Method for improving electrical property test consistency of sodium ion battery
By performing the electrodeoxygenation process in a sodium ion battery, the sodium oxide in the sodium tablet is removed, the problem of electrochemical performance inconsistency caused by sodium tablet oxidation is solved, and the consistency and reliability of electrical performance tests are improved.
Patent Information
- Application Number
- CN202411130773.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
The oxidation of sodium tablets in sodium ion batteries leads to inconsistent electrochemical performance, affecting the test results, and the existing processing technology is immature, resulting in difficulty in evaluating material performance.
The electrical deoxygenation process is carried out before the electrical performance test, including constant current charging and constant voltage charging, removing sodium oxide from the sodium tablet, triggering the electrical deoxygenation reduction reaction through constant current charging, removing trace oxygen elements, and then reducing current polarization by constant voltage charging The impact of the sodium sheet surface structure is stabilized.
Effectively remove sodium oxide impurities in sodium tablets, improve the consistency of electrical performance testing of sodium ion batteries, ensure material reactive activity, and improve the reliability of test results.
Smart Images

Figure CN119009181A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of sodium ion batteries, and in particular to a method for improving the consistency of electrical performance testing of sodium ion batteries. Background Art
[0002] The development of positive and negative electrode material systems for sodium-ion batteries is of great significance for promoting their commercial applications. In this process, researchers inevitably need to assemble a large number of button batteries. Metallic sodium is often used as a counter electrode to evaluate the performance of positive (negative) electrode materials. + The potential of the battery is considered to be 0V at this time, so the voltage of the battery during the test is the potential of the positive (negative) electrode material.
[0003] Unlike lithium-ion batteries, the manufacturing and processing of metallic lithium is relatively mature, and lithium sheets of specific sizes can be customized to meet usage requirements. However, due to the strong activity and soft texture of metallic sodium, the current sodium sheet processing technology is not yet mature and needs to be improved. This is mainly reflected in the fact that sodium sheets are easily oxidized during storage and transportation, and the storage conditions are relatively harsh. The operation of using sodium ingots (soaked in kerosene, small pieces of metallic sodium are cut according to the amount and rolled into sodium sheets of uniform thickness, and then the sodium sheets are punched out with a round gun of suitable diameter) is relatively cumbersome and time-consuming.
[0004] If there is a large demand for button cells, raw material manufacturers or battery company testers generally choose to directly order sodium sheets and store them in a glove box with a good inert atmosphere to prevent oxidation as much as possible. The metallic luster of the sodium sheet surface can be observed with the naked eye. If it is relatively bright, it can be used. However, the tiny oxidation on the surface of the sodium sheet cannot be detected without relying on physical and chemical characterization instruments. At this time, the presence of sodium oxide will hinder the redox of sodium ions at the interface between the sodium sheet and the electrolyte, affecting the ion current density between the electrode material part facing the oxidized part of the sodium sheet, and then affecting the electrochemical performance of the material, resulting in a decrease in the capacity of the button half-cell, an increase in impedance, and a decrease in consistency. Obviously, this is not conducive to the evaluation and analysis of materials by researchers. Summary of the invention
[0005] The purpose of this application is to provide a method for improving the consistency of electrical performance testing of sodium ion batteries to solve the above problems.
[0006] To achieve the above objectives, the present application provides a method for improving the consistency of electrical performance testing of sodium ion batteries, comprising:
[0007] For sodium ion batteries, an electrical deoxidation process is set up before the electrical performance test process;
[0008] The electrical deoxidation process includes firstly performing constant current charging until the cut-off voltage is greater than the open circuit potential, and then performing constant voltage charging until the cut-off current is obtained.
[0009] Optionally, the constant current charging current is 0.010mA-0.020mA.
[0010] Optionally, the cut-off voltage is greater than the open circuit potential by 0.1V-0.2V.
[0011] Optionally, the open circuit potential is 2.6V-2.9V.
[0012] Optionally, the cut-off current is 1 μA - 3μA.
[0013] Optionally, the sodium ion battery is allowed to stand before the electrical deoxidation step.
