrolyte is relatively high. Excessive acrylic polymer is easily freed and forms a bond with PVDF, making the interface between the diaphragm and the negative electrode in an unstable state, which is easy to cause the negative electrode and the diaphragm to peel off during a long cycle, thereby reducing the capacity retention rate of the battery.

[0067] Specifically, the thickness tμm of the adhesive layer satisfies 0.5<t<3. For example, the thickness of the adhesive layer may be 0.6μm, 1.0μm, 1.5μm, 2.0μm, 2.5μm, 2.9μm or a range formed by any two of the above values.

[0068] The present invention does not specifically limit the type of base film, which can be selected from base films conventionally used in the art, such as polyethylene film, polypropylene film, polyethylene and polypropylene composite film, and the like.

[0069] The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector. The present invention does not specifically limit the type of the negative electrode current collector, which can be selected from the negative electrode current collectors commonly used in the art, such as copper foil or carbon-coated copper foil.

[0070] Acrylic polymers will not only form SEI film on the negative electrode, but also adhere to the exposed surface of the negative electrode current collector to form a corresponding protective film. When the battery is in a half-charged state, the inside of the battery is not in a steady state, and a weak electrochemical reaction will occur. At this time, the potential of the negative electrode current collector is lower than that of the negative electrode active material, and it will react first, resulting in pitting holes on the surface of the negative electrode current collector. Acrylics adhere to the surface of the negative electrode current collector to form a protection, so that the battery can avoid the electrochemical reaction of the negative electrode current collector when it is stationary or over-discharged, and ensure its integrity.

[0071] Further, the tensile toughness of the negative electrode current collector is s joules, and the relationship between the tensile strength s of the negative electrode current collector and the mass content c% of the acrylic polymer in the electrolyte satisfies 50≤980s+c≤125. Exemplarily, 980s+c can be 50, 60, 70, 80, 90, 100, 110, 120, 125 or a range consisting of any two of the above values.

[0072] When 980s+c<50, the tensile strength of the negative electrode current collector is weak, and the content of acrylic polymers in the electrolyte is also low, which makes it difficult to protect the negative electrode current collector and makes it easy for it to be corroded by the electrolyte or bend or squeezed under external force conditions. When 980s+c>125, the tensile strength of the negative electrode current collector is strong, and the content of acrylic polymers in the electrolyte is also high. Although it can better protect the negative electrode current collector, the negative electrode current collector with too high strength is prone to burrs and dust during the cutting process, which can easily cause micro-short circuit in the battery.

[0073] Preferably, the tensile toughness s of the negative electrode current collector satisfies 0.03≤s≤0.1. For example, s may be 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, or a range consisting of any two of the above values.

[0074] The composition of the negative electrode active material layer can refer to the composition of the negative electrode active material layer in the negative electrode sheet conventionally used in the art, and its main substance is the negative electrode active material, and it can also include auxiliary components such as a conductive agent, a binder and a thickener. Among them, the negative electrode active material includes a carbon material and / or a silicon material. Specifically, the carbon material includes one or more of artificial graphite, natural graphite, hard carbon and soft carbon, and the silicon material includes one or more of elemental silicon, silicon-oxygen material, and silicon-carbon material.

[0075] Furthermore, the mass content of the negative electrode active material in the negative electrode active material layer is 97% to 98.8%. Exemplarily, the mass content of the negative electrode active material in the negative electrode active material layer can be 97%, 97.5%, 98.0%, 98.5%, 98.8% or a range consisting of any two of the above values.

[0076] The conductive agent is selected from one or more of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotube and metal powder.

[0077] The binder is selected from one or more of styrene-butadiene rubber, polytetrafluoroethylene and polyethylene oxide.

[0078] The thickener is selected from one or more of sodium carboxymethyl cellulose, carboxymethyl cellulose, methyl cellulose, polyvinyl pyrrolidone, etc.

[0079] The negative electrode sheet of the present invention can be obtained by dispersing components such as negative electrode active materials, conductive agents, binders and thickeners in water to form slurry, then coating the slurry on a negative electrode current collector, drying, rolling and slitting.

[0080] The positive electrode sheet of the present invention includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector. Among them, the positive electrode current collector can be selected from aluminum foil, a composite current collector (aluminum foil / PP / aluminum foil, aluminum foil / PE / aluminum foil). The main substance in the positive electrode active material layer is a positive electrode active material, and also includes auxiliary components such as a conductive agent and a binder. Among them, the mass content of the positive electrode active material in the positive electrode active material layer is 96.5wt%-98.5wt%. Exemplarily, the mass content of the positive electrode active material in the positive electrode active material layer can be 96.5%, 97.0%, 97.5%, 98.0%, 98.5% or a range consisting of any two of the above values.

[0081] Further, the positive electrode active material is selected from lithium cobalt oxide material. Preferably, the lithium cobalt oxide material includes doping elements, wherein the doping elements include but are not limited to one or more of Mn, Ni, Mg, Al, W, Zn, Ca, Fe, Ba, Sr, B, Cr, V, Zr, Ti, Sn, Mo, Ru, Si, Sb, Nb, and Te.

[0082] The types of the binder and the conductive agent may refer to the selection of the binder and the conductive agent in the negative electrode active material layer, and will not be described in detail here.

[0083] The negative electrode sheet of the present invention can be obtained by dispersing components such as positive electrode active materials, conductive agents and binders in NMP to form slurry, then coating the slurry on a positive electrode current collector, drying, rolling and slitting.

[0084] The battery of the present invention may be a wound battery or a laminated battery. In a specific embodiment, the negative electrode sheet, the separator and the positive electrode sheet may be sequentially stacked and then wound or laminated to obtain a battery core, and then packaged, injected with electrolyte, aged, formed, and sorted to obtain the battery of the present invention.

[0085] The electrolyte and the battery of the present invention will be described in detail below in conjunction with specific embodiments.

[0086] In the following examples and comparative examples, the performance test method of the battery is as follows:

[0087] 1. Overcharge test

[0088] Test method: At 25℃±5℃, discharge the battery at 0.2C to the lower limit voltage of 3.0V, let it stand for 2 minutes, then charge it at 0.7C constant current and constant voltage to the upper limit voltage of 4.5V, let it stand for 10 minutes, and then charge it at 18.5V constant voltage for 40 hours. Observe whether there is fire or explosion on the surface of the battery. If there is no fire or explosion, it means it has passed. Test 10 groups of batteries in parallel, and calculate the battery overcharge test pass rate = pass number / 10×100%.

[0089] 2. Acupuncture test

[0090] Test method: At 25℃±5℃, discharge the battery at 0.2C to the lower limit voltage of 3.0V, let it stand for 2 minutes, then charge it at 0.7C constant current and constant voltage to the upper limit voltage of 4.5V, let it stand for 10 minutes, and then pierce the battery with a 2.5mm steel needle at 200mm / s. Observe whether there is fire or explosion on the surface of the battery. If there is no fire or explosion, it means it has passed. Test 10 groups of batteries in parallel, and calculate the battery overcharge test pass rate = pass number / 10×100%.

[0091] 3. 45℃ cycle test

[0092] The batteries prepared in the examples and comparative examples were placed at 45°C for 2h, charged at a constant current of 1C to 4.48V, then charged at 0.7C to the upper limit voltage (4.53V), then charged at a constant voltage of 4.53V to 0.05C, left standing for 5 minutes, and then discharged at a constant current of 0.7C to 3V, left standing for 5 minutes. This was one charge and discharge cycle. The charge / discharge was repeated for 700T, and the cycle capacity retention rate was recorded.

[0093] 4. 10℃ cycle test

[0094] The batteries prepared in the examples and comparative examples were placed at 10°C for 2 h, charged to 4.53 V at a constant current of 0.7 C, charged to 0.05 C at a constant voltage, and allowed to stand for 5 minutes. They were then discharged to 3 V at a constant current of 0.5 C and allowed to stand for 5 minutes. This was one charge and discharge cycle. The battery was charged / discharged for 500 T in this manner, and the cycle capacity retention rate was recorded.

[0095] Examples 1 to 21

[0096] Embodiments 1 to 21 provide an electrolyte and a lithium ion battery, and the preparation method thereof comprises the following steps:

[0097] 1. Preparation of electrolyte

[0098] 1) In a glove box with H2O<0.01ppm, O2<0.01ppm and argon atmosphere, an acrylic polymer and lithium bis(fluorosulfonyl)imide were mixed and heated and stirred at 60°C until the liquid became clear and transparent, thereby obtaining a eutectic solution;

[0099] 2) adding lithium hexafluorophosphate to the eutectic solution, stirring until the lithium hexafluorophosphate is completely dissolved, then adding additives (fluoroethylene carbonate, 1,3-propylene sultone, succinonitrile, 1,3,6-hexanetrinitrile in a mass ratio of 12:3:2:3), stirring evenly, and obtaining an electrolyte after passing the moisture and free acid tests.

[0100] 2. Preparation of positive electrode

[0101] The positive electrode active material lithium cobalt oxide, the conductive agent Super P and the binder PVDF are dispersed in an appropriate amount of NMP solvent in a mass ratio of 98:1:1, and stirred thoroughly to form a uniform positive electrode slurry;

[0102] The positive electrode slurry is coated on the positive electrode current collector aluminum foil, and then dried, rolled and cut to obtain the positive electrode sheet.

[0103] 3. Preparation of negative electrode sheet

[0104] Disperse the negative electrode active material, conductive agent Super P, binder SBR, and thickener sodium carboxymethyl cellulose in an appropriate amount of deionized water at a mass ratio of 97:1:1.5:0.5, and stir thoroughly to form a uniform negative electrode slurry;

[0105] The negative electrode slurry is coated on the surface of a copper foil with a tensile toughness of 0.05s, and then dried, rolled and cut to obtain a negative electrode sheet.

[0106] 4. Preparation of diaphragm

[0107] The front side of a 5 μm thick polyolefin-based film is in contact with a 1.5 μm thick PVDF film, and the back side is in contact with a 1 μm thick PMMA film. After hot pressing by a machine, a composite diaphragm is obtained, wherein the PVDF layer formed after hot pressing is a glue layer.

[0108] 5. Assembly of lithium-ion batteries

[0109] The positive electrode sheet, separator and negative electrode sheet are placed in order, and then wound to obtain a winding core, and then after welding the pole ears and injecting the above electrolyte, vacuum sealing, standing, forming and other processes, a lithium-ion battery is prepared.

[0110] In the above preparation process, the type and molecular weight of the acrylic polymer, the mass ratio of the acrylic polymer to lithium bis(fluorosulfonyl)imide, the mass content of the acrylic polymer in the electrolyte c%, and the mass content of the lithium salt in the electrolyte h% are listed in Table 1, wherein the mass content of the lithium salt is the sum of the mass contents of LiTFSI and lithium hexafluorophosphate in the electrolyte.

[0111] Table 1

[0112]

[0113] In Table 1, the structural unit of PMMA is Formula 1-1, the structural unit of polymer 1 is Formula 1-2, the structural unit of polymer 2 is Formula 1-3, the structural unit of polymer 3 is Formula 1-4, the structural unit of polymer 4 is Formula 1-5, and the structural unit of polymer 5 is Formula 1-6.

[0114] The following conclusions can be drawn from Table 1:

[0115] 1) From the comparison of Examples 1 to 6, it can be seen that the acrylate compounds with different types of substituents such as halogen, cyano, methyl, methoxy, alkenyl, phenyl, etc. can form eutectic solutions with LiTFSI, and make the battery have excellent 45°C cycle performance, 10°C cycle performance, needle penetration test pass rate and overcharge test pass rate.

[0116] 2) From the comparison of Examples 1 and 7 to 10, it can be seen that the molecular weight of PMMA used in the eutectic solution also affects the performance of the battery. When the molecular weight is lower than 50W or higher than 270W, the 10°C and 45°C cycle performance of the battery are reduced. Among them, the molecular weight is preferably in the range of 50W to 270W, so that the battery can have excellent 10°C and 45°C cycle performance as well as puncture safety and overcharge safety.

[0117] 3) From the comparison of Examples 1 and 11 and Comparative Example 1, it can be seen that the mixing of PMMA and LiTFSI in the eutectic solution in different mass ratios will affect the battery performance. When the mass ratio is 2:1 and the mass ratio is 10:1, the battery can have excellent 10°C and 45°C cycle performance as well as puncture safety and overcharge safety. When the mass ratio is 11:1, the battery's 10°C and 45°C cycle as well as puncture and overcharge safety are significantly reduced.

[0118] 3) From the comparison of Example 1 and Examples 12 to 15, it can be seen that the different contents of the acrylic polymer in the electrolyte also affect the battery performance. When the content of the acrylic polymer is in the range of 10% to 50%, the battery's 10°C and 45°C cycle performance, puncture safety and overcharge safety are relatively excellent. When the content of the acrylic polymer is less than 10% or greater than 50%, the battery's 45°C and 10°C cycle performance are both reduced, and the battery's puncture safety is also significantly reduced.

[0119] 4) From the comparison between Example 1 and Examples 16 to 19, it can be seen that when the relationship h / (c+20) between the content c% of the acrylic polymer in the electrolyte and the content h% of the lithium salt exceeds 0.5 (Example 16 and Example 19), the eutectic solution formed has limited solubility for the lithium salt, resulting in a decrease in various aspects of the battery performance. Among them, Example 19 further increases the content of lithium salt on the basis of Example 16, resulting in excessive lithium salt content and further decreases in various aspects of the battery performance; when the content of the lithium salt does not exceed 25% and the relationship h / (c+20) satisfies 0.025 to 0.5, the battery performance is relatively excellent in all aspects.

[0120] Embodiments 20 to 30

[0121] Embodiments 20 to 30 provide an electrolyte and a lithium ion battery, and the preparation method thereof is basically the same as that of Embodiment 1, except that the preparation of the separator and the negative electrode sheet is different from that of Embodiment 1. The specific preparation method is as follows:

[0122] Preparation of negative electrode:

[0123] Disperse the negative electrode active material, conductive agent Super P, binder SBR, and thickener sodium carboxymethyl cellulose in an appropriate amount of deionized water at a mass ratio of 97:1:1.5:0.5, and stir thoroughly to form a uniform negative electrode slurry;

[0124] The negative electrode slurry is coated on the surface of the copper foil, and then dried, rolled and cut to obtain the negative electrode sheet.

[0125] The tensile toughness of the copper foils used in different embodiments is listed in Table 2.

[0126] Preparation of diaphragm:

[0127] The front side of a 5 μm thick polyolefin base film is in contact with a PVDF film, and the back side is in contact with a 1 μm thick PMMA film, and a composite diaphragm is obtained after hot pressing by a machine;

[0128] The PVDF layer formed after hot pressing is the adhesive layer, and the thickness of the adhesive layer in different embodiments is listed in Table 2.

[0129] For the convenience of comparison, Example 1 is also listed in Table 2.

[0130] Table 2

[0131]

[0132] The following conclusions can be drawn from Table 2:

[0133] 1) By comparing Example 1 and Examples 20 to 25, it can be seen that when a PVDF layer is composited in the diaphragm and the thickness of the PVDF layer tμm and the content c% of the acrylic polymer in the electrolyte satisfy the range of 3.5≤c / t≤50, the battery's 45°C and 10°C cycle performance, puncture safety and overcharge safety are better. When no PVDF glue layer is provided in the diaphragm, the battery's various performances are reduced. At the same time, the thickness of the PVDF glue layer should not be set too thick or too thin. When the thickness of the PVDF layer in Examples 23 and 24 is 3μm or 0.5μm respectively, the battery's various performances are also reduced compared to Examples 1 and 20 to 22.

[0134] 2) From the comparison between Example 1 and Examples 26 to 30, it can be seen that the tensile toughness of the negative electrode current collector copper foil also affects the cycle performance and safety performance of the battery. When the tensile toughness of the copper foil is larger (0.12J) or smaller (0.01J), the cycle performance and safety performance of the battery are slightly worse than those of the embodiments in which the tensile toughness is in the range of 0.03 to 0.1J. At the same time, when the relationship between the tensile toughness s of the copper foil and the content c% of the acrylic polymer in the electrolyte satisfies 50≤980s+c≤125, the 45°C cycle performance, 10°C cycle performance, puncture safety and overcharge safety of the battery are better. Among them, the relationship between s and c of Examples 26, 29 and 30 does not satisfy the above range, and the cycle and safety performance of the battery are relatively poor overall.

[0135] Comparative Example 2

[0136] This comparative example provides an electrolyte and a lithium ion battery, and the preparation method thereof is similar to that of Example 1, except that the preparation of the electrolyte comprises the following steps:

[0137] In a glove box with H2O<0.01ppm, O2<0.01ppm and argon atmosphere, PMMA (molecular weight of 1 million) was heated and stirred at 80°C until the liquid was clear and transparent, and then ethylene carbonate, propyl propionate and ethyl propionate were added and mixed uniformly, and then lithium hexafluorophosphate LiPF6 was added and stirred until completely dissolved, and then additives (fluoroethylene carbonate, 1,3-propylene sulfone, succinonitrile, 1,3,6-hexanetrinitrile in a mass ratio of 12:3:2:3) were added and stirred uniformly to obtain an electrolyte;

[0138] The electrolyte includes 20% PMMA, 10% ethylene carbonate, 30% propyl propionate, 15% ethyl propionate, 19% LiPF6, and the remainder is additives in terms of mass percentage.

[0139] Comparative Example 3

[0140] This comparative example provides an electrolyte and a lithium ion battery, and the preparation method thereof is similar to that of Example 1, except that the preparation of the electrolyte comprises the following steps:

[0141] In a glove box with H2O<0.01ppm, O2<0.01ppm and argon atmosphere, PMMA (molecular weight of 1 million) and lithium perchlorate are heated and stirred at 80°C in a mass ratio of 2:1 until the liquid becomes clear and transparent to obtain a mixed solution, and then 10% ethylene carbonate, 30% propyl propionate, and 15% ethyl propionate are added to the mixed solution respectively, and mixed evenly, and then lithium hexafluorophosphate LiPF6 is added, and after stirring until completely dissolved, additives (fluoroethylene carbonate, 1,3-propylene sulfone, succinonitrile, 1,3,6-hexanetrinitrile in a mass ratio of 12:3:2:3) are added thereto, and stirred evenly to obtain an electrolyte;

[0142] The electrolyte includes, by mass percentage, 20% of a mixture of PMMA and lithium perchlorate, 10% of ethylene carbonate, 30% of propyl propionate, 15% of ethyl propionate, 19% of lithium salt (including LiPF6 and lithium perchlorate), and the remainder is additives.

[0143] Comparative Example 4

[0144] This comparative example provides an electrolyte and a lithium ion battery, and the preparation method thereof is similar to that of Example 1, except that the preparation of the electrolyte comprises the following steps:

[0145] In a glove box with H2O<0.01ppm, O2<0.01ppm and argon atmosphere, PMMA (molecular weight of 1 million) and lithium chloride are heated and stirred at 80°C in a mass ratio of 2:1 until the liquid becomes clear and transparent to obtain a mixed solution, and then ethylene carbonate, propyl propionate and ethyl propionate are added to the mixed solution respectively and mixed evenly, and then lithium hexafluorophosphate LiPF6 is added and stirred until completely dissolved, and then additives (fluoroethylene carbonate, 1,3-propylene sulfone, succinonitrile and 1,3,6-hexanetrinitrile in a mass ratio of 12:3:2:3) are added thereto, and stirred evenly to obtain an electrolyte;

[0146] The electrolyte includes, by mass percentage, 20% of a mixture of PMMA and lithium chloride, 10% of ethylene carbonate, 30% of propyl propionate, 15% of ethyl propionate, 19% of lithium salt (including LiPF6 and lithium chloride), and the remainder is additives.

[0147] Comparative Example 5

[0148] This comparative example provides an electrolyte and a lithium ion battery, and the preparation method thereof is similar to that of Example 1, except that the preparation of the electrolyte comprises the following steps:

[0149] In a glove box with H2O<0.01ppm, O2<0.01ppm and argon atmosphere, ethylene carbonate, propyl propionate and 15% ethyl propionate were mixed evenly, 15% lithium hexafluorophosphate was added thereto, and after stirring until completely dissolved, additives (fluoroethylene carbonate, 1,3-propylene sultone, succinonitrile, 1,3,6-hexanetrinitrile in a mass ratio of 12:3:2:3) were added thereto, and stirred evenly to obtain an electrolyte;

[0150] The electrolyte includes 20% ethylene carbonate, 40% propyl propionate, 15% ethyl propionate, 19% LiPF6 in terms of mass percentage, and the remainder is additives.

[0151] The battery performance test results of Comparative Examples 2 to 5 are shown in Table 3:

[0152] Table 3

[0153]

[0154] It can be seen from the data in Table 3 that in Comparative Examples 2 to 4, PMMA alone, PMMA mixed with lithium perchlorate, and PMMA heated and mixed with lithium chloride cannot form a eutectic solution, and sufficient carbonate and carboxylic acid ester solvents need to be added to completely dissolve the lithium salt, and the obtained battery has poor 45°C cycle performance, 10°C cycle performance, needle puncture test pass rate, and overcharge test pass rate. By comparing Comparative Example 2 with Comparative Example 5, it can be seen that the conventional carbonate and carboxylic acid ester as solvents improve the battery's 45°C cycle performance and 10°C cycle performance compared to adding PMMA to the carbonate solvent, but the battery's needle puncture test pass rate and overcharge test pass rate are significantly reduced.

[0155] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An electrolyte, characterized in that: The electrolyte includes an acrylic acid ester polymer and a lithium salt, wherein the lithium salt includes lithium bis(fluorosulfonyl)imide, and the mass ratio of the acrylic acid ester polymer to the lithium bis(fluorosulfonyl)imide is (1-10):

1.

2. The electrolyte according to claim 1, characterized in that The acrylic acid ester polymer has a structural unit shown in Formula 1: In Formula 1, R1, R2, and R3 are each independently selected from H, halogen, cyano, C1-C6 alkyl, C1-C6 alkoxy, C2-C6 alkenyl, or C6-C10 aryl; Preferably, the structural unit is selected from at least one of the following structures:

3. The electrolyte according to claim 1, characterized in that The lithium salt also includes other lithium salts, and the other lithium salts include at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium bis(trifluoromethylsulfonyl)imide, lithium difluorobis(oxalatophosphate), lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium hexafluoroantimonate, lithium hexafluoroarsenate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, tris(trifluoromethylsulfonyl)methyllithium and lithium bis(trifluoromethylsulfonyl)imide; Preferably, the mass content of other lithium salts in the electrolyte is 1% to 18%.

4. The electrolyte according to claim 1, characterized in that Based on the total mass of the electrolyte, the mass content of the lithium salt is h%, and the mass content of the acrylic ester polymer is c%, wherein 0.025≤h / (c+20)≤0.

5.

5. The electrolyte according to claim 4, characterized in that 5≤h≤25, and / or, 20≤c≤50.

6. The electrolyte according to claim 1, characterized in that The electrolyte further includes an additive, wherein the additive includes one or more of fluoroethylene carbonate, vinylene carbonate, vinyl sulfate, 1,3-propylene sultone, vinylethylene carbonate, succinonitrile, adiponitrile, and 1,3,6-hexanetrinitrile; Preferably, the content of the additive in the electrolyte is 0wt% to 20wt%.

7. A battery comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, characterized in that: The electrolyte is selected from the electrolyte described in any one of claims 1 to 6, and the diaphragm includes a base film and a glue layer arranged on at least one surface of the base film.

8. The battery according to claim 7, characterized in that The adhesive layer includes polyvinylidene fluoride, and / or the thickness of the adhesive layer is t μm, wherein 0.5<t<3; Preferably, 3.5≤c / t≤50.

9. The battery according to claim 8, characterized in that The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector; The tensile toughness of the negative electrode current collector is s joules, where 50≤980s+c≤125; Preferably, 0.03≤s≤0.

1.

10. The battery according to any one of claims 7 to 9, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector; The positive electrode active material layer includes a lithium cobalt oxide material. Preferably, the lithium cobalt oxide material includes doping elements, and the doping elements include one or more of Mn, Ni, Mg, Al, W, Zn, Ca, Fe, Ba, Sr, B, Cr, V, Zr, Ti, Sn, Mo, Ru, Si, Sb, Nb, and Te.

Citation Information

Patent Citations

  • Application of polymer containing hindered amine structure in secondary lithium battery

    CN109786869A

  • Electrolyte raw material composition, electrolyte, lithium ion secondary battery and preparation method thereof

    CN111430780A

  • Solid electrolyte membrane, solid lithium ion battery and preparation method of solid lithium ion battery

    CN112038692A

  • Preparation method of wide-temperature-range electrolyte for lithium ion battery

    CN115377489A

  • Electrolyte, electrochemical device and electronic device

    CN116487694A

Cited By

  • Flame-retardant sulfuryl eutectic electrolyte and preparation method and application thereof