Complex of hydrotalcite-based compound and amino acid

By preparing hydrotalcite compound with high aspect ratio and yellowness-controlled hydrotic acid complex, combining polymers to form a coating with high gas barrier and transparency, the problem of limited use in the prior art is solved and the complex is realized multi-purpose application.

CN119013232APending Publication Date: 2024-11-22SETOLAS HLDG INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380033204.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-11-11
Filing Date
2023-03-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, increasing the aspect ratio of hydrotalcite compounds will lead to the use of the complex being limited, especially the colorability increases, affecting its transparency and aesthetics.

Method used

By preparing a complex of hydrotalcite compounds with an aspect ratio of 85 or more, controlling their yellowness (Y.I. value) within the range of 0 to 5, combining polymers to form a coating liquid, which is used to form a high gas barrier and transparency. sexual coating.

Benefits of technology

It achieves a high gas barrier and multi-purpose composite without damaging transparency and aesthetics, and is suitable for packaging film and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013232A_ABST
    Figure CN119013232A_ABST
Patent Text Reader

Abstract

Provided is a complex of a hydrotalcite-based compound and an amino acid, the complex having a high aspect ratio and capable of controlling colorability. The complex according to the present disclosure has a hydrotalcite-based compound and an amino acid. The composite has an aspect ratio of 85 or more. The composite has a Y.I. Value of 0 to 5. And the Y.I. Value represents the yellowness. The content of amino acids in the complex is more than 0% by mass but not more than 10.0% by mass. The content of the amino acid is relative to the total mass of the complex.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a complex of a hydrotalcite compound and an amino acid. Background Art

[0002] Hydrotalcite or a hydrotalcite compound representing a calcined product thereof has an ion exchange capacity and is used for various purposes such as inhibiting the deterioration of the resin by being compounded in a resin. As such a hydrotalcite compound, a method of further improving the aspect ratio by using an amino acid is known (Patent Document 1 and Non-Patent Document 1). By using the method disclosed in Patent Document 1 and Non-Patent Document 1, a complex of a hydrotalcite compound and an amino acid can be obtained.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2019 / 092453

[0006] Non-patent literature

[0007] Non-patent document 1: NATURE COMMUNICATIONS (2019) 10: 2398, High gas barrier coating us ing non-toxic nanosheet di spers ions for flexible food packaging film. Summary of the invention

[0008] Problems to be solved by the invention

[0009] However, the methods disclosed in Patent Document 1 and Non-Patent Document 1 have a problem in that increasing the aspect ratio of the hydrotalcite compound causes coloring, and thus the use of the composite is limited.

[0010] Therefore, an object of the present invention is to provide a composite having a higher utilization range.

[0011] Means for solving problems

[0012] The present inventors have conducted intensive studies to achieve the above object and have found that a complex of a hydrotalcite compound and an amino acid having a high aspect ratio and controllable coloring properties can be formed to provide a complex with a higher number of uses.

[0013] The present disclosure has been completed based on this finding, and includes the following aspects.

[0014] (First Publication)

[0015] In the first disclosure, the composite has a hydrotalcite compound and an amino acid. The aspect ratio of the composite is 85 or more. The YI value of the composite is 0 to 5. The YI value represents the yellowness. The amino acid content of the composite is greater than 0 mass % and less than 10.0 mass %. The amino acid content is the content relative to the total mass of the composite.

[0016] (Second Publication)

[0017] As far as the second disclosure is concerned, in the first disclosure, the amino acid is a glycine compound.

[0018] (Third Publication)

[0019] In the third disclosure, in the first disclosure or the second disclosure, the hydrotalcite compound is represented by the following formula (1).

[0020] (M 2+ ) 1-X (M 3+ ) X (OH)2(A n- ) X / n ·mH2O···(1)

[0021] (In formula (1), M 2+ is a divalent metal cation. In formula (1), M 3+ is a trivalent metal cation. In formula (1), A n- is an anion with a valence of n. In formula (1), X is a number satisfying 0.17<X<0.36. In formula (1), n ​​is an integer of 1 to 6. In formula (1), m is a number satisfying 0<m<1.80. )

[0022] (Fourth Publication)

[0023] In the fourth disclosure, in any one of the first to third disclosures, the thickness of the primary particle of the composite is 20 nm or less, and the aspect ratio of the composite is 100 or more.

[0024] (Fifth Publication)

[0025] The fifth disclosure is a coating liquid, wherein the coating liquid contains the composite according to any one of the first to fourth disclosures, and the coating liquid contains a polymer.

[0026] (Sixth Publication)

[0027] With regard to the present sixth disclosure, in the fifth disclosure, the polymer is a water-soluble polymer.

[0028] (Seventh Publication)

[0029] In the seventh disclosure, in the sixth disclosure, the water-soluble polymer is polyvinyl alcohol.

[0030] (Eighth Publication)

[0031] The eighth disclosure is a film having a coating layer.

[0032] The covering layer is formed using the coating solution according to any one of the fifth to seventh disclosures.

[0033] (9th Publication)

[0034] In the ninth disclosure, in the eighth disclosure, the coating layer has a thickness of 1 μm or more and 1000 μm or less.

[0035] Effects of the Invention

[0036] According to the present invention, a complex of a hydrotalcite compound and an amino acid which has a high aspect ratio and can control colorability can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 A schematic diagram showing a film production apparatus for producing a packaging film according to an embodiment of the present invention.

[0038] Figure 2 These are photographs of the slurry solutions after the heating step of Examples 1 to 3 of the present invention and Comparative Examples 1 to 3, and photographs of the slurry solutions when the temperature was raised to 100° C. in the heating step of Comparative Examples 4 to 6. DETAILED DESCRIPTION

[0039] Preferred embodiments of the complex of a hydrotalcite compound and an amino acid of the present invention (hereinafter sometimes referred to as "the complex of the present invention" etc.) are described in detail below. It should be noted that the "complex of a hydrotalcite compound and an amino acid" in this specification means a state in which the hydrotalcite compound is chemically modified with an amino acid.

[0040] [Complex]

[0041] In one embodiment of the present invention, the composite is a composite of a hydrotalcite compound and an amino acid having an aspect ratio of 85 or more. In the composite of this embodiment, the YI value indicating the yellowness of the composite is 0 to 5. Furthermore, in the composite of this embodiment, the content of the amino acid relative to the total mass of the composite is greater than 0 mass % and less than 10.0 mass %.