[0014] Optionally, the standing time is greater than or equal to 12 hours.
[0015] Optionally, the sodium ion battery comprises a button cell.
[0016] Optionally, the electrical performance testing process includes a capacity testing process and a cycle testing process.
[0017] Optionally, during the capacity testing process, the oxygen content in the sodium sheet in the sodium ion battery is 1 ppm-100 ppm.
[0018] Compared with the prior art, the beneficial effects of this application include:
[0019] The method for improving the consistency of the electrical performance test of a sodium ion battery provided in the present application removes the sodium oxide impurity component present in the sodium sheet in the sodium ion button half-cell in situ without affecting the electrode material, thereby improving the reaction activity of the sodium sheet and providing a good guarantee for the consistency of the electrical performance test. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0021] Figure 1 A schematic diagram of the principle provided for this application;
[0022] Figure 2 A sodium sheet image of a LIR2430 button half-cell provided in Example 1;
[0023] Figure 3 A test curve diagram of the LIR2430 button-type half-cell provided in Example 2;
[0024] Figure 4A sodium sheet image of a LIR2430 button half-cell provided in Example 2;
[0025] Figure 5 The test curve diagram of the LIR2430 button half-cell provided for Comparative Example 1;
[0026] Figure 6 This is a test curve chart of the LIR2430 button half-cell provided for Comparative Example 2. DETAILED DESCRIPTION
[0027] As used herein:
[0028] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0029] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0030] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0031] In these examples, parts and percentages are by mass unless otherwise indicated.
[0032] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.
[0033] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0034] As a branch of molten salt electrolysis, the FFC Cambridge method has attracted little attention due to its complicated electrode manufacturing process and its reliance on suitable electrochemical reaction conditions to obtain electrolytic products of higher purity. This application reproduces the electrochemical concept of molten salt electro-deoxygenation for the first time in the field of sodium-ion batteries, and through experimental research, develops a set of test procedures that can in situ remove trace oxygen elements in sodium sheets, solving the problem of poor consistency of buckling due to micro-oxidation of sodium sheets.
[0035] Based on the above problems, the present application provides a method for improving the consistency of electrical performance testing of sodium ion batteries, comprising:
[0036] For sodium ion batteries, an electrical deoxidation process is set up before the electrical performance test process;
[0037] The electrical deoxidation process includes firstly performing constant current charging until the cut-off voltage is greater than the open circuit potential, and then performing constant voltage charging until the cut-off current is obtained.
[0038] It should be noted that the constant current charging in the electro-deoxidation process is essentially a constant potential electrolysis of trace sodium oxide, that is, a constant reverse potential is applied to the battery. The principle is as follows Figure 1 As shown, the potential of the sodium sheet is slightly lower than that of Na / Na + The reduction potential triggers the electro-deoxidation reduction reaction, and the chemical reaction formula is as follows:
[0039] Na2O+2e - =2Na+O 2- ;
[0040] O 2- It is separated from the sodium oxide lattice and migrates to the anode to react with carbon to produce CO or CO2. The chemical reaction formula is as follows:
[0041] C+O 2- =CO2+e - ;
[0042] C+O 2- =CO+2e - .
[0043] It can be understood that Na2O is reduced to obtain metallic Na through constant current charging, thereby removing trace oxygen elements in the sodium sheet;
[0044] It should also be noted that further constant voltage charging can continuously reduce the impact of current polarization, making the loose and porous sodium surface layer structure after deoxidation more compact and stable, which is convenient for subsequent use.
[0045] In some embodiments, the constant current charging current is 0.010mA-0.020mA.
[0046] Optionally, the constant current charging current can be 0.010mA, 0.011mA, 0.012mA, 0.013mA, 0.014mA, 0.015mA, 0.016mA, 0.017mA, 0.018mA, 0.019mA, 0.020mA or any value between 0.010mA and 0.020mA.
[0047] It should be noted that the polarization degree is controlled by limiting the constant current charging current to 0.010mA-0.020mA. If the current setting is too large, the Na + Deposited on the sodium sheet, causing the surface of the sodium oxide to be covered with metallic sodium, blocking the pores and affecting the O 2- If the current is set too small, although the polarization is smaller and the reaction is more stable, it takes a longer reaction time to proceed to the next step, which has a high time cost.
