Diaphragm, negative electrode, lithium / sodium ion battery and preparation method
By setting patterned electronic guide and protective layer in the lithium/sodium separator and negative electrode of lithium/sodium ion battery, the cycle life and energy density of lithium/sodium ion battery is solved, and more efficient lithium/sodium ion is achieved Transmission and lower battery weight and cost.
Patent Information
- Application Number
- CN202411121320.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-15
AI Technical Summary
During the circulation process of existing lithium/sodium ion batteries, there are problems such as transition metal dissolution of cathode active materials, particle breakage, etc., resulting in the decay of the battery cell cycle life and the reduction of energy density, and the existing lithium/sodium supplementation process has by-products. The cycle life is decayed, complicated operation, high risk and high cost.
A patterned electronic conductive layer is provided in the lithium/sodium separator and the negative electrode, and a protective layer isolates the lithium/sodium metal from the air, improves interface contact and electric field distribution, and builds an electronic channel to improve conductivity and lithium/sodium ion transmission efficiency. Reduce inactive lithium/sodium consumption.
It improves the utilization rate of lithium/sodium ions and the energy density of the battery, extends the cycle life of the battery, reduces the production cost and weight of the battery, enhances the electrochemical performance, and adapts to industrial applications.
Smart Images

Figure CN119009375A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of battery technology, and in particular, to a separator, a negative electrode and a lithium / sodium ion battery, and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have advantages such as high specific energy and long cycle life, and are widely used in electronic products, electric vehicles and other fields. However, existing lithium-ion batteries still have problems such as transition metal dissolution and particle breakage of cathode active materials, which in turn lead to technical problems such as battery cell cycle life reduction and energy density reduction. Sodium-ion batteries also face the same technical problems.
[0003] In order to alleviate the above technical problems, the existing technology proposes to pre-lithiate / sodiumize the positive electrode, negative electrode or separator to increase the total amount of active lithium / sodium during the cycle, which not only helps to improve the battery energy density, but also can significantly extend the service life of the battery cell.
[0004] However, the existing positive electrode, negative electrode or diaphragm pre-lithiation / sodium still has at least the following technical problems: the existence of byproducts after the existing positive electrode lithium supplementation reaction will lead to the attenuation of the cycle life, and the lithium supplementation effect is limited. The existing negative electrode lithium / sodium supplementation is still limited by several major problems in the battery manufacturing process: the use of metal lithium / sodium is incompatible with the production environment, conventional solvents, binders, air and heat treatment processes, which makes the negative electrode lithium / sodium supplementation complicated to operate, high in risk, low in metal lithium utilization, and high in humidity requirements for storage and use environments. The existing diaphragm lithium / sodium supplementation is mainly achieved by a lithium / sodium functional layer or a lithium / sodium gel layer, but the lithium / sodium functional coating contains catalysts, conductive agents, etc. The lithium / sodium supplementation through the lithium / sodium functional layer will greatly increase the cost of the lithium / sodium supplementation diaphragm, thereby increasing the production cost of lithium / sodium ion batteries; the lithium / sodium supplementation through the lithium / sodium gel layer containing lithium supplementation will increase the thickness of the diaphragm, and the gel layer is easy to block the micropores of the diaphragm after drying, hindering the transmission of lithium ions.
[0005] Therefore, how to propose a separator, a negative electrode and a lithium / sodium ion battery, as well as a preparation method to solve or at least alleviate at least one of the above technical problems is a problem that needs to be solved urgently. Summary of the invention
[0006] In view of the above technical problems, the present disclosure provides a separator, a negative electrode and a lithium / sodium ion battery, and a preparation method to solve or at least alleviate at least one of the above technical problems existing in the prior art.
[0007] According to a specific embodiment of the present disclosure, in a first aspect, the present disclosure provides a lithium / sodium supplementing diaphragm, comprising:
[0008] Diaphragm layer;
[0009] A first protective layer, disposed on one side of the diaphragm layer;
[0010] A lithium / sodium supplement layer is arranged on a side of the first protective layer away from the diaphragm layer;
[0011] A patterned electron-conducting layer is disposed on a side of the lithium / sodium supplementing layer away from the separator layer; and
[0012] The second protective layer is disposed on a side of the patterned electron conductive layer away from the lithium / sodium supplementing layer.
[0013] Optionally, the pattern of the patterned electron conductive layer includes at least one of a dot shape, a line shape or a surface shape.
[0014] Optionally, the pattern of the patterned electron conductive layer includes at least one of the following shapes: a lattice shape, a plurality of linear structures arranged at intervals, a network structure formed by a plurality of linear structures intersecting each other, or a planar structure formed by at least one linear structure.
[0015] Optionally, the line shape is a straight line, a broken line or a curved line.
[0016] Optionally, the continuity of the patterned electron-conducting layer is 50% to 80%.
[0017] Optionally, the thickness of the patterned electron-conducting layer is 20-100 nm.
[0018] Optionally, the material of the patterned electron-conducting layer includes at least one of a metal material and a carbon material.
[0019] Optionally, the metal material includes at least one of Au, Ag, Cu, Zn, Mg and metal alloys thereof.
[0020] Optionally, the carbon material includes at least one of conductive graphite, conductive carbon black, conductive carbon fiber and graphene.
[0021] Optionally, a component of the first protective layer includes at least one of Na2CO3, NaTiO3, NaF, Na3N, Li2CO3, Li3N, LiTiO3, Li3P, and LiF.
[0022] Optionally, a component of the second protective layer includes at least one of Na2CO3, NaTiO3, NaF, Na3N, Li2CO3, Li3N, LiTiO3, Li3P, and LiF.
[0023] Optionally, the material of the lithium supplement layer includes at least one of metallic lithium, lithium silicon alloy, lithium magnesium alloy, lithium copper alloy, lithium silver alloy, lithium beryllium alloy, lithium zinc alloy, lithium cadmium alloy, lithium aluminum alloy, lithium gold alloy and lithium boron alloy.
[0024] Optionally, the material of the sodium supplement layer includes at least one of metallic sodium, sodium silicon alloy, sodium indium alloy, sodium zinc alloy, sodium phosphorus alloy, sodium arsenic alloy, sodium tin alloy, sodium bismuth alloy, sodium lead alloy, and sodium antimony alloy.
[0025] According to a specific embodiment of the present disclosure, in a second aspect, the present disclosure provides a lithium / sodium supplemented negative electrode, comprising:
[0026] A negative electrode sheet, comprising a negative electrode current collector and a negative electrode active material layer located on at least one surface of the negative electrode current collector;
[0027] The patterned electron conductive layer is arranged on one side or both sides of the negative electrode sheet and is located on the surface of the negative electrode active material layer away from the negative electrode current collector;
[0028] A lithium / sodium supplement layer is disposed on a side of the patterned electron conductive layer away from the negative electrode sheet; and
[0029] The protective layer is arranged on a side of the lithium / sodium supplementing layer away from the patterned electron conducting layer.
[0030] Optionally, the pattern of the patterned electron conductive layer includes at least one of a dot shape, a line shape or a surface shape.
[0031] Optionally, the dot shape includes a dot matrix shape formed by a plurality of discontinuous dots.
[0032] Optionally, the line shape comprises a plurality of lines arranged at intervals.
[0033] Optionally, the planar shape includes a network structure formed by a plurality of lines intersecting each other, and / or a planar structure formed by at least one line enclosing each other.
[0034] Optionally, the line shape is a straight line, a broken line or a curved line.
[0035] Optionally, the continuity of the patterned electron-conducting layer is 50% to 80%.
[0036] Optionally, the thickness of the patterned electron-conducting layer is 20-100 nm.