[0042] The composite of the present embodiment has a high aspect ratio, so that when forming a coating layer, a plurality of composites are arranged in parallel relative to the surface direction of the coating layer in the coating layer, and excellent gas barrier properties can be exerted. In addition, the YI value of the composite of the present embodiment is within a specific range of less than 5, and the content of amino acids is within a specific range of less than 10.0 mass %. Thus, the composite of the present embodiment can form a coating layer with high transparency without coloring such as yellow-brown. The mechanism of action for obtaining such a coating layer with high transparency is not subject to any theoretical constraints and is considered to be as follows.

[0043] First, the composite of the present embodiment can be obtained by the following manufacturing method, which has: a solution preparation step of mixing the composite metal oxide obtained by calcining the precursor hydrotalcite compound with an amino acid (such as glycine, etc.) as a stripping agent to prepare a slurry solution; and a heating step of heating the slurry solution prepared by the solution preparation step. This manufacturing method uses an amino acid as a stripping agent, so that the interlayer stripping of the hydrotalcite compound occurs, so it is advantageous in terms of obtaining a thin hydrotalcite compound with a thickness of a primary particle. However, in the heating step for stripping the hydrotalcite compound, the peptide binding between the amino acids is promoted under alkaline conditions to generate polyamino acids (such as peptides such as polyglycine). It is known that if peptides such as polyglycine become long chains, yellowing occurs, and the longer the molecular chain, the more the yellow tone increases. Therefore, if a hydrotalcite compound containing such a long-chain peptide (polypeptide) and an amino acid complex are combined with a polymer, etc. in a coating liquid, the transparency and beauty of the obtained coating layer will be impaired.

[0044] In the present embodiment, in the above-mentioned solution preparation process, by making the slurry concentration and the amino acid concentration respectively within a specific range, the formation of peptide bonds between amino acids can be suppressed under alkaline conditions, thereby hindering the generation of polyamino acids (peptides). As a result, it is believed that the yellowing of the obtained complex can be suppressed. In this way, a complex having an aspect ratio of more than 85, a YI value representing yellowness of 0 to 5, and an amino acid content of more than 0 mass % and less than 10.0 mass % can be obtained. Moreover, such a complex can be combined with a polymer or the like in a coating liquid to form a coating layer having both high gas barrier properties and transparency. In this way, the complex of the present embodiment can be used for a variety of purposes requiring gas barrier properties without compromising transparency and aesthetics. For example, when a coating liquid containing the complex of the present embodiment is applied to a film, high gas barrier properties can be imparted to the film without compromising transparency.

[0045] It should be noted that, in the composite of the present embodiment, in the above-mentioned solution preparation process, an aqueous solution of amino acids is used to hydrate the composite metal oxide obtained by calcining the precursor hydrotalcite compound. The aqueous solution of amino acids can be exemplified by an aqueous solution of glycine. During hydration, the amino acid molecules in the solution enter the interlayer of the hydrotalcite compound as anions, thereby exfoliating the interlayer of the hydrotalcite compound. Through the exfoliation of the interlayer of the hydrotalcite compound, thin particles are formed. The thin particles are heated by a heating process, and the hydrotalcite compound whose particle growth in the width direction is promoted forms a composite. In other words, particles with a high aspect ratio are formed. At this time, when the amount of amino acids is too small relative to the amount of the hydrotalcite compound, the hydrotalcite compound particles that are not fully exfoliated remain, and the aspect ratio of the resulting composite is reduced. That is, the aspect ratio of the composite becomes less than 85.

[0046] As described above, for the composite of the present embodiment, the YI value indicating the yellowness is 0 to 5. This YI value becomes an index of the "polyamino acid content" that affects coloring such as yellowing. If the YI value exceeds 5, a state of coloring such as yellowish brown is produced, so if such a colored composite is used as a component of a coating liquid to form a coating layer, it is possible to impair transparency and appearance. The preferred range of the YI value is 4 or less, and more preferably 3 or less. If the YI value is within such a range, a coating layer with higher transparency can be formed.

[0047] Various components contained in the composite body of this embodiment will be described below.

[0048] (Hydrotalcite compounds)

[0049] The hydrotalcite compound contained in the composite of the present embodiment is not particularly limited, and examples thereof include a hydrotalcite compound represented by the following formula (1).

[0050] (M 2+ ) 1-X (M 3+ ) X (OH)2(A n- ) X / n ·mH2O···(1)

[0051] (In formula (1), M 2+ is a divalent metal cation, M 3+ A is a trivalent metal cation. n- is an anion with a valence of n. X is a number satisfying 0.17<X<0.36. n is an integer of 1 to 6, and m is a number satisfying 0<m<1.80. )

[0052] In the above formula (1), preferably M2+ Mg 2+ , preferably M 3+ For Al 3+ These hydrotalcite compounds are highly safe for living organisms, and have a refractive index close to that of resins such as polypropylene and polyethylene, so that when a coating layer is formed on a substrate formed of such resins, transparency is easily maintained. Furthermore, the molar ratio of Mg / Al2 is preferably in the range of 4 to 8 from the perspective of more reliably obtaining a hydrotalcite structure.

[0053] In the above formula (1), n- The type of anion is not particularly limited, and examples thereof include carbonate ions (CO3 2- ), hydroxide ion (OH - )wait.

[0054] It should be noted that the above-mentioned hydrotalcite compounds are the hydrotalcite compounds contained in the composite of the present embodiment, and the same is true for the precursor hydrotalcite compounds used as raw materials in the manufacture of the composite of the present embodiment. As described later, the precursor hydrotalcite compounds are mixed with an aqueous solution of amino acids after being calcined to form a composite metal oxide. From the perspective that the precursor hydrotalcite compounds, i.e., the hydrotalcite compounds before calcination, do not produce corrosive gases such as chlorine and nitrogen dioxide gas during calcination, carbonate ions are preferred.

[0055] (Amino Acid)

[0056] On the other hand, there is no particular limitation on the amino acids contained in the complex of the present embodiment, and various amino acids such as α-amino acids, β-amino acids, and γ-amino acids can be listed. More specifically, for example, aspartic acid, glutamic acid, asparagine, serine, glycine, β-alanine, β-aminobutyric acid, γ-aminobutyric acid, β-leucine, etc. can be listed. With respect to these amino acids, one amino acid can be contained alone, or two or more amino acids can be contained. Furthermore, these amino acids can be in the form of a polymer (i.e., a peptide) formed by bonding multiple amino acids.