[0048] In some embodiments, the cut-off voltage is 0.1V-0.2V greater than the open circuit potential.
[0049] Optionally, the cut-off voltage may be greater than the open circuit potential of 0.1 V, 0.11 V, 0.12 V, 0.13 V, 0.14 V, 0.15 V, 0.16 V, 0.17 V, 0.18 V, 0.19 V, 0.2 V or any value between 0.1 V and 0.2 V.
[0050] It should be noted that when the cut-off voltage is set according to the open circuit potential and is greater than the open circuit potential by 0.1V-0.2V, irreversible damage may be caused to the structure of the material.
[0051] In some embodiments, the open circuit potential is 2.6V-2.9V.
[0052] Optionally, the open circuit potential may be 2.6V, 2.7V, 2.8V, 2.9V or any value between 2.6V and 2.9V.
[0053] In some embodiments, the cutoff current is 1 μA-3 μA.
[0054] Optionally, the cut-off current may be 1 μA, 2 μA, 3 μA or any value between 1 μA and 3 μA.
[0055] It should be noted that when the cut-off current is 1 μA-3 μA, the slight polarization caused by the constant current process is eliminated, so that the reaction can be carried out thoroughly enough, while saving time cost and preventing the reaction time of this step from being too long.
[0056] In some embodiments, the sodium ion battery is allowed to stand before the electro-deoxidation step.
[0057] In some embodiments, the standing time is greater than or equal to 12 hours.
[0058] Optionally, the standing time may be 12 h, 15 h, 20 h, 24 h, or any value greater than or equal to 12 h.
[0059] It should be noted that the electrolyte should be left to completely wet the diaphragm.
[0060] In some embodiments, the sodium ion battery comprises a button cell.
[0061] In some embodiments, the electrical performance testing process includes a capacity testing process and a cycle testing process.
[0062] In some embodiments, during the capacity testing process, the oxygen content in the sodium sheet in the sodium ion battery is 1 ppm-100 ppm.
[0063] Optionally, the oxygen content in the sodium sheet in the sodium ion battery can be 1 ppm, 10 ppm, 20 ppm, 30 ppm, 40 ppm, 50 ppm, 60 ppm, 70 ppm, 80 ppm, 90 ppm, 100 ppm or any value between 1 ppm and 100 ppm.
[0064] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0065] Example 1
[0066] This embodiment provides a method for improving the consistency of electrical performance testing of a sodium ion battery, comprising:
[0067] S1: Take the rolled hard carbon negative electrode from the manufacturer with a nominal specific capacity of 288g / mAh, cut it and assemble it with a sodium sheet (oxidation amount of 1ppm-100ppm) into a LIR2430 button half-cell (5PCS);
[0068] S2: On the blue battery test cabinet, connect the positive and negative electrodes with a snap-on clamp and let it stand for 12 hours to ensure that the electrolyte infiltrates the electrode material;
[0069] S3: Setting an electric deoxidation test process, firstly, the open circuit potential is 2.883V through the test, the current is set to 0.015mA for constant current charging, and the cut-off voltage is set to 3V according to the open circuit potential. When the voltage reaches the set cut-off voltage, constant voltage charging is performed until the cut-off current is 1μA;
[0070] S4: Set the capacity test process, 0.1C constant current discharge, 0V cut-off; 0.09C discharge, 0V cut-off; 0.08C constant current discharge, 0V cut-off; 0.07C constant current discharge, 0V cut-off; 0.06C constant current discharge, 0V cut-off; 0.05C constant current discharge, 0V cut-off; 0.04C constant current discharge, 0V cut-off; 0.03C constant current discharge, 0V cut-off; 0.02C constant current discharge, 0V cut-off; 0.01C constant current discharge, 0V cut-off; 0.1C charge, 2V cut-off;
[0071] S5: Start the test program of S3 and S4, and output the data after the test is completed.
[0072] After being assembled into a LIR2430 button-type half-cell, the sodium sheet Figure 2 shown.
[0073] Example 2
[0074] This embodiment provides a method for improving the consistency of electrical performance testing of a sodium ion battery, comprising:
[0075] S1: The hard carbon negative electrode is consistent with that in Example 1, and after cutting, it is assembled with a sodium sheet (oxidation amount is 1ppm-100ppm) into a LIR2430 button half-cell (5PCS);
[0076] S2: On the blue battery test cabinet, connect the positive and negative electrodes with a snap-on clamp and let it stand for 12 hours to ensure that the electrolyte infiltrates the electrode material;
[0077] S3: Setting an electric deoxidation test process, firstly, the open circuit potential is 2.744V through the test, the current is set to 0.010mA for constant current charging, and the cut-off voltage is set to 2.85V according to the open circuit potential. When the voltage reaches the set cut-off voltage, constant voltage charging is performed until the cut-off current is 1μA;
[0078] S4: Set the capacity test process, 0.1C constant current discharge, 0V cut-off; 0.09C discharge, 0V cut-off; 0.08C constant current discharge, 0V cut-off; 0.07C constant current discharge, 0V cut-off; 0.06C constant current discharge, 0V cut-off; 0.05C constant current discharge, 0V cut-off; 0.04C constant current discharge, 0V cut-off; 0.03C constant current discharge, 0V cut-off; 0.02C constant current discharge, 0V cut-off; 0.01C constant current discharge, 0V cut-off; 0.1C charge, 2V cut-off;
[0079] S5: Start the test program of S3 and S4, and output the data after the test is completed;
[0080] Repeat the above steps 5 times in total, and draw the data curve of these 5 times. The data curve is as follows: Figure 3 shown.
[0081] The sodium sheets assembled into LIR2430 button half-cells are as follows: Figure 4 shown.
[0082] Example 3
[0083] This embodiment provides a method for improving the consistency of electrical performance testing of a sodium ion battery, comprising:
[0084] S1: The hard carbon negative electrode is consistent with that in Example 1, and after cutting, it is assembled with a sodium sheet (oxygen content of 1ppm-100ppm) into a LIR2430 button half-cell (5PCS);
[0085] S2: On the blue battery test cabinet, connect the positive and negative electrodes with a snap-on clamp and let it stand for 12 hours to ensure that the electrolyte infiltrates the electrode material;
[0086] S3: Setting an electric deoxidation test process, firstly, the open circuit potential is 2.644V through the test, the current is set to 0.012mA for constant current charging, and the cut-off voltage is set to 2.80V according to the open circuit potential. When the voltage reaches the set cut-off voltage, constant voltage charging is performed until the cut-off current is 1μA;
[0087] S4: Set the capacity test process, 0.1C constant current discharge, 0V cut-off; 0.09C discharge, 0V cut-off; 0.08C constant current discharge, 0V cut-off; 0.07C constant current discharge, 0V cut-off; 0.06C constant current discharge, 0V cut-off; 0.05C constant current discharge, 0V cut-off; 0.04C constant current discharge, 0V cut-off; 0.03C constant current discharge, 0V cut-off; 0.02C constant current discharge, 0V cut-off; 0.01C constant current discharge, 0V cut-off; 0.1C charge, 2V cut-off;
[0088] S5: Start the test program of S3 and S4, and output the data after the test is completed.
[0089] Example 4
[0090] This embodiment provides a method for improving the consistency of electrical performance testing of a sodium ion battery, comprising:
[0091] S1: The hard carbon negative electrode is consistent with that in Example 1, and after cutting, it is assembled with a sodium sheet (oxidation amount is 1ppm-100ppm) into a LIR2430 button half-cell (5PCS);
[0092] S2: On the blue battery test cabinet, connect the positive and negative electrodes with a snap-on clamp and let it stand for 12 hours to ensure that the electrolyte infiltrates the electrode material;
[0093] S3: Setting an electric deoxidation test process, firstly, the open circuit potential is 2.785V through the test, the current is set to 0.018mA for constant current charging, and the cut-off voltage is set to 2.95V according to the open circuit potential. When the voltage reaches the set cut-off voltage, constant voltage charging is performed until the cut-off current is 1μA;
[0094] S4: Set the capacity test process, 0.1C constant current discharge, 0V cut-off; 0.09C discharge, 0V cut-off; 0.08C constant current discharge, 0V cut-off; 0.07C constant current discharge, 0V cut-off; 0.06C constant current discharge, 0V cut-off; 0.05C constant current discharge, 0V cut-off; 0.04C constant current discharge, 0V cut-off; 0.03C constant current discharge, 0V cut-off; 0.02C constant current discharge, 0V cut-off; 0.01C constant current discharge, 0V cut-off; 0.1C charge, 2V cut-off;
[0095] S5: Start the test program of S3 and S4, and output the data after the test is completed.
[0096] Example 5
[0097] This embodiment provides a method for improving the consistency of electrical performance testing of a sodium ion battery, comprising:
[0098] S1: The hard carbon negative electrode is consistent with that in Example 1, and after cutting, it is assembled with a sodium sheet (oxidation amount is 1ppm-100ppm) into a LIR2430 button half-cell (5PCS);
[0099] S2: On the blue battery test cabinet, connect the positive and negative electrodes with a snap-on clamp and let it stand for 12 hours to ensure that the electrolyte infiltrates the electrode material;
[0100] S3: Setting an electric deoxidation test process, firstly, the open circuit potential is 2.625V through the test, the current is set to 0.020mA for constant current charging, and the cut-off voltage is set to 2.95V according to the open circuit potential. When the voltage reaches the set cut-off voltage, constant voltage charging is performed until the cut-off current is 1μA;
[0101] S4: Set the capacity test process, 0.1C constant current discharge, 0V cut-off; 0.09C discharge, 0V cut-off; 0.08C constant current discharge, 0V cut-off; 0.07C constant current discharge, 0V cut-off; 0.06C constant current discharge, 0V cut-off; 0.05C constant current discharge, 0V cut-off; 0.04C constant current discharge, 0V cut-off; 0.03C constant current discharge, 0V cut-off; 0.02C constant current discharge, 0V cut-off; 0.01C constant current discharge, 0V cut-off; 0.1C charge, 2V cut-off;
[0102] S5: Start the test program of S3 and S4, and output the data after the test is completed.
[0103] Comparative Example 1
[0104] This comparative example provides a method for improving the consistency of electrical performance testing of a sodium ion battery, comprising:
[0105] S1: Assemble LIR2430 button half-cells (5 PCS) in the same manner as in Example 1;
[0106] S2: On the blue battery test cabinet, connect the positive and negative electrodes with a snap-on clamp and let it stand for 12 hours to ensure that the electrolyte infiltrates the electrode material;
[0107] S3: Setting an electric deoxidation test process, firstly, the open circuit potential is 2.883V through the test, the current is set to 0.030mA for constant current charging, and the cut-off voltage is set to 3.1V according to the open circuit potential. When the voltage reaches the set cut-off voltage, constant voltage charging is performed until the cut-off current is 1μA;
[0108] S4: Set the capacity test process, 0.1C constant current discharge, 0V cut-off; 0.09C discharge, 0V cut-off; 0.08C constant current discharge, 0V cut-off; 0.07C constant current discharge, 0V cut-off; 0.06C constant current discharge, 0V cut-off; 0.05C constant current discharge, 0V cut-off; 0.04C constant current discharge, 0V cut-off; 0.03C constant current discharge, 0V cut-off; 0.02C constant current discharge, 0V cut-off; 0.01C constant current discharge, 0V cut-off; 0.1C charge, 2V cut-off;
[0109] S5: Start the test program of S3 and S4, and output the data after the test is completed;
[0110] Repeat the above steps 5 times in total, and draw the data curve of the 5 times. The data curve is as shown in Figure 5 shown.
[0111] Comparative Example 2
[0112] This comparative example provides a method for improving the consistency of electrical performance testing of a sodium ion battery, comprising:
[0113] S1: Assemble LIR2430 button half-cells (5 PCS) in the same manner as in Example 1;
[0114] S2: On the blue battery test cabinet, connect the positive and negative electrodes with a snap-on clamp and let it stand for 12 hours to ensure that the electrolyte infiltrates the electrode material;
[0115] S3: Set the capacity test process, 0.1C constant current discharge, 0V cut-off; 0.09C discharge, 0V cut-off; 0.08C constant current discharge, 0V cut-off; 0.07C constant current discharge, 0V cut-off; 0.06C constant current discharge, 0V cut-off; 0.05C constant current discharge, 0V cut-off; 0.04C constant current discharge, 0V cut-off; 0.03C constant current discharge, 0V cut-off; 0.02C constant current discharge, 0V cut-off; 0.01C constant current discharge, 0V cut-off; 0.1C charge, 2V cut-off;
[0116] S4: Start the test program of S3, output the data after the test is completed, and draw the data curve;
[0117] Repeat the above steps 5 times in total, and draw the data curve of the 5 times as shown in Figure 6 shown.
[0118] Comparative Example 3
[0119] This comparative example provides a method for improving the consistency of electrical performance testing of sodium ion batteries, which is different from Example 1 in that the cut-off voltage of this comparative example is 2.95V, and other conditions are the same.
[0120] Comparative Example 4
[0121] This comparative example provides a method for improving the consistency of electrical performance testing of sodium ion batteries, which is different from Example 1 in that the cutoff current of this comparative example is 5 μA, and other conditions are the same.
[0122] The test results of the gram capacity fluctuation range of the above embodiments and comparative examples are shown in Table 1.
[0123] Table 1 Gram capacity test results
[0124]
[0125]
[0126] As can be seen from Table 1, the fluctuation range of the gram capacity of Examples 1-5 is reduced to within 8 mAh, and the experimental results have good consistency.
[0127] In comparative example 1, the constant current charging current is 0.030mA, the consistency of the experimental results is reduced, and the gram capacity fluctuates by 15mAh. The reason is that the parameters are improperly controlled, and the current density of the constant current charging is too large, resulting in residual sodium oxide that cannot be removed, affecting the consistency of the experimental results.
[0128] In Comparative Example 2, the sodium sheet was not subjected to electro-deoxidation treatment, so the fluctuation range of gram capacity was significantly larger than that of Examples 1-5, and the consistency of the experimental results was poor.
[0129] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0130] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for improving the consistency of electrical performance testing of sodium ion batteries, characterized in that: include: For sodium ion batteries, an electrical deoxidation process is set up before the electrical performance test process; The electrical deoxidation process includes firstly performing constant current charging until the cut-off voltage is greater than the open circuit potential, and then performing constant voltage charging until the cut-off current is obtained.
2. The method for improving the electrical performance test consistency of a sodium ion battery according to claim 1, characterized in that: The constant current charging current is 0.010mA-0.020mA.
3. The method for improving the electrical performance test consistency of a sodium ion battery according to claim 1, characterized in that: The cut-off voltage is greater than the open circuit potential by 0.1V-0.2V.
4. The method for improving the electrical performance test consistency of a sodium ion battery according to claim 1, characterized in that: The open circuit potential is 2.6V-2.9V.
5. The method for improving the electrical performance test consistency of a sodium ion battery according to claim 1, characterized in that: The cut-off current is 1 μA-3 μA.
6. The method for improving the electrical performance test consistency of a sodium ion battery according to claim 1, characterized in that: The sodium ion battery is also allowed to stand before the electrical deoxidation step.
7. The method for improving the electrical performance test consistency of a sodium ion battery according to claim 6, characterized in that: The standing time is greater than or equal to 12 hours.
8. The method for improving the electrical performance test consistency of a sodium ion battery according to claim 1, characterized in that: The sodium ion battery comprises a button cell.
9. The method for improving the consistency of electrical performance testing of a sodium ion battery according to any one of claims 1 to 8, characterized in that: The electrical performance testing process includes a capacity testing process and a cycle testing process.
10. The method for improving the electrical performance test consistency of a sodium ion battery according to claim 9, characterized in that: During the capacity testing process, the oxygen content in the sodium sheet in the sodium ion battery is 1 ppm-100 ppm.