[0037] Optionally, the material of the patterned electron-conducting layer includes at least one of a metal material and a carbon material.
[0038] Optionally, the metal material includes at least one of Au, Ag, Cu, Zn, Mg and metal alloys thereof.
[0039] Optionally, the carbon material includes at least one of conductive graphite, conductive carbon black, conductive carbon fiber and graphene.
[0040] Optionally, the component of the protective layer includes at least one of Na2CO3, NaTiO3, NaF, Na3N, Li2CO3, Li3N, LiTiO3, Li3P, and LiF.
[0041] Optionally, the material of the lithium supplement layer includes at least one of metallic lithium, lithium silicon alloy, lithium magnesium alloy, lithium copper alloy, lithium silver alloy, lithium beryllium alloy, lithium zinc alloy, lithium cadmium alloy, lithium aluminum alloy, lithium gold alloy and lithium boron alloy.
[0042] Optionally, the material of the sodium supplement layer includes at least one of metallic sodium, sodium silicon alloy, sodium indium alloy, sodium zinc alloy, sodium phosphorus alloy, sodium arsenic alloy, sodium tin alloy, sodium bismuth alloy, sodium lead alloy, and sodium antimony alloy.
[0043] According to a specific embodiment of the present disclosure, in a third aspect, the present disclosure provides a lithium / sodium ion battery, comprising a positive electrode, a negative electrode and a separator, wherein the separator is arranged between the positive electrode and the negative electrode, and the separator is any one of the lithium / sodium supplementing separators described above; and / or the negative electrode is any one of the lithium / sodium supplementing negative electrodes described above.
[0044] According to a specific embodiment of the present disclosure, in a fourth aspect, the present disclosure provides a method for preparing any lithium / sodium supplementing diaphragm as described above, comprising the following steps:
[0045] depositing a first protective layer on one side of the diaphragm layer;
[0046] Depositing a lithium / sodium supplement layer on a side of the first protective layer away from the separator layer;
[0047] A shielding plate with a hollow pattern is designed, and the shielding plate with the hollow pattern is installed on the side of the lithium / sodium supplement layer away from the diaphragm layer. After the evaporation source evaporates, it passes through the shielding plate with the hollow pattern and is deposited on the side of the lithium / sodium supplement layer away from the diaphragm layer to form a patterned electron conductive layer;
[0048] The shielding plate with the hollow pattern is removed, and a second protective layer is deposited on a side of the patterned electron conductive layer away from the lithium / sodium supplementing layer.
[0049] Optionally, a method for depositing the first protective layer on one side of the diaphragm layer is vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering.
[0050] Optionally, the method of depositing the lithium / sodium supplementing layer on the side of the first protective layer away from the diaphragm layer is vacuum evaporation or magnetron sputtering.
[0051] Optionally, a method for forming a patterned electronic conductive layer on a side of the lithium / sodium supplementing layer away from the separator layer is vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering.
[0052] Optionally, the method of depositing the second protective layer on the side of the patterned electronic conductive layer away from the lithium / sodium supplementing layer is vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering.
[0053] According to a specific embodiment of the present disclosure, in a fifth aspect, the present disclosure provides a method for preparing any of the lithium / sodium supplemented negative electrodes as described above, comprising the following steps:
[0054] A shielding plate with a hollow pattern is designed, and the shielding plate with the hollow pattern is installed on one side of the negative electrode sheet. After the evaporation source evaporates, it passes through the shielding plate with the hollow pattern and is deposited on the surface of the negative electrode active material layer of the negative electrode sheet to form a patterned electron conductive layer;
[0055] The shielding plate with the hollow pattern is removed, and a lithium / sodium supplement layer is deposited on the side of the patterned electron conductive layer away from the negative electrode sheet;
[0056] A protective layer is deposited on a side of the lithium / sodium supplementing layer away from the patterned electron conducting layer.
[0057] Optionally, the method of depositing the patterned electron conductive layer on the surface of the negative electrode active material layer of the negative electrode sheet is vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering.
[0058] Optionally, the method of depositing the lithium / sodium supplementing layer on the side of the patterned electron conductive layer away from the negative electrode sheet is vacuum evaporation or magnetron sputtering.
[0059] Optionally, the protective layer is deposited on the side of the lithium / sodium supplementing layer away from the patterned electronic conductive layer by vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering.
[0060] According to a specific embodiment of the present disclosure, in a sixth aspect, the present disclosure provides a method for preparing a lithium / sodium ion battery, comprising the following steps:
[0061] Providing a positive electrode, a separator and a negative electrode, wherein the separator is obtained by using any of the above-mentioned methods for preparing a lithium / sodium supplemented separator, or the negative electrode is obtained by using any of the above-mentioned methods for preparing a lithium / sodium supplemented negative electrode;
[0062] The separator is arranged between the positive electrode and the negative electrode, and the positive electrode, the separator and the negative electrode are placed in a shell, and the shell is sealed after the electrolyte is injected into the shell.
[0063] Compared with the prior art, the above solution of the embodiment of the present disclosure has at least the following beneficial effects:
[0064] (1) The present invention provides a patterned electron conductive layer on one side of the lithium / sodium supplement layer in the lithium / sodium supplement separator, and provides a patterned electron conductive layer between the negative electrode sheet and the lithium / sodium supplement layer in the lithium / sodium supplement negative electrode, thereby improving the interface contact and uniformizing the interface electric field distribution; and constructing electron channels in the separator and the negative electrode respectively through the patterned electron conductive layer, which helps to improve the conductivity and lithium ion transmission efficiency of the battery, realize the improvement of the lithium / sodium utilization rate in the lithium / sodium supplement layer, reduce the consumption of inactive lithium / sodium in the battery cell system, and thus achieve the purpose of improving energy density, cycle life and rate performance.
[0065] (2) The present disclosure can control the morphology, continuity and composition of the patterned electronic conductive layer to make the lithium / sodium ions in the lithium / sodium supplement layer more orderly and faster to be transported, thereby improving the lithium / sodium ion conduction efficiency, regulating the distribution uniformity of lithium / sodium ions, and avoiding excessive aggregation or sparseness of lithium ions in local areas. It can significantly enhance the electronic conduction capacity of the lithium / sodium layer, improve the utilization rate of the metal lithium / sodium layer, reduce the consumption of inactive lithium / sodium in the battery system, and thus improve the energy density and electrochemical performance of the battery.
[0066] (3) The present disclosure provides a protective layer to isolate the lithium / sodium metal in the lithium / sodium supplement layer in the diaphragm and the negative electrode from water, gas, etc. in the air, thereby preventing the lithium / sodium from being consumed by water, gas, etc. in the air during the assembly process of the lithium / sodium supplement diaphragm and the lithium / sodium supplement negative electrode, thereby affecting the lithium / sodium supplement efficiency. The lithium / sodium supplement diaphragm and lithium / sodium supplement negative electrode disclosed in the present disclosure can adapt to the assembly environment of lithium / sodium ion batteries and reduce the limitations of industrial applications. Moreover, providing a protective layer on the surface of the diaphragm layer can also prevent lithium / sodium, etc. from entering the micropores of the diaphragm layer during the evaporation process, blocking the micropores of the diaphragm and hindering the transmission of lithium ions.
[0067] (4) The patterned electron conductive layer of the present invention is stacked with the second protective layer. The patterned electron conductive layer does not penetrate the second protective layer. Therefore, the thickness of the patterned electron conductive layer is not limited by the thickness of the outermost second protective layer. The thickness of the patterned electron conductive layer can be selected in a wider range; and the protection effect on lithium / sodium metal can also be enhanced.
[0068] (5) The thickness of the patterned electron-conducting layer, lithium / sodium supplementing layer, and protective layer disclosed in the present invention are relatively small, and the increase in thickness of the separator and the negative electrode is basically negligible, so the weight and volume of the battery will not be significantly increased.
[0069] (6) The preparation method of the lithium / sodium supplemented diaphragm and the lithium / sodium supplemented negative electrode disclosed in the present invention is simple, has low requirements on the temperature and humidity of the environment, is highly safe, and has low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] The drawings herein are incorporated into the specification and constitute a part of the specification, showing embodiments consistent with the present disclosure, and together with the specification, are used to explain the principles of the present disclosure. Obviously, the drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the drawings:
[0071] Figure 1 It is a schematic structural diagram of the lithium / sodium supplementing diaphragm in the first embodiment of the present disclosure;
[0072] Figure 2 This is a schematic diagram of a structure in which a patterned electron-conducting layer is in a lattice shape in some embodiments of the present disclosure;
[0073] Figure 3 A schematic diagram of a linear structure in which a patterned electron-conducting layer is formed by a plurality of lines arranged at intervals in some embodiments of the present disclosure;
[0074] Figure 4 A schematic diagram of a network structure in which a patterned electron-conducting layer is formed by a plurality of cross-line arrangements in some embodiments of the present disclosure;
[0075] Figure 5 A schematic diagram of a structure in which a patterned electron-conducting layer is a planar structure formed by at least one line in some embodiments of the present disclosure;
[0076] Figure 6 A flow chart of a method for preparing a lithium / sodium supplementing diaphragm provided in a second embodiment of the present disclosure;
[0077] Figure 7 A schematic diagram of the structure of a lithium / sodium supplemented negative electrode provided in the third embodiment of the present disclosure;
[0078] Figure 8 A schematic diagram of the structure of a lithium / sodium supplemented negative electrode provided in some embodiments of the present disclosure;
[0079] Fig. 9 This is a flow chart of a method for preparing a lithium / sodium supplemented negative electrode provided in a fourth embodiment of the present disclosure;
[0080] Fig.10 It is a schematic structural diagram of a lithium / sodium ion battery provided in a fifth embodiment of the present disclosure;
[0081] Fig.11 A flow chart of a method for preparing a lithium / sodium ion battery provided in the sixth embodiment of the present disclosure.
[0082] The reference numerals in the specific implementation manner are as follows:
[0083] Lithium / sodium ion battery 100;
[0084] Lithium / sodium supplementing membrane 10, membrane layer 11, first protective layer 12, lithium / sodium supplementing layer 13, patterned electron conductive layer 14, second protective layer 15; lithium / sodium supplementing negative electrode 20, negative electrode sheet 21, patterned electron conductive layer 22, lithium / sodium supplementing layer 23, protective layer 24; positive electrode 30; negative electrode 40. DETAILED DESCRIPTION
[0085] In order to make the purpose, technical solutions and advantages of the present disclosure clearer, the present disclosure will be further described in detail below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.
[0086] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure.
[0087] It should also be noted that the term "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, so that a commodity or device comprising a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprising a" do not exclude the presence of other identical elements in the commodity or device comprising the elements.
[0088] In the description of the embodiments of the present disclosure, the terms "upper", "lower", "thickness", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present disclosure and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present disclosure.
[0089] In the description of the embodiments of the present disclosure, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0090] In the description of the embodiments of the present disclosure, the symbol “~” represents the two endpoint data before and after the “~” and all data between the two endpoints. For example, A~B represents all data greater than or equal to A and less than or equal to B.
[0091] In the description of the embodiments of the present disclosure, the terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present disclosure, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0092] Reference to "embodiments" in this disclosure means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the disclosure. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this disclosure may be combined with other embodiments.
[0093] The existing technology proposes to pre-lithiate / sodiumize the positive electrode, negative electrode or separator to increase the total amount of active lithium / sodium during the cycle, which not only helps to improve the battery energy density, but also can significantly extend the service life of the battery cell.
[0094] However, the inventors have found through research that the existing positive electrode, negative electrode or diaphragm pre-lithiation / sodium still has at least the following technical problems: the presence of byproducts after the existing positive electrode lithium supplementation reaction will lead to the attenuation of the cycle life, and the lithium supplementation effect is limited. The existing negative electrode lithium / sodium supplementation is still limited by several major problems in the battery manufacturing process: the use of metal lithium / sodium is incompatible with the production environment, conventional solvents, binders, air and heat treatment processes, which makes the negative electrode lithium / sodium supplementation complicated to operate, high in risk, low in metal lithium utilization, and high in humidity requirements for storage and use environments. The existing diaphragm lithium / sodium supplementation is mainly achieved by a lithium / sodium functional layer or a lithium / sodium gel layer, but the lithium / sodium functional coating contains catalysts, conductive agents, etc., and the lithium / sodium supplementation through the lithium / sodium functional layer will greatly increase the cost of the lithium / sodium supplementation diaphragm, thereby increasing the production cost of lithium / sodium ion batteries; the lithium / sodium supplementation by coating a lithium-containing lithium / sodium gel layer will increase the thickness of the diaphragm, and the gel layer is easy to block the micropores of the diaphragm after drying, hindering the transmission of lithium ions.
[0095] In order to solve the above technical problems, the present invention provides a patterned electronic conductive layer on one side of the lithium / sodium supplement layer in the lithium / sodium supplement membrane, and provides a patterned electronic conductive layer between the negative electrode sheet and the lithium / sodium supplement layer in the lithium / sodium supplement negative electrode, so as to improve the interface contact and homogenize the interface electric field distribution, and can construct electronic channels in the membrane and the negative electrode respectively, which is helpful to improve the conductivity and lithium ion transmission efficiency of the battery, realize the improvement of the lithium / sodium utilization rate in the lithium / sodium supplement layer, and further realize the purpose of improving the energy density, cycle life and rate performance.
[0096] Specifically, an embodiment of the present disclosure provides a lithium / sodium supplementing diaphragm, comprising: a diaphragm layer; a first protective layer, arranged on one side of the diaphragm layer; a lithium / sodium supplementing layer, arranged on a side of the first protective layer away from the diaphragm layer; a patterned electronic conductive layer, arranged on a side of the lithium / sodium supplementing layer away from the diaphragm layer; and a second protective layer, arranged on a side of the patterned electronic conductive layer away from the lithium / sodium supplementing layer.
[0097] The disclosed embodiments also provide a lithium / sodium supplemented negative electrode, comprising: a negative electrode sheet, comprising a negative electrode current collector and a negative electrode active material layer located on at least one surface of the negative electrode current collector; a patterned electron conductive layer, arranged on one side or both sides of the negative electrode sheet and located on the surface of the negative electrode active material layer away from the negative electrode current collector; a lithium / sodium supplemented layer, arranged on a side of the patterned electron conductive layer away from the negative electrode sheet; and a protective layer, arranged on a side of the lithium / sodium supplemented layer away from the patterned electron conductive layer.
[0098] In the technical solution disclosed in the present invention, a patterned electronic conductive layer is provided on one side of the lithium / sodium supplement layer in the lithium / sodium supplement diaphragm, and a patterned electronic conductive layer is provided between the negative electrode sheet and the lithium / sodium supplement layer in the lithium / sodium supplement negative electrode, so as to improve the interface contact and uniformize the interface electric field distribution; and by controlling the morphology of the patterned electronic conductive layer, an electronic channel can be constructed in the diaphragm and the negative electrode respectively, which helps to improve the conductivity and lithium ion transmission efficiency of the battery, realize the improvement of the lithium / sodium utilization rate in the lithium / sodium supplement layer, reduce the consumption of inactive lithium / sodium in the battery core system, and thus achieve the purpose of improving energy density, cycle life and rate performance. Moreover, the lithium / sodium ions in the lithium / sodium supplement layer can be transmitted more orderly and faster, the lithium / sodium ion conduction efficiency can be improved, the distribution uniformity of lithium / sodium ions can be regulated, and the excessive aggregation or sparseness of lithium ions in local areas can be avoided. By controlling the continuity of the patterned electronic conductive layer, the conductivity and lithium ion transmission properties are both relatively high. By providing a protective layer, the lithium / sodium metal in the lithium / sodium supplement layer of the separator and the negative electrode is isolated from water, gas, etc. in the air, so as to avoid the lithium / sodium being consumed by water, gas, etc. in the air during the assembly process of the lithium / sodium supplement separator, which affects the efficiency of lithium / sodium supplement. In addition, the patterned electronic conductive layer is stacked with the second protective layer, and the patterned electronic conductive layer does not penetrate the second protective layer. Therefore, the thickness of the patterned electronic conductive layer is not limited to the thickness of the outermost second protective layer, and the thickness of the patterned electronic conductive layer can be selected in a wider range; and the protection effect on lithium / sodium metal can also be enhanced.
[0099] The optional embodiments of the present disclosure are described in detail below with reference to the accompanying drawings.
[0100] See also Figure 1The first embodiment of the present disclosure provides a lithium / sodium supplementing membrane 10, comprising: a membrane layer 11, a first protective layer 12, a lithium / sodium supplementing layer 13, a patterned electron conductive layer 14, and a second protective layer 15. The first protective layer 12 is disposed on the surface of the membrane layer 11, the lithium / sodium supplementing layer 13 is disposed on a side of the first protective layer 12 away from the membrane layer 11, the patterned electron conductive layer 14 is disposed on a side of the lithium / sodium supplementing layer 13 away from the membrane layer 11, and the second protective layer 15 is disposed on a side of the patterned electron conductive layer 14 away from the lithium / sodium supplementing layer 13.
[0101] The diaphragm layer 11 can be selected from conventional diaphragms in lithium / sodium ion batteries. As an example, the diaphragm layer 11 includes but is not limited to polyolefin diaphragms such as polyethylene and polypropylene or polypyrrole nanomaterial diaphragms, and the diaphragm surface may also include inorganic and organic coatings such as aluminum oxide and polyvinylidene fluoride.
[0102] The first protective layer 12 and the second protective layer 15 isolate the lithium / sodium metal of the lithium / sodium supplement layer 13 from water, gas, etc. in the air, so as to prevent the lithium / sodium from being consumed by water, gas, etc. in the air during the assembly process of the lithium / sodium supplement membrane, thereby affecting the efficiency of lithium / sodium supplementation. The components of the first protective layer 12 and / or the second protective layer 15 include but are not limited to at least one of lithium / sodium salts such as Na2CO3, NaTiO3, NaF, Na3N, Li2CO3, Li3N, LiTiO3, Li3P, and LiF.
[0103] The thickness of the first protective layer 12 and / or the second protective layer 15 is preferably in the range of 20 nm to 5 μm. The thickness of the second protective layer 15 may be the same as or different from that of the first protective layer 12 . Preferably, the thickness of the second protective layer 15 is greater than that of the first protective layer 12 .
[0104] When the diaphragm is a lithium-supplemented diaphragm, the material of the lithium-supplemented layer 2 includes, but is not limited to, one or more of metallic lithium, lithium-silicon alloy, lithium-magnesium alloy, lithium-copper alloy, lithium-silver alloy, lithium-beryllium alloy, lithium-zinc alloy, lithium-cadmium alloy, lithium-aluminum alloy, lithium-gold alloy, and lithium-boron alloy. When the diaphragm is a sodium-supplemented diaphragm, the material of the sodium-supplemented layer 2 includes, but is not limited to, at least one of metallic sodium, sodium-silicon alloy, sodium-indium alloy, sodium-zinc alloy, sodium-phosphorus alloy, sodium-arsenic alloy, sodium-tin alloy, sodium-bismuth alloy, sodium-lead alloy, and sodium-antimony alloy.
[0105] In some embodiments, the thickness of the lithium / sodium supplement layer 13 is 50 nm to 10 μm. Preferably, the thickness of the lithium / sodium supplement layer 13 is 500 nm to 3 μm.
[0106] The pattern of the patterned electron conductive layer 14 may be in the form of dots, lines or surfaces. Preferably, the pattern of the patterned electron conductive layer 14 is in the form of dots or surfaces. The lines may be straight lines, broken lines or curves. For example, the surfaces include but are not limited to squares, diamonds, trapezoids, triangles, polygons, crosses, rings or irregular shapes. Figure 2-5 In some embodiments, the point shape includes a dot matrix formed by multiple discontinuous points; the line shape includes a plurality of spaced lines; the surface shape includes a network structure formed by a plurality of crossed lines, and / or a surface structure formed by at least one line.
[0107] The percentage of the area of the conductive material in the patterned electronic conductive layer 14 to the upper surface area of the diaphragm layer 11 is referred to as continuity. If the continuity of the patterned electronic conductive layer 14 is too low, for example, less than 50%, the conductivity of the patterned electronic conductive layer 14 is weak, and if the continuity is too high, for example, higher than 80%, it will hinder the transmission of lithium / sodium ions. In some preferred embodiments, the continuity of the patterned electronic conductive layer 14 is 50% to 80%, and the patterned electronic conductive layer 14 within this continuity range has both good conductivity and lithium / sodium ion transport properties. In some embodiments, the thickness of the patterned electronic conductive layer 14 is 20 to 100 nm.
[0108] The material of the patterned electron-conducting layer 14 includes at least one of a metal material and a carbon material. The metal material includes, but is not limited to, Au, Ag, Cu, Zn, Mg, etc., or an alloy of two or more of the above metals. Preferably, the metal material is Ag, Cu or Ag-Cu alloy. The carbon material includes, but is not limited to, at least one of conductive graphite, conductive carbon black, conductive carbon fiber and graphene, etc., and preferably, the carbon material is conductive graphite or conductive carbon black.
[0109] By controlling the morphology, continuity and composition of the patterned electron-conducting layer 14 to construct an electron channel, the electron conduction capacity of the lithium / sodium layer can be significantly enhanced, the utilization rate of the metal lithium / sodium layer can be improved, and the consumption of inactive lithium / sodium in the battery system can be reduced, thereby improving the energy density and electrochemical performance of the battery.
[0110] See also Figure 6 The second embodiment of the present disclosure provides a method for preparing the lithium / sodium supplementing membrane 10 described in any one of the first embodiments, comprising the following steps:
[0111] Step (S1), depositing the first protective layer 12 on one side of the diaphragm layer 11;
[0112] Step (S2), depositing the lithium / sodium supplementing layer 13 on the side of the first protective layer 12 away from the diaphragm layer 11;
[0113] Step (S3), designing a shielding plate with a hollow pattern, installing the shielding plate with the hollow pattern on the side of the lithium / sodium supplement layer 13 away from the diaphragm layer 11, and after evaporation, the evaporation source passes through the shielding plate with the hollow pattern to deposit on the side of the lithium / sodium supplement layer 13 away from the diaphragm layer 11 to form the patterned electron conductive layer 14;
[0114] Step (S4), removing the shielding plate with the hollow pattern, and depositing the second protective layer 15 on the side of the patterned electron conductive layer 14 away from the lithium / sodium supplementing layer 13.
[0115] In some embodiments, in step (S1), the deposition method of the first protective layer 12 includes but is not limited to vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering, etc. Preferably, the first protective layer 12 is deposited on one side of the diaphragm layer 11 by vacuum evaporation.
[0116] In some embodiments, in step (S2), the lithium / sodium supplement layer 2 is formed on one side of the first protective layer 12 by vacuum evaporation or magnetron sputtering.
[0117] In step (S3), the shielding plate with a hollow pattern is used to partially shield the lithium / sodium supplement layer 13, thereby forming a patterned electron conductive layer 14 on the surface of the lithium / sodium supplement layer 13, and the pattern of the patterned electron conductive layer 14 is the same as the hollow pattern of the shielding plate.
[0118] In some embodiments, the method for forming the patterned electronic conductive layer 14 on one side of the lithium / sodium supplement layer 13 includes but is not limited to at least one of vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering. Preferably, the patterned electronic conductive layer 14 is formed on the surface of the lithium / sodium supplement layer 13 by vacuum evaporation. Specifically, a corresponding shielding plate with a hollow pattern is designed according to the morphology of the patterned electronic conductive layer 14, and then the shielding plate with a hollow pattern is introduced to the side of the lithium / sodium supplement layer 2 away from the diaphragm layer 11, and then the metal or carbon material is evaporated onto the lithium / sodium supplement layer 2 by vacuum evaporation to form the patterned electronic conductive layer 14.
[0119] In some embodiments, in step (S4), the second protective layer 15 is deposited on the side of the patterned electronic conductive layer 14 away from the lithium / sodium supplementing layer 13, including but not limited to vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering, etc. Preferably, the second protective layer 15 is deposited on the side of the patterned electronic conductive layer 14 away from the lithium / sodium supplementing layer 13 by vacuum evaporation.
[0120] See also Figure 7, the third embodiment of the present disclosure provides a lithium / sodium supplemented negative electrode 20, comprising: a negative electrode sheet 21, a patterned electronic conductive layer 22, a lithium / sodium supplemented layer 23 and a protective layer 24. The negative electrode sheet 21 comprises a negative electrode current collector and a negative electrode active material layer located on the surface of the negative electrode current collector, the patterned electronic conductive layer 22 is arranged on both sides of the negative electrode sheet 21, and is located on the surface of the negative electrode active material layer away from the negative electrode current collector, the lithium / sodium supplemented layer 23 is arranged on the side of the patterned electronic conductive layer 22 away from the negative electrode sheet 21, and the protective layer 24 is arranged on the side of the lithium / sodium supplemented layer 23 away from the patterned electronic conductive layer 22. That is, in this embodiment, the lithium / sodium supplemented negative electrode 20 comprises a protective layer 24, a lithium / sodium supplemented layer 23, a patterned electronic conductive layer 22, a negative electrode sheet 21, a patterned electronic conductive layer 22, a lithium / sodium supplemented layer 23 and a protective layer 24 which are stacked in sequence.
[0121] The negative electrode sheet 21 includes a negative electrode current collector and a negative electrode active material. The negative electrode active material is located on at least one surface of the negative electrode current collector. The negative electrode active material includes but is not limited to at least one of graphite, hard carbon, soft carbon, intermediate carbon microspheres, tin-based, and silicon-based materials.
[0122] The pattern of the patterned electron conductive layer 22 may be dot-shaped, line-shaped or surface-shaped. Preferably, the pattern of the patterned electron conductive layer 22 is dot-shaped or surface-shaped. The line-shaped may be a straight line, a broken line or a curve, etc. As an example, the surface-shaped includes but is not limited to a square, a rhombus, a trapezoid, a triangle, a polygon, a cross, a circular ring or an irregular shape, etc. In some embodiments, the dot-shaped includes a dot-shaped structure formed by a plurality of discontinuous points; the line-shaped includes a plurality of spaced lines; the surface-shaped includes a network structure formed by a plurality of lines intersecting and arranged, and / or a surface structure formed by at least one line enclosing.
[0123] The percentage of the area of the conductive material in the patterned electronic conductive layer 22 to the upper surface area of the negative electrode sheet 21 is referred to as continuity. If the continuity of the patterned electronic conductive layer 22 is too low, for example, less than 50%, the conductivity of the patterned electronic conductive layer 22 is weak. If the continuity is too high, for example, higher than 80%, it will hinder the transmission of lithium / sodium ions. In some preferred embodiments, the continuity of the patterned electronic conductive layer 22 is 50% to 80%, and the patterned electronic conductive layer 22 within this continuity range has both good conductivity and lithium / sodium ion transport properties. In some embodiments, the thickness of the patterned electronic conductive layer 22 is 20 to 100 nm.
[0124] The material of the patterned electron-conducting layer 22 includes at least one of a metal material and a carbon material. The metal material includes, but is not limited to, Au, Ag, Cu, Zn, Mg, etc., or an alloy of two or more of the above metals. Preferably, the metal material is Ag, Cu or Ag-Cu alloy. The carbon material includes, but is not limited to, at least one of conductive graphite, conductive carbon black, conductive carbon fiber and graphene, etc., and preferably, the carbon material is conductive graphite or conductive carbon black.
[0125] By controlling the morphology, continuity and composition of the patterned electron-conducting layer 22 to construct an electron channel, the electron conduction capacity of the lithium / sodium layer can be significantly enhanced, the utilization rate of the metal lithium / sodium layer can be improved, and the consumption of inactive lithium / sodium in the battery system can be reduced, thereby improving the energy density and electrochemical performance of the battery.
[0126] When the negative electrode is a lithium-supplemented negative electrode, the material of the lithium-supplemented layer 23 includes but is not limited to one or more of metallic lithium, lithium-silicon alloy, lithium-magnesium alloy, lithium-copper alloy, lithium-silver alloy, lithium-beryllium alloy, lithium-zinc alloy, lithium-cadmium alloy, lithium-aluminum alloy, lithium-gold alloy and lithium-boron alloy. When the negative electrode separator is a sodium-supplemented negative electrode, the material of the sodium-supplemented layer 23 includes but is not limited to at least one of metallic sodium, sodium-silicon alloy, sodium-indium alloy, sodium-zinc alloy, sodium-phosphorus alloy, sodium-arsenic alloy, sodium-tin alloy, sodium-bismuth alloy, sodium-lead alloy and sodium-antimony alloy.
[0127] In some embodiments, the thickness of the lithium / sodium supplement layer 23 is 50 nm to 10 μm. Preferably, the thickness of the lithium / sodium supplement layer 23 is 500 nm to 3 μm.
[0128] The protective layer 24 is used to protect the lithium / sodium supplement layer 23, so that the lithium / sodium metal of the lithium / sodium supplement layer 13 is isolated from water, gas, etc. in the air, to prevent the lithium / sodium from being consumed by water, gas, etc. in the air during the assembly process of the lithium / sodium supplement membrane, thereby affecting the lithium / sodium supplement efficiency. The components of the protective layer 24 include but are not limited to at least one of Na2CO3, NaTiO3, NaF, Na3N, Li2CO3, Li3N, LiTiO3, Li3P, LiF and other lithium / sodium salts. The thickness of the protective layer 24 is preferably in the range of 20nm to 5μm.
[0129] See also Figure 8 In some embodiments, the patterned electron conductive layer 22 is only disposed on one side of the negative electrode sheet 21 , and the lithium / sodium supplemented negative electrode 20 includes a negative electrode sheet 21 , a patterned electron conductive layer 22 , a lithium / sodium supplemented layer 23 and a protective layer 24 which are stacked in sequence.
[0130] See also Fig. 9 The fourth embodiment of the present disclosure provides a method for preparing the lithium / sodium supplemented negative electrode 20 described in any one of the third embodiments, comprising the following steps:
[0131] Step (I), designing a shielding plate with a hollow pattern, installing the shielding plate with the hollow pattern on one side of the negative electrode sheet 21, and evaporating the evaporation source through the shielding plate with the hollow pattern to form the patterned electron conductive layer 22 on the surface of the negative electrode active material layer of the negative electrode sheet 21;
[0132] Step (II), removing the shielding plate with the hollow pattern, and depositing the lithium / sodium supplementing layer 23 on the side of the patterned electron conductive layer away from the negative electrode sheet 21;
[0133] Step (III) depositing a protective layer 24 on a side of the lithium / sodium supplementing layer 23 away from the patterned electron conducting layer 22 .
[0134] In some embodiments, in step (I), the shielding plate with a hollow pattern is used to shield part of the surface of the negative electrode sheet 21, so that a patterned electron conductive layer 22 can be formed on one side or both sides of the negative electrode sheet 21. In some embodiments, the method for forming a patterned electron conductive layer 22 on at least one side of the negative electrode sheet 21 includes but is not limited to vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering. Preferably, a patterned electron conductive layer 22 is formed on at least one side of the negative electrode sheet 21 by vacuum evaporation. Specifically, a corresponding shielding plate with a hollow pattern is designed according to the morphology of the patterned electron conductive layer 22, and then the shielding plate with a hollow pattern is installed in the working position, and then the metal or carbon material is evaporated onto one side or both sides of the negative electrode sheet 21 by vacuum evaporation to form a patterned electron conductive layer 14.
[0135] In some embodiments, in step (II), the lithium / sodium supplement layer 23 is deposited on the side of the patterned electron conductive layer 22 away from the negative electrode sheet 21 by vacuum evaporation or magnetron sputtering.
[0136] In some embodiments, in step (III), the method of depositing the protective layer 24 on the side of the lithium / sodium supplementing layer 23 away from the patterned electronic conductive layer 22 includes but is not limited to vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering, etc. Preferably, the protective layer 24 is deposited on the side of the lithium / sodium supplementing layer 23 away from the patterned electronic conductive layer 22 by vacuum evaporation.
[0137] A fifth embodiment of the present disclosure provides a lithium / sodium ion battery, comprising a positive electrode, a negative electrode and a separator, wherein the separator is arranged between the positive electrode and the negative electrode, the separator is the lithium / sodium supplementing separator 10 described in any one of the first embodiments, and / or the negative electrode is the lithium / sodium supplementing negative electrode 20 described in any one of the third embodiments.
[0138] See also Fig.10In some embodiments, the lithium / sodium ion battery 100 includes a positive electrode 30, a negative electrode 40 and a lithium / sodium supplementing membrane 10, wherein the lithium / sodium supplementing membrane 10 is located between the positive electrode 30 and the negative electrode 40, and the second protective layer 15 is close to the negative electrode 40, and the membrane layer 11 is close to the positive electrode 30.
[0139] See also Fig.11 The sixth embodiment of the present disclosure also provides a method for preparing a lithium / sodium ion battery, comprising the following steps:
[0140] Providing a positive electrode, a separator and a negative electrode, wherein the separator is obtained by the preparation method of the lithium / sodium supplemented separator described in the second embodiment, or the negative electrode is obtained by the preparation method of the lithium / sodium supplemented negative electrode described in the fourth embodiment;
[0141] The separator is arranged between the positive electrode and the negative electrode, and the positive electrode, the separator and the negative electrode are placed in a shell, and the shell is sealed after the electrolyte is injected into the shell.
[0142] The preparation process, test methods and test data of the embodiments and comparative examples are introduced below:
[0143] Embodiment 1:
[0144] The lithium supplementing diaphragm of this embodiment includes a diaphragm layer 11, a first protective layer 12, a lithium supplementing layer 12, a patterned electron conductive layer 14 and a second protective layer 15 in sequence. Among them, the diaphragm layer 11 is a polypropylene (PP) diaphragm layer, the lithium supplementing layer 12 is a metal lithium layer, the patterned electron conductive layer 14 is a lattice-shaped metal copper layer, and the first protective layer 12 and the second protective layer 15 are Li2CO3 layers of different thicknesses. The preparation method includes the following steps:
[0145] Start the vacuum evaporation coating equipment and adjust the working vacuum degree to 5×10 -2 Pa~5×10 -3 Pa, start the evaporation source device, and after the evaporation state stabilizes, evaporate a 50nm thick Li2CO3 protective layer on the surface of the PP diaphragm;
[0146] Adjust the evaporation parameters and evaporation source to evaporate a 3μm metal lithium layer on the Li2CO3 layer;
[0147] A shielding plate with a dot-matrix pattern is designed, the shielding plate is installed in the working position, the evaporation source is replaced with metal copper, and a 50nm thick dot-matrix metal copper layer is evaporated on the metal lithium layer;
[0148] Remove the shielding plate, adjust the evaporation parameters and evaporation source, and evaporate a 100nm thick Li2CO3 protective layer on the surface of the metal copper layer;
[0149] After the evaporation is completed, the power of the evaporation source is turned off, the vacuum is broken, the equipment is opened, and a pre-lithiation diaphragm is obtained.
[0150] Embodiment 2:
[0151] The difference between this embodiment and the first embodiment is that in this embodiment, a shielding plate with a square pattern is designed, thereby obtaining a metal copper layer with a square pattern.
[0152] Embodiment 3:
[0153] The difference between this embodiment and embodiment 1 is that in this embodiment, a shielding plate with a linear pattern is designed, and a metal Ag-Cu alloy layer is evaporated on the metal lithium layer to obtain a linear metal Ag-Cu alloy layer.
[0154] Embodiment 4:
[0155] The difference between this embodiment and embodiment 1 is that in this embodiment, a layer of conductive graphite is evaporated on the metal lithium layer.
[0156] Embodiment 5:
[0157] The difference between this embodiment and embodiment 1 is that: in this embodiment, a shielding plate with a linear pattern is designed, and a layer of conductive graphite-conductive carbon fiber mixed electron conductive layer is evaporated on the metal lithium layer, thereby obtaining a linear conductive graphite-conductive carbon fiber mixed electron conductive layer.
[0158] Embodiment 6:
[0159] This embodiment provides a lithium-supplemented negative electrode. Since a button battery is used for subsequent evaluation, this embodiment only performs pre-lithiation on one side of the negative electrode. The lithium-supplemented negative electrode includes a negative electrode sheet 21, a patterned electron-conducting layer 22, a lithium-supplementing layer 23, and a protective layer 24. Among them, the patterned electron-conducting layer 22 is a lattice-shaped metal copper layer, the lithium-supplementing layer 23 is a 3μm metal lithium layer, and the protective layer 24 is a 100nm Li3N protective layer. The specific preparation method is as follows:
[0160] Select a negative electrode sheet with graphite + silicon oxide as the negative electrode active material, design a shielding plate with a dot pattern, install the shielding plate in the working position, start the vacuum evaporation coating equipment, and adjust the working vacuum degree to 5×10 -2 Pa~5×10 -3 Pa; start the evaporation source device, preheat the evaporation boat, and then evaporate a 20nm thick lattice-shaped metal copper layer on the surface of the negative electrode;
[0161] After the evaporation is completed, the evaporation source power is turned off, the vacuum is broken, the equipment is opened, the shielding plate is removed, and the metal copper is replaced with metal lithium, and a 3 μm thick metal lithium layer is evaporated on the surface of the metal copper layer;
[0162] After the evaporation is completed, the evaporation source power is turned off, the vacuum is broken, the equipment is opened, the evaporation source is replaced, and a 100nm thick Li3N protective layer is evaporated on the metal lithium layer;
[0163] After the evaporation is completed, the power supply of the evaporation source is turned off, the vacuum is broken, the equipment is opened, and the lithium-supplemented negative electrode is obtained.
[0164] Embodiment 7:
[0165] The difference between this embodiment and the embodiment 6 is that in this embodiment, a shielding plate with a square pattern is designed, thereby obtaining a metal copper layer with a square shape.
[0166] Embodiment 8:
[0167] The difference between this embodiment and embodiment 6 is that in this embodiment, a shielding plate with a linear pattern is designed, and a metal Ag-Cu alloy layer is evaporated on the surface of the negative electrode sheet to obtain a linear metal Ag-Cu alloy layer.
[0168] Embodiment 9:
[0169] The difference between this embodiment and embodiment 6 is that in this embodiment, a layer of conductive graphite is evaporated on the surface of the negative electrode sheet.
[0170] Embodiment 10:
[0171] The difference between this embodiment and embodiment 6 is that: in this embodiment, a shielding plate with a linear pattern is designed, and a layer of conductive graphite-conductive carbon fiber mixed electron conductive layer is evaporated on the surface of the negative electrode to obtain a linear conductive graphite-conductive carbon fiber mixed electron conductive layer.
[0172] Embodiment 11:
[0173] The sodium supplementing membrane of this embodiment includes a membrane layer 11, a first protective layer 12, a sodium supplementing layer 12, a patterned electron conductive layer 14 and a second protective layer 15 in sequence. Among them, the membrane layer 11 is a PP membrane layer, the sodium supplementing layer 12 is a metallic sodium layer, the patterned electron conductive layer 14 is a lattice-shaped metallic copper layer, and the first protective layer 12 and the second protective layer 15 are Na2CO3 protective layers of different thicknesses. The preparation method includes the following steps:
[0174] Start the vacuum evaporation coating equipment and adjust the working vacuum degree to 5×10 -2 Pa~5×10 -3 Pa, start the evaporation source device, and after the evaporation state stabilizes, evaporate a 50nm thick Na2CO3 protective layer on the surface of the PP diaphragm;
[0175] Adjust the evaporation parameters and evaporation source to evaporate a 3μm metallic sodium layer on the Na2CO3 layer;
[0176] Design a shielding plate with a dot-shaped pattern, install the shielding plate in the working position, replace the evaporation source with metal copper, and evaporate a 20nm dot-shaped metal copper layer on the metal sodium layer;
[0177] Remove the shielding plate, adjust the evaporation parameters and evaporation source, and evaporate another 100nm thick Na2CO3 protective layer on the surface of the metal copper layer;
[0178] After the evaporation is completed, the power of the evaporation source is turned off, the vacuum is broken, the equipment is opened, and the sodium-supplemented diaphragm is obtained.
[0179] Embodiment 12:
[0180] This embodiment provides a sodium supplemented negative electrode. Since a button battery is used for subsequent evaluation, this embodiment only performs sodium pre-treatment on one side of the negative electrode. The sodium supplemented negative electrode includes a negative electrode sheet 21, a patterned electron conductive layer 22, a sodium supplemented layer 23, and a protective layer 24. Among them, the patterned electron conductive layer 22 is a lattice-shaped metal copper layer, the sodium supplemented layer 23 is a 3μm metal sodium layer, and the protective layer 24 is a 100nm NaF protective layer. The specific preparation method is as follows:
[0181] Select the negative electrode sheet with hard carbon as the negative electrode active material, design a shielding plate with a dot pattern, install the shielding plate in the working position, start the vacuum evaporation coating equipment, and adjust the working vacuum degree to 5×10 -2 Pa~5×10 -3 Pa; start the evaporation source device, preheat the evaporation boat, and then evaporate a 20nm thick lattice metal copper layer on the surface of the negative electrode;
[0182] After the evaporation is completed, turn off the power of the evaporation source, break the vacuum, open the equipment, remove the shielding plate, replace the evaporation source metal copper with metal sodium, and evaporate a 3μm metal sodium layer on the surface of the copper layer;
[0183] After the evaporation is completed, turn off the evaporation source power, break the vacuum, and open the equipment. After replacing the evaporation source, evaporate a 100nm NaF protective layer on the metal sodium layer;
[0184] After the evaporation is completed, the power of the evaporation source is turned off, the vacuum is broken, the equipment is opened, and the sodium-supplemented negative electrode is obtained.
[0185] Comparative Example 1:
[0186] In Comparative Example 1, no lithium supplementation measures are taken for the separator and the negative electrode plate. The separator is a PP separator, and the negative electrode active material in the negative electrode is a graphite + silicon oxide negative electrode plate.
[0187] Comparative Example 2:
[0188] The separator in comparative example 2 is a lithium supplement separator, including a separator matrix and a lithium supplement layer, the separator matrix is a PP separator, and the lithium supplement layer is a 3 μm metal lithium layer. The negative electrode active material in the negative electrode is a graphite + silicon oxide negative electrode sheet.
[0189] Comparative Example 3:
[0190] In Comparative Example 3, no sodium supplementation measures were taken for the separator and the negative electrode plate. The separator was a PP separator, and the negative electrode active material in the negative electrode was a hard carbon negative electrode plate.
[0191] The separators and negative electrodes of Comparative Examples 1-2 and the lithium-supplemented separators or lithium-supplemented negative electrodes of Examples 1-10 were used to make button batteries, and the production process was as follows:
[0192] The positive and negative pole pieces come from the battery cell production line. The positive pole uses ternary 8 series NCM material, and the negative pole uses graphite + silicon oxide material. The double-sided pole piece is wiped on one side and then dried.
[0193] Positive and negative electrodes and diaphragm punching, the diameter of the negative electrode is 14mm, the diameter of the positive electrode is 12mm, and the diameter of the diaphragm is 16mm;
[0194] The electrolyte used was 1M LiPF6 (lithium hexafluorophosphate), in which the solvent ratio was ethylene carbonate (EC): diethyl carbonate (DEC): ethyl methyl carbonate (EMC) = 1:1:1;
[0195] Assemble the CR2032 battery in the order of negative electrode shell - negative electrode - separator - positive electrode - gasket - spring - positive electrode shell.
[0196] The charge and discharge capacity, initial coulombic efficiency, capacity retention rate after 50 cycles, and capacity ratio at charge rates of 0.2C and 0.33C of the assembled button battery were tested. The results are shown in Table 1.
[0197] Table 1 Test data of button cell assembled in Examples 1-10 and Comparative Example 1
[0198]
[0199] Comparing the results of Examples 1-10 with those of Comparative Examples 1-2, it can be seen that the charging capacity of Examples 1-10 is substantially smaller than that of Comparative Examples 1-2, and the discharge capacity, first coulombic efficiency, capacity retention rate, and 2C / 0.33C capacity ratio are all greater than those of Comparative Examples 1-2, especially the first coulombic efficiency is significantly improved. This indicates that relative to conventional diaphragms, lithium-supplementing diaphragms, and negative electrodes in lithium-ion batteries, the lithium-supplementing diaphragms and lithium-supplementing negative electrodes disclosed herein can significantly improve the utilization rate of lithium by providing a patterned electron-conducting layer and constructing an electron channel, thereby greatly improving the energy density, first coulombic efficiency, cycle performance, and rate performance of lithium-ion batteries.
[0200] It can also be seen from Table 1 that the various performances of the battery of Example 2 are better than those of Example 1, and the various performances of the battery of Example 7 are better than those of Example 6, indicating that compared with the lithium-supplementing diaphragm or lithium-supplementing negative electrode with a lattice-shaped patterned electron conductive layer, the lithium-supplementing diaphragm or lithium-supplementing negative electrode with a square patterned electron conductive layer is better in improving the energy density, first coulombic efficiency, cycle performance, and rate performance of lithium-ion batteries.
[0201] It can also be seen from Table 1 that, compared with the lithium-supplementing separator of Example 5 and the lithium-supplementing negative electrode of Example 10, the performance of the battery assembled with the lithium-supplementing separator of Example 3 and the lithium-supplementing negative electrode of Example 8 is significantly improved, indicating that when the material of the patterned electron-conducting layer is a carbon mixed material and the material of the patterned electron-conducting layer is a metal alloy, the utilization rate of lithium ions is higher and the battery performance is better.
[0202] The diaphragm and negative electrode of Comparative Example 3 and the sodium-supplemented diaphragm or sodium-supplemented negative electrode of Examples 11 and 12 were respectively used to make button batteries, and the production process was as follows:
[0203] The positive and negative electrode sheets come from the battery cell production line. The positive electrode uses NaNiFeMnO2 material, and the negative electrode uses hard carbon material. The double-sided electrode sheets are wiped on one side and then dried.
[0204] Positive and negative electrodes and diaphragm punching, the diameter of the negative electrode is 14mm, the diameter of the positive electrode is 12mm, and the diameter of the diaphragm is 16mm;
[0205] The electrolyte used was 1M NaPF6 (sodium hexafluorophosphate), in which the solvent ratio was ethylene carbonate (EC): diethyl carbonate (DEC): ethyl methyl carbonate (EMC) = 1:1:1;
[0206] Assemble the CR2032 battery in the order of negative electrode shell - negative electrode - separator - positive electrode - gasket - spring - positive electrode shell.
[0207] The charge and discharge capacity, initial coulombic efficiency, capacity retention rate after 50 cycles, and capacity ratio at charge rates of 0.2C and 0.33C of the assembled button battery were tested. The results are shown in Table 2.
[0208] Table 2 Test data of button cell assembled in Examples 11 and 12 and Comparative Example 3
[0209]
[0210] Comparing the results of Examples 11 and 12 with those of Comparative Example 3, it can be seen that the charging capacity of Examples 11 and 12 is less than that of Comparative Example 3, and the discharge capacity, first coulombic efficiency, capacity retention rate and 2C / 0.33C capacity ratio are significantly greater than those of Comparative Example 3. This shows that compared with the traditional separator and negative electrode in the sodium ion battery, the sodium supplement separator and the sodium supplement negative electrode disclosed in the present invention can significantly improve the utilization rate of sodium by providing a patterned electron conductive layer and constructing an electron channel, thereby greatly improving the energy density, first coulombic efficiency, cycle performance and rate performance of the sodium ion battery.
[0211] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present disclosure, rather than to limit them; although the present disclosure has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present disclosure, and they should all be included in the scope of the claims and specification of the present disclosure. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present disclosure is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A lithium / sodium supplementing membrane, characterized in that: include: Diaphragm layer; A first protective layer, disposed on one side of the diaphragm layer; A lithium / sodium supplementing layer is arranged on a side of the first protective layer away from the diaphragm layer; A patterned electron-conducting layer is disposed on a side of the lithium / sodium supplementing layer away from the diaphragm layer; as well as The second protective layer is arranged on a side of the patterned electron-conducting layer away from the lithium / sodium supplementing layer.
2. The lithium / sodium supplement membrane according to claim 1, characterized in that: The pattern of the patterned electron-conducting layer includes at least one of a dot shape, a line shape or a surface shape.
3. The lithium / sodium supplementing membrane according to claim 2, characterized in that: The point shape includes a dot matrix formed by multiple discontinuous points; and / or the line shape includes a plurality of lines arranged at intervals; and / or the surface shape includes a network structure formed by a plurality of lines arranged crosswise, and / or a surface structure formed by at least one line.
4. The lithium / sodium supplement membrane according to any one of claims 1 to 3, characterized in that: The continuity of the patterned electron-conducting layer is 50% to 80%.
5. A lithium / sodium supplemented negative electrode, characterized in that: include: A negative electrode sheet, comprising a negative electrode current collector and a negative electrode active material layer located on at least one surface of the negative electrode current collector; A patterned electron conductive layer is disposed on one side or both sides of the negative electrode sheet and is located on the surface of the negative electrode active material layer away from the negative electrode current collector; a lithium / sodium supplementing layer, disposed on a side of the patterned electron conductive layer away from the negative electrode sheet; and The protective layer is arranged on a side of the lithium / sodium supplementing layer away from the patterned electron conducting layer.
6. The lithium / sodium supplemented negative electrode according to claim 5, characterized in that: The pattern of the patterned electron-conducting layer includes at least one of a dot shape, a line shape or a surface shape.
7. The lithium / sodium supplemented negative electrode according to claim 6, characterized in that: The point shape includes a dot matrix formed by multiple discontinuous points; and / or the line shape includes a plurality of lines arranged at intervals; and / or the surface shape includes a network structure formed by a plurality of lines arranged crosswise, and / or a surface structure formed by at least one line.
8. The lithium / sodium supplemented negative electrode according to any one of claims 5 to 7, characterized in that: The continuity of the patterned electron-conducting layer is 50% to 80%.
9. A lithium / sodium ion battery, comprising a positive electrode, a negative electrode and a separator, wherein the separator is arranged between the positive electrode and the negative electrode, characterized in that: The separator is the lithium / sodium supplement separator according to any one of claims 1 to 4; and / or the negative electrode is the lithium / sodium supplement negative electrode according to any one of claims 5 to 8.
10. A method for preparing a lithium / sodium supplementing membrane as claimed in claims 1 to 4, characterized in that: The following steps are involved: Depositing the first protective layer on one side of the diaphragm layer; Depositing the lithium / sodium supplement layer on a side of the first protective layer away from the diaphragm layer; Designing a shielding plate with a hollow pattern, installing the shielding plate with the hollow pattern on the side of the lithium / sodium supplement layer away from the diaphragm layer, and after evaporation, the evaporation source passes through the shielding plate with the hollow pattern and is deposited on the side of the lithium / sodium supplement layer away from the diaphragm layer to form the patterned electron conductive layer; The shielding plate with the hollow pattern is removed, and the second protective layer is deposited on the side of the patterned electron conductive layer away from the lithium / sodium supplementing layer.
11. A method for preparing a lithium / sodium supplemented negative electrode as claimed in claims 5-8, characterized in that: include: Designing a shielding plate with a hollow pattern, installing the shielding plate with the hollow pattern on one side of the negative electrode sheet, and allowing the evaporation source to evaporate through the shielding plate with the hollow pattern and deposit on the surface of the negative electrode active material layer of the negative electrode sheet to form the patterned electron conductive layer; Removing the shielding plate with the hollow pattern, and depositing the lithium / sodium supplementing layer on the side of the patterned electron conductive layer away from the negative electrode sheet; A protective layer is deposited on a side of the lithium / sodium supplementing layer away from the patterned electron conducting layer.
12. A method for preparing a lithium / sodium ion battery, characterized in that: The following steps are involved: Providing a positive electrode, a separator and a negative electrode, wherein the separator is obtained by the preparation method of the lithium / sodium supplemented separator according to claim 10, or the negative electrode is obtained by the preparation method of the lithium / sodium supplemented negative electrode according to claim 11; The separator is arranged between the positive electrode and the negative electrode, and the positive electrode, the separator and the negative electrode are placed in a shell, and the shell is sealed after the electrolyte is injected into the shell.
Citation Information
Patent Citations
Composite negative pole piece, battery and preparation method
CN113871736A
Negative electrode sheet, secondary battery, and electrical apparatus
WO2024073897A1
Cited By
Sodium metal negative electrode structure, preparation method thereof and sodium ion battery
CN120149330A
A sodium metal negative electrode structure and preparation method thereof, and sodium ion battery