[0057] Among the various amino acids mentioned above, the amino acids contained in the complex of the present embodiment are preferably amino acids having a solubility of 10 g / 100 mL H2O or more, and glycine compounds are particularly preferred. Such amino acids, especially glycine compounds, are advantageous in obtaining a complex with a thin primary particle thickness due to their high dielectric constant. Furthermore, glycine has an antibacterial effect and is also used in supplements, colorants, fragrances, etc., which is advantageous from the perspective of biological safety.

[0058] In addition, in this specification, substances containing amino acids and amino acid polymers may be referred to as "amino acid compounds." For example, substances containing glycine and polyglycine may be referred to as "glycine compounds."

[0059] Furthermore, in the present specification, the so-called "solubility of 10 g / 100 mL H2O or more" means a solubility of 10 g or more of the mass of the object (ie, amino acid) dissolved in 100 g of water at 25°C.

[0060] In the composite of the present embodiment, the content of amino acids relative to the total mass of the composite is greater than 0 mass % and less than 10.0 mass %. The content of amino acids is preferably greater than 1.0 mass % and less than 8.0 mass %, and more preferably greater than 1.5 mass % and less than 6.0 mass %, from the perspective of being able to more reliably form a coating layer having both high gas barrier properties and transparency.

[0061] In addition, the composite of the present embodiment has a high aspect ratio of 85 or more as described above. Therefore, the composite of the present embodiment can exhibit excellent gas barrier properties when forming a coating layer. The aspect ratio of the composite is preferably 90 or more, and more preferably 100 or more, from the perspective of obtaining higher gas barrier properties. The upper limit of the aspect ratio of the composite is not particularly limited, and is, for example, 500 or less.

[0062] In this specification, the aspect ratio of the composite is the ratio of the width (diameter) to the thickness of the primary particle of the composite having a layered structure, and can be obtained by dividing the width of the primary particle of the composite by the thickness.

[0063] The thickness of the primary particle of the composite of the present embodiment is not particularly limited as long as it has an aspect ratio of 85 or more, and for example, a thickness of 20 nm or less can be cited. In terms of obtaining better gas barrier properties when forming a coating layer, it is preferred that the thickness of the primary particle of the composite is 20 nm or less and the aspect ratio is 100 or more.

[0064] It should be noted that the thickness of the primary particles of the composite is more preferably in the range of 0.7 nm to 10 nm. If the thickness of the primary particles of the composite is in the range of 0.7 nm to 10 nm, the hydrotalcite compound is fully exfoliated, and a higher gas barrier property can be exerted when forming a coating layer.

[0065] Next, a method for producing the composite body according to the present embodiment will be described.

[0066] [Method for producing a composite body]

[0067] The composite body of the present embodiment can be obtained by the following manufacturing method as described above: the manufacturing method comprises: a solution preparation step of mixing an aqueous solution of an amino acid of a specified concentration as a stripping agent with a composite metal oxide obtained by calcining a precursor hydrotalcite compound to prepare a slurry solution; and a heating step of heating the slurry solution obtained in the solution preparation step.

[0068] In the solution preparation step, the amino acid concentration of the slurry solution may be a concentration within a range of more than 0 mass % and 50.0 mass % or less of the amino acid content relative to the total mass of the obtained composite.

[0069] (Solution preparation process)

[0070] In the solution preparation process, first, the precursor hydrotalcite compound is calcined to obtain a composite metal oxide. As the precursor hydrotalcite compound, the same hydrotalcite compound as that contained in the above-mentioned composite can be used. There is no particular limitation on the calcination time when the precursor hydrotalcite compound is calcined. For example, when a calcination furnace is used for calcination, the calcination time is 0.1 hours or more and 24 hours or less. Similarly, there is no particular limitation on the calcination temperature. For example, when a calcination furnace is used for calcination, the calcination temperature is 300°C or more and 700°C or less. As for the calcination time when the precursor hydrotalcite compound is calcined, for example, when microwave calcination is used, the calcination time is 1 minute or more and 12 hours or less. When microwave calcination is used, for example, the temperature can also be set to 300°C or more and 700°C or less.

[0071] Secondly, by adding an aqueous solution of amino acids of a prescribed concentration to the powder of the composite metal oxide obtained by calcining the precursor hydrotalcite compound and mixing, a slurry solution is obtained. At this time, the slurry concentration of the slurry solution is preferably less than 30g / L. Usually, the hydrotalcite compound obtained using such a stripping agent has a thickness of a primary particle as thin as a few nm, so if the slurry concentration is high, gelation occurs during the stripping process, and sometimes an inhomogeneous sample is formed. Therefore, in the manufacturing method of the composite of the present embodiment, by making the slurry concentration in the solution preparation process less than 30g / L, the particle interaction of the hydrotalcite compound can be reduced, and the gelation during the stripping process can be suppressed. Thus, the above-mentioned manufacturing method can maintain the slurry state of the slurry solution, so that the composite can be produced uniformly and efficiently.

[0072] In addition, the slurry concentration in the solution preparation step is more preferably in the range of 10 g / L to 28 g / L from the viewpoint of productivity, etc. The slurry concentration can be calculated using the following formula.

[0073] Slurry concentration (g / L) = weight of composite metal oxide (g) / slurry volume (L)

[0074] In the solution preparation step, the amino acid concentration of the slurry solution is preferably less than 0.6 mol / L. If the amino acid concentration of the slurry solution is within such a range, a composite having an aspect ratio of 85 or more and a YI value of 0 to 5 can be obtained more reliably. That is, a composite having a high gas barrier property and a highly transparent coating layer without coloring such as yellow-brown can be obtained more reliably. It should be noted that the amino acid concentration of the slurry solution is more preferably within the range of 0.2 mol / L to 0.5 mol / L.

[0075] In the solution preparation step, the molar ratio of the amino acid in the slurry solution to the trivalent metal cation of the hydrotalcite compound, that is, amino acid / (M 3+ )2 is preferably in the range of 2 to 6. For example, when the amino acid is glycine and the trivalent metal cation of the hydrotalcite compound is Al 3+ In the case of glycine / Al2, the molar ratio of glycine / Al2 is preferably in the range of 2 to 6. If the molar ratio is in such a range, a composite having an aspect ratio of 85 or more and a YI value of 0 to 5 can be obtained more reliably, that is, a composite having a high gas barrier property and a highly transparent coating layer without coloration such as yellowish brown can be formed.

[0076] (Heating process)

[0077] In the heating step, the slurry solution obtained in the solution preparation step is heated to promote the particle growth of the hydrotalcite compound. At this time, the amino acid molecules in the solution enter the interlayer of the hydrotalcite compound as anions, so that the interlayer of the hydrotalcite compound is peeled off, and a complex of the hydrotalcite compound and the amino acid is generated as a thin particle (i.e., a particle with a high aspect ratio).

[0078] In the heating step, the slurry solution is preferably heated while being stirred. The stirring means is not particularly limited, but a means capable of uniformly stirring the slurry solution while maintaining fluidity is preferred.

[0079] In the heating step, the heating temperature is not particularly limited, and is preferably a temperature in the range of 20°C to 250°C. From the viewpoint of being able to more reliably suppress amino acid modification, the upper limit of the particularly preferred heating temperature is 170°C. The heating time is not particularly limited, and is preferably a time in the range of 1 minute to 100 hours. In addition, from the perspective of the difficulty in changing the concentration of the slurry solution, it is preferred to implement the heating step in a closed system.

[0080] (Other processes)

[0081] The process after the heating process is not particularly limited as long as it does not hinder the effect of the present invention. As the process after the heating process, for example, a washing process of washing the slurry solution after the heating process with an alkaline solution (e.g., a sodium hydroxide solution), a solid-liquid separation process of performing solid-liquid separation treatment to obtain a solid after the washing process, a drying process of drying the solid obtained in the solid-liquid separation process to obtain a powder of the composite, a surface treatment process of treating the surface of the particles of the composite with various surface treatment agents, etc. can be listed.

[0082] It should be noted that as the surface treatment agent used in the surface treatment process, anionic surfactants, cationic surfactants, phosphate treatment agents, silane coupling agents, titanate coupling agents, aluminum coupling agents, silicone treatment agents, silicic acid and water glass can be exemplified, but are not limited to these. Particularly preferred surface treatment agents are selected from oleic acid, stearic acid, octanoic acid and octanoic acid. By surface treating the particles of the composite, the aggregation of the primary particles can be prevented in the case of adding, mixing, and dispersing in the resin.

[0083] Before the above-mentioned washing step, a dilution step of diluting the slurry after the heating step with ion exchange water may be performed. Also, instead of the above-mentioned drying step, a coating liquid preparation step of preparing a coating liquid by mixing with a polymer solution or the like may be performed.

[0084] The composite of the present embodiment obtained by the above-described production method can be mixed with a polymer solution as described above to prepare a coating liquid.

[0085] [Coating liquid]

[0086] The coating liquid containing the composite of the present embodiment and the polymer can be applied on a substrate described later and dried to form a coating layer. The concentration of the composite contained in the coating liquid is not particularly limited, but from the perspective of coating properties on the substrate, a concentration of 20% by mass or less is preferred, and a concentration of 10% by mass or less is more preferred.

[0087] (polymer)

[0088] The polymer contained in the coating liquid is used in the form of a solution dissolved in a solvent such as water or alcohol. It should be noted that the polymer concentration in the solution is not particularly limited, but is preferably 20% by mass or less, and more preferably 10% by mass or less, from the perspective of coating properties on a substrate.

[0089] There is no particular limitation on the type of polymer contained in the coating solution, and any polymer that is consistent with the purpose of the coating layer or film to be formed can be used. As such a polymer, for example, water-soluble polymers can be listed, and more specifically, polyvinyl alcohol, copolymers containing vinyl alcohol (such as polyethylene vinyl alcohol, etc.), carboxymethyl cellulose, polyacrylic acid, polyacrylamide, etc. can be listed. These water-soluble polymers can be used alone as one polymer, or two or more polymers can be used in combination. By using a water-soluble polymer, the separation of the substrate and the coating layer is easy, and the recyclability is improved, so it can contribute to the realization of the SDGs (sustainable development goals) adopted at the United Nations Summit.

[0090] Among these water-soluble polymers, polyvinyl alcohol is preferably used from the viewpoints of gas barrier properties, transparency, coating properties, and the like.

[0091] (Other ingredients)

[0092] In the range that does not hinder the effect of the present invention, in addition to the above-mentioned complex and polymer, the coating liquid may contain other additives. Such additives are not particularly limited, and for example, antioxidants, reinforcing agents, ultraviolet absorbers, pigments, crosslinking agents, flame retardants, etc. can be listed. These additives can be used alone as one additive, or two or more additives can be used in combination.

[0093] [membrane]

[0094] The coating solution containing the composite of the present embodiment and the polymer is applied on a substrate and dried to form a coating layer. The drying conditions can be appropriately set, for example, in a temperature range of room temperature to 160° C. and between 1 second and 24 hours. Among them, when a film-like substrate (hereinafter sometimes referred to as a "film-like substrate") is used as a substrate, a film of a multilayer structure in which the film-like substrate is covered with a coating layer can be obtained. In addition, by peeling off the coating layer on the substrate, a film of a single-layer structure composed of the coating layer can be obtained. The multilayer structure or single-layer structure film obtained in this way can be suitable for use as various packaging films, for example.

[0095] When a water-soluble polymer is used, the packaging film may be formed with a multilayer structure of the water-soluble polymer or a monolayer structure of the water-soluble polymer. As such a packaging film, for example, films for packaging detergents, pesticides, or pharmaceuticals may be cited. As the form of the pharmaceutical, for example, powders, solids, gels, and liquids may be cited. In addition, the packaging film may be used as a film for packaging fish baits. Furthermore, the packaging film may be used as a film for packaging liquid detergents.

[0096] (Base material)

[0097] The substrate used in forming the film is not particularly limited, and any substrate that is suitable for the purpose of the film to be formed can be used. Examples of such substrates include the above-mentioned film-like substrates, and more specifically, resin films such as polyolefin films such as polyethylene and polypropylene, and polyester films such as polyethylene terephthalate; paper; and fiber sheets such as woven fabrics, nonwoven fabrics, and knitted fabrics.

[0098] When a film-like substrate is used as the substrate, the thickness thereof is not particularly limited, and for example, the thickness is preferably in the range of 0.01 μm to 250 μm, and more preferably in the range of 1 μm to 100 μm. It should be noted that the thickness of the coating layer formed by the above-mentioned coating liquid is also not particularly limited, and for example, the thickness is in the range of 0.01 μm to 100 μm.

[0099] The film obtained using the composite of the present invention can be used in a wide range of fields such as food packaging films, beverage packaging films, beverage bottles, pharmaceutical packaging films, industrial gas barrier films, gas separation films, and paper barrier materials.

[0100] Furthermore, the film containing the composite of the present invention can be used for a bag-shaped package. The package can have any structure in accordance with the packaging object contained therein, in addition to individual packaging, inner packaging, and outer packaging.

[0101] When the film containing the composite of the present invention is used for a bag-shaped package, the bag-shaped package can be configured to have a coating layer on the outside of the package, for example. The coating layer can be formed by applying a coating liquid containing the composite to the outside of the package and drying it. The package can have a high aspect ratio, improved gas barrier properties, and controlled colorability. In particular, the package has a coating layer formed by a coating liquid on the outside of the package, so that even if the packaged object is a liquid or an object containing a liquid, the dissolution of the coating component can be prevented.

[0102] Furthermore, when the film containing the composite of the present invention is used for a bag-shaped packaging body, the bag-shaped packaging body can be configured to have a coating layer on the inside of the packaging body, for example. The coating layer can be formed by applying a coating liquid containing the composite on the inside of the packaging body and drying it. For example, the packaging body has a coating layer formed by a coating liquid on the inside of the packaging body, so that when the packaging body is subjected to external influences such as friction and water wetting, the coating layer can be maintained without being damaged. As a result, the packaging body can maintain the quality of the contents by maintaining the gas barrier effect of the coating layer. It should be noted that, in the case of a bag-shaped packaging body, for example, in the case of a coating layer on the inside of the packaging body, the coating layer can be formed in addition to the welded surface of the packaging body. In addition, in the case of a bag-shaped packaging body, for example, in the case of a coating layer on the inside of the packaging body, an adhesive layer with gas barrier properties is formed on the welded surface of the packaging body, and the coating layer can be formed in addition to the adhesive layer.

[0103] In addition, when the film containing the composite of the present invention is used for a bag-shaped package, the bag-shaped package can be configured to have a coating layer on both the inner and outer sides of the package. The bag-shaped package has a coating layer formed by a coating liquid on both the inner and outer sides of the package, thereby achieving higher gas barrier properties than the case where the coating layer is provided on either the inner or outer sides. As a result, the bag-shaped package can maintain the quality of low-water-activity contents such as wheat flour, snacks, tea leaves, and dried vegetables for a long time.

[0104] The film containing the composite of the present invention can be formed into a structure of a multilayer film having a coating layer formed by a coating liquid between film-like substrates. When the multilayer film containing the composite of the present invention is used in a bag-like packaging body, the bag-like packaging body can be constructed in such a way that a packaging object can be accommodated inside by a pair of multilayer films. The bag-like packaging body using the multilayer film containing the composite can bond the film-like substrates to each other, so it can be constructed without using an adhesive separately. The bag-like packaging body using the multilayer film can have the advantages of both a bag-like packaging body having a coating layer formed by a coating liquid on the outside of the packaging body and a bag-like packaging body having a coating layer formed by a coating liquid on the inside of the packaging body.

[0105] When the film containing the composite body is a single-layer structure, the coating layer itself becomes the film. The single-layer film can be, for example, Figure 1 The film manufacturing apparatus 100 shown is manufactured.

[0106] The film manufacturing apparatus 100 includes: a first tank 1, a second tank 2, and a third tank 3. In addition, the film manufacturing apparatus 100 includes: a first coating drum 71, a second coating drum 72, and a casting belt 8. The film manufacturing apparatus 100 is configured such that the casting belt 8 moves between the first coating drum 71 and the second coating drum 72 by rotating the first coating drum 71 and the second coating drum 72. In other words, the casting belt 8 is configured to be movable between the first coating drum 71 and the second coating drum 72 by rotating the first coating drum 71 and the second coating drum 72. In the film manufacturing apparatus 100, a drying device 9 capable of sending hot air 10 is arranged with respect to the casting belt 8 moving between the first coating drum 71 and the second coating drum 72. Figure 1 In FIG. 1 , the hot air 10 is exemplified by a dotted line.

[0107] Figure 1 The first tank 1 stores a slurry containing a composite and water. The first tank 1 is provided with a first agitator 41 for agitating the slurry. The second tank 2 stores a polymer. The second tank 2 is provided with a second agitator 42 for agitating the polymer. The first tank 1 is configured so that the slurry can be supplied to the third tank 3 via a first pump 51. The second tank 2 is configured so that the polymer can be supplied to the third tank 3 via a second pump 52. The third tank 3 is provided with a third agitator 43 for agitating a mixed polymer mixed with the slurry supplied from the first tank 1 and the polymer supplied from the second tank 2.

[0108] The third tank 3 casts the mixed polymer from the casting die 6 onto the casting belt 8 via the third pump 53. The mixed polymer cast from the casting die 6 moves in the running direction together with the casting belt 8 and is arranged in the width direction and running direction of the casting belt 8. The mixed polymer moving in the running direction together with the casting belt 8 is dried by the hot air 10 from the drying device 9 to form a film 12. Figure 1 In FIG. 1 , an arrow written in parallel with the casting belt 8 indicates the traveling direction of the casting belt 8 .

[0109] In the film manufacturing apparatus 100, a peeling roller 11 is provided adjacent to the second coating drum 72 to peel off the film 12 on the casting belt 8. The film manufacturing apparatus 100 is provided with a winding device 13 corresponding to the peeling roller 11. The winding device 13 winds up the film 12 peeled off by the peeling roller 11. Figure 1 In FIG. 1 , an arrow written in parallel with the film 12 to be peeled off by the peeling roller 11 indicates the traveling direction of the film 12 .

[0110] The film production apparatus 100 may use a plated roll as a support, for example, instead of the casting belt 8. The film is not limited to the one using the solution casting method, and may be formed using the melt extrusion method.

[0111] The packaging film having the coating layer containing the composite of the present embodiment is sealed between the ends of the film, for example, using a heated sealing strip, to form a bag-shaped packaging body in which the contents are packaged. The sealing method of the film can be, for example, heat sealing, water sealing, or glue sealing.

[0112] The packaging film can seal and package a single portion of liquid detergent, for example. When polyvinyl alcohol is used, the coating layer becomes a water-soluble bag-shaped bag body. The bag-shaped bag body can also maintain high fragrance retention by having water solubility from polyvinyl alcohol and further containing the composite of the present embodiment. In addition, the bag-shaped bag body can also be thinned while maintaining strength by containing the composite. In the case of a water-soluble bag-shaped packaging body, the thickness of the film is preferably 1 μm or more, more preferably 10 μm or more. In the case of a water-soluble bag-shaped packaging body, the thickness of the film is preferably 1000 μm or less, more preferably 500 μm or less. It should be noted that the thickness of the film can be measured, for example, using a micrometer or a film thickness meter using an optical interferometry method.

[0113] The coating liquid may contain at least one auxiliary agent of, for example, a surfactant, a plasticizer, a release agent, a stabilizer, a colorant, an ultraviolet absorber, an extender, a defoamer, and a dispersant. The auxiliary agent may be either an organic substance or an inorganic substance.

[0114] Examples of surfactants include ionic surfactants, nonionic surfactants, and polymer surfactants. Examples of ionic surfactants include anionic surfactants, cationic surfactants, and amphoteric surfactants. The content of the surfactant is not particularly limited, and for example, it is preferably 0.03 parts by mass or more, and more preferably 0.05 parts by mass or more, relative to 100 parts by mass of the polymer. The content of the surfactant is, for example, preferably 2.5 parts by mass or less, and more preferably 1.5 parts by mass or less, relative to 100 parts by mass of the polymer.

[0115] Examples of the plasticizer include glycerin, diglycerin, glucose, fructose, lactose, sorbitol, mannitol, ethylene glycol, propylene glycol, and trimethylolpropane.

[0116] The coating liquid may contain inorganic particles in addition to the complex of the hydrotalcite compound and the amino acid. Examples of inorganic particles other than the complex include silica, talc, kaolin, mica, graphite, calcium sulfate, magnesium oxide, and magnesium hydroxide.

[0117] [Application examples other than membranes]

[0118] In addition, the complex of the present invention can be used as an additive added to cosmetics. In other words, one embodiment of the present invention is a cosmetic comprising the complex of the present invention. The complex inhibits the permeation of characteristic molecules such as oxygen and water. Therefore, cosmetics comprising the complex can control the permeability of characteristic molecules such as oxygen and water by adjusting the content of the complex. The complex shows a specific yellowness and reflects light. Therefore, by making a cosmetic comprising the complex, a cosmetic capable of controlling the reflection characteristics of light can be obtained.

[0119] In addition, the composite of the present invention can be used as an additive added to a coating. In other words, one embodiment of the present invention is a coating comprising the composite of the present invention. The composite inhibits the penetration of characteristic molecules such as oxygen and water vapor. Therefore, the coating comprising the composite can control the permeability of characteristic molecules such as oxygen and water vapor by adjusting the content of the composite. The composite has flame retardancy derived from a hydrotalcite compound. Therefore, by preparing a coating comprising the composite, a coating capable of inhibiting combustion can be obtained. In addition, the composite shows a specific yellowness and reflects light. Therefore, by preparing a coating comprising the composite, a coating capable of controlling the reflection characteristics of light can be obtained.

[0120] Furthermore, the composite of the present invention can be used as a resin additive added to a resin. One embodiment of the present invention is a resin composition comprising the composite of the present invention. The resin composition containing the composite as a resin additive can improve strength compared to a resin composition not containing the composite. In other words, by using the composite as a resin additive, a resin composition having a reinforcing effect due to a high aspect ratio can be obtained. In addition, the resin composition containing the composite as a resin additive can be colored to a specified color that matches the yellowness of the composite, depending on the content of the composite.

[0121] In addition, the resin composition containing the composite of the present invention can be molded in accordance with the appropriate use. For example, it can be molded into a tubular shape by extrusion molding. In other words, one embodiment of the present invention is a tube containing the composite of the present invention. The composite inhibits the penetration of characteristic molecules such as inert gases such as helium, oxygen, and moisture. Therefore, the tube containing the composite can control the permeability of characteristic molecules such as inert gases such as helium, oxygen, and moisture by adjusting the content of the composite. For example, a tube obtained by combining the composite of the present invention with a resin with high biocompatibility can be used as various tubes that require gas barrier properties and the like for use in the medical field. As an example of such a tube, a medical catheter can be cited.

[0122] It should be noted that the present invention is not limited to the above-mentioned embodiment, the examples described below, etc., and appropriate combinations, substitutions, changes, etc. can be made without departing from the purpose and gist of the present invention.

[0123] Example

[0124] The present invention will be described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples.

[0125] Example 1

[0126] (Manufacturing of Precursor Hydrotalcite Compounds)

[0127] Ion exchange water is placed in a 1L reaction tank, and a mixed solution of 160mL of 1.5mol / L magnesium chloride aqueous solution, 120mL of 1mol / L aluminum chloride aqueous solution, 90mL of 8mol / L sodium hydroxide aqueous solution, and 60mL of 1mol / L sodium carbonate aqueous solution is dripped into the reaction tank while stirring to obtain a reactant. The pH during the reaction is 9.5. After washing the obtained reactant with water, ion exchange water is added to obtain 700mL of re-emulsified slurry. The obtained re-emulsified slurry is hydrothermally treated at 170°C for 13 hours. Then, the obtained solid is washed with water, dried at 105°C for 16 hours, and crushed. The chemical formula of the obtained powder is Mg: 0.67 Al 0.33 (OH)2(CO3) 0.17 · A hydrotalcite compound represented by 0.50H2O. This hydrotalcite compound is used as a precursor hydrotalcite compound for the production of the composite.

[0128] (Calcination of Precursor Hydrotalcite Compound)

[0129] The obtained precursor hydrotalcite compound was calcined in an electric furnace at 450° C. for 12 hours to obtain a calcined product (complex metal oxide).

[0130] (Solution preparation process)

[0131] 17.5 g of the obtained calcined product was put into a glass beaker, 175 mL of a 2 mol / L aqueous solution of glycine (equivalent to 26.3 g of glycine powder) was added, and the mixture was stirred until uniform. At this time, the molar ratio of glycine / Al2 in the obtained slurry solution was 5.26. Then, ion exchange water was added to a total amount of 700 mL, and the mixture was stirred again until uniform. The slurry concentration at this time was 25 g / L. In addition, the glycine concentration at this time was 0.5 mol / L.

[0132] (Heating process)

[0133] Next, the slurry solution was hydrothermally treated at 100°C for 48 hours while being stirred at 700 rpm. The obtained sample (slurry solution) was slurry-like and white in color, and had no particular odor. Figure 2 A photograph of the slurry solution after the heating step is shown.

[0134] (Washing process ~ Drying process)

[0135] Secondly, ion exchange water was added to the obtained slurry solution to make a total amount of 1750 mL, and a stirrer was used to stir at 400 rpm for 16 hours at room temperature. While maintaining the stirring of the slurry solution, 88.4 mL of a 3.96 mol / L sodium hydroxide aqueous solution was slowly dripped into the slurry solution. The obtained slurry solution was solid-liquid separated to obtain a solid. Furthermore, the obtained solid was dried at 60° C. for 16 hours to obtain the sample (composite) of Example 1. The characteristics of the obtained sample are shown in Table 1 below.

[0136] Example 2

[0137] The sample of Example 2 was obtained in the same manner as in Example 1, except that 14.0 g of the burned product and 140 mL of a 2 mol / L glycine aqueous solution (equivalent to 21.0 g of glycine powder) were used in the solution preparation step. The slurry concentration of the slurry solution in the solution preparation step was 20 g / L, and the glycine concentration was 0.4 mol / L.

[0138] Example 3

[0139] The sample of Example 3 was obtained in the same manner as in Example 1, except that 7.0 g of the burned product and 70 mL of a 2 mol / L glycine aqueous solution (equivalent to 10.5 g of glycine powder) were used in the solution preparation step. The slurry concentration of the slurry solution in the solution preparation step was 10 g / L, and the glycine concentration was 0.2 mol / L.

[0140] Comparative Example 1

[0141] The sample of Comparative Example 1 was obtained in the same manner as in Example 1, except that 70.0 g of the burned product and 700 mL of a 2 mol / L glycine aqueous solution (equivalent to 105.1 g of glycine powder) were used in the solution preparation step and stirring was not performed in the heating step. The slurry concentration of the slurry solution in the solution preparation step was 100 g / L, and the glycine concentration was 2 mol / L.

[0142] Comparative Example 2

[0143] The sample of Comparative Example 2 was obtained in the same manner as in Example 1, except that 70.0 g of the burned product and 266 mL of a 2 mol / L glycine aqueous solution (equivalent to 39.9 g of glycine powder) were used in the solution preparation step and stirring was not performed in the heating step. The slurry concentration of the slurry solution in the solution preparation step was 100 g / L, and the glycine concentration was 0.76 mol / L.

[0144] Comparative Example 3

[0145] The sample of Comparative Example 3 was obtained in the same manner as in Example 1, except that 70.0 g of the burned product was used in the solution preparation step, no glycine aqueous solution was used, stirring was not performed in the heating step, and no washing step was performed. The slurry concentration of the slurry solution in the solution preparation step was 100 g / L, and the glycine concentration was 0 mol / L.

[0146] Comparative Example 4

[0147] The sample of Comparative Example 4 was obtained in the same manner as in Example 1 except that 35.0 g of the burned product and 350 mL of a 2 mol / L glycine aqueous solution (equivalent to 52.5 g of glycine powder) were used in the solution preparation step. The slurry concentration of the slurry solution in the solution preparation step was 50 g / L, and the glycine concentration was 1 mol / L.

[0148] Comparative Example 5

[0149] The sample of Comparative Example 5 was obtained in the same manner as in Example 1 except that 28.0 g of the burned product and 280 mL of a 2 mol / L glycine aqueous solution (corresponding to 42.0 g of glycine powder) were used in the solution preparation step. The slurry concentration of the slurry solution in the solution preparation step was 40 g / L, and the glycine concentration was 0.8 mol / L.

[0150] Comparative Example 6

[0151] The sample of Comparative Example 6 was obtained in the same manner as in Example 1, except that 21.0 g of the burned product and 210 mL of a 2 mol / L glycine aqueous solution (equivalent to 31.5 g of glycine powder) were used in the solution preparation step. The slurry concentration of the slurry solution in the solution preparation step was 30 g / L, and the glycine concentration was 0.6 mol / L.

[0152] Example 4

[0153] (Preparation of coating liquid)

[0154] The solid content concentrations of the sample of Example 1 and a polyvinyl alcohol (PVA) aqueous solution (manufactured by Sigma-Aldrich, Mw 67000, Mowiol (registered trademark) 8-88) were measured, and ion exchange water was added to adjust the composite of the hydrotalcite compound and the glycine compound of Example 1 to 3 wt % and the PVA to 2 wt %, and the mixtures were stirred and mixed to obtain a coating solution.

[0155] (Film Production)

[0156] First, a polyethylene terephthalate (PET) film (manufactured by Toray Industries, Ltd., Lumirror (registered trademark), film thickness 50 μm, product model #50-U483) cut into 55 mm in length and 105 mm in width as a film-like substrate was fixed on a glass plate of an automatic coating device (manufactured by Tester Industries, Ltd., PI-1210 model). Next, a Baker Applicator (manufactured by Yoshimitsu Seiki Co., Ltd., YBA model) was set on the glass plate of the automatic coating device, and the coating liquid was applied to the PET film in a manner that the thickness was uniformly 50 μm. The coating layer formed by the applied coating liquid was dried at room temperature for 16 hours to obtain the film of Example 4.

[0157] Comparative Example 7

[0158] A film of Comparative Example 7 was obtained in the same manner as in Example 4 except that the sample of Comparative Example 1 was used instead of the sample of Example 1.

[0159] Comparative Example 8

[0160] A film of Comparative Example 8 was obtained in the same manner as in Example 4 except that the precursor hydrotalcite compound obtained in the step of "manufacturing a precursor hydrotalcite compound" of Example 1 was used instead of the sample of Example 1 (complex of a hydrotalcite compound and a glycine compound). That is, the film of Comparative Example 8 was a film in which an unexfoliated hydrotalcite compound (unexfoliated HT) was used instead of the complex of a hydrotalcite compound and a glycine compound.

[0161] Comparative Example 9

[0162] A film of Comparative Example 9 was obtained in the same manner as in Example 4 except that the coating liquid was not applied. That is, the film of Comparative Example 9 was a single PET film (film-like substrate) in which a coating layer was not formed using the coating liquid.

[0163] Comparative Example 10

[0164] A film of Comparative Example 10 was obtained in the same manner as in Example 4 except that a coating liquid containing only PVA was used.

[0165] Example 5

[0166] (Film Production)

[0167] The film of Example 5 was obtained in the same manner as in Example 4, except that a polypropylene (PP) film (manufactured by Toyobo Co., Ltd., Pairen (registered trademark) film-OT, film thickness 50 μm, brand P2261) was used as the film substrate and the coating liquid was applied in a manner to have a uniform thickness of 25 μm.

[0168] Example 6

[0169] A film of Example 6 was obtained in the same manner as in Example 5 except that the coating liquid was applied so as to have a uniform thickness of 12.5 μm.

[0170] Comparative Example 11

[0171] A film of Comparative Example 11 was obtained in the same manner as in Example 5 except that the coating liquid was not applied. That is, the film of Comparative Example 11 was a single PP film (film-like substrate) in which a coating layer was not formed using the coating liquid.

[0172] Comparative Example 12

[0173] A film of Comparative Example 12 was obtained in the same manner as in Example 5 except that a coating liquid containing only PVA was used.

[0174] [Various measurements]

[0175] The samples of Examples 1 to 3 and Comparative Examples 1 to 6 were subjected to the following measurements of various physical properties. The results of these measurements are shown in Table 1 below. In addition, photographs were taken of the slurry solutions after the heating process of Examples 1 to 3 and Comparative Examples 1 to 3, and the slurry solutions when the temperature was raised to 100° C. in the heating process of Comparative Examples 4 to 6. The photographs are shown in Table 1. Figure 2 .

[0176] (Viscosity measurement after heating process)

[0177] After adjusting the temperature of the slurry solution to 25°C, the viscosity was measured at the same temperature using a B-type viscometer (DV2T model, manufactured by Brookfield).

[0178] (Measurement of Thickness and Aspect Ratio of Primary Particles of Composite)

[0179] The width and thickness of the primary particles were measured using a scanning probe microscope (SPM-9700HT, manufactured by Shimadzu Corporation). The aspect ratio was determined by the following formula.

[0180] (aspect ratio of primary particle) = (width of primary particle) / (thickness of primary particle)

[0181] In addition, the aspect ratio was calculated for each of 20 arbitrary primary particles, and the average value thereof was defined as the aspect ratio of the sample.

[0182] (Determination of the content of glycine compounds)

[0183] 0.5 g of powder sample dried at 60°C for 16 hours, 5 g of potassium sulfate and 2 g of copper sulfate (II) 5 hydrate were fully mixed, placed in a sample tube, and 15 ml of concentrated sulfuric acid was added. Then, a KjelFlex K-360 / K-425 Speed ​​Digester (Buchi) was used to treat at 470°C for 90 minutes. Furthermore, 10 mL of ion exchange water, 40 mL of 30% sodium hydroxide aqueous solution and 2% boric acid aqueous solution were used to perform steam distillation for 240 seconds. Three drops of a mixed indicator of methyl red and methylene blue were dripped into the obtained distillate, and the distillate was titrated with a 0.1 mol / L hydrochloric acid aqueous solution until the distillate became purple. For a blank test without using a powder sample, titration was also performed in the same manner, and the content of glycine compounds was calculated from the following formulas (I) and (II).

[0184] (Nitrogen N content) [wt%] = ((factor of 0.1 mol / L hydrochloric acid aqueous solution) × (drop amount [ml] - blank [ml]) × 1.401 [mg / ml]) × 100 / powder sample amount [mg] ··· (I) (glycine compound content) [wt%] = (Nitrogen N content) [wt%] × (75.07 [g / mol] / 14.01 [g / mol]) ··· (II)

[0185] (Yellowness (YI value) measurement)

[0186] The powder sample dried at 60°C for 16 hours was crushed, sieved with a mesh of 150 μm, and 0.2 g was placed in a glass reagent bottle. Next, a 10Φ observation port (view port) and a sample stand were used to measure the colorimetric colorimeter (manufactured by Nippon Denshoku Industries Co., Ltd., Color meter ZE6000) that had been pre-calibrated with a standard white plate. A total of 3 measurements were performed, and before each measurement, the reagent bottle was vibrated 10 times. The average value was calculated from the 3 measured values ​​obtained to obtain the Yellow Index value (YI value).

[0187] [Evaluation of film]

[0188] The following various physical properties and the like were measured for the films of Examples 4 to 6 and Comparative Examples 7 to 12. The results of these measurements are shown in Tables 2 and 3 below.

[0189] (Total light transmittance and Haze measurement)

[0190] The film was cut 20 mm from the coating end point, with the coated surface facing the incident light side, and measured using a haze meter (NDH4000, manufactured by Nippon Denshoku Industries Co., Ltd.) to obtain total light transmittance and haze.

[0191] (Oxygen permeability measurement)

[0192] The film was cut into a circular shape with a diameter of about 55 mm, and the gas permeability was measured using a gas permeability measuring device (GTR-11AET, manufactured by GTR Tech Co., Ltd.) The measurement method was based on JIS K 7126-1 Part 1 (differential pressure method) and the measurement was performed under the following conditions.

[0193] ·Measurement temperature: 23.0℃

[0194] Relative humidity: zero

[0195] ·Through area: 15.2cm 2

[0196] ·Measured gas: oxygen

[0197] The oxygen permeability was obtained by analyzing the oxygen permeating through the membrane using a capillary gas chromatography system (GC-2014, manufactured by Shimadzu Corporation). In the oxygen permeability measurement, the measurement and analysis time can be appropriately adjusted according to the gas permeability of the membrane.

[0198] [Table 1]

[0199]

[0200] [Table 2]

[0201] Table 2

[0202]

[0203] [Table 3]

[0204] Table 3

[0205]

[0206] As shown in Tables 1 to 3 and Figure 2 As shown in , the composite of the hydrotalcite compound and the glycine compound of the embodiment of the present invention can form a film (coating layer) having both high gas barrier properties and transparency. On the other hand, the composite of the comparative example is colored yellow-brown or gelled, and cannot form a film having both high gas barrier properties and transparency as in the present invention.

[0207] Industrial Applicability

[0208] The composite of the present invention, the coating liquid containing the composite, and the film having a coating layer formed using the coating liquid can be used, for example, for food packaging films, beverage packaging films, beverage bottles, pharmaceutical packaging films, industrial gas barrier films, and gas separation films. In addition, the composite of the present invention and the coating liquid containing the composite can be suitably used in a wide range of fields such as paper barrier materials, coatings, scratch-resistant materials, cosmetics, and additives.

[0209] Description of Reference Numerals

[0210] 100 membrane manufacturing equipment

[0211] 1 First Can

[0212] 2 Second Can

[0213] 3 The third can

[0214] 41 First Mixer

[0215] 42 Second Mixer

[0216] 43 Third Mixer

[0217] 51 First Pump

[0218] 52 Second Pump

[0219] 53 Third Pump

[0220] 6 Casting die

[0221] 71 First coating roller

[0222] 72 Second coating roller

[0223] 8 Casting tape

[0224] 9 Drying device

[0225] 10 Hot air

[0226] 11 Peeling roller

[0227] 12 Membrane

[0228] 13 Winding device

Claims

1. A complex comprising a hydrotalcite compound and an amino acid having an aspect ratio of 85 or more, characterized in that: The YI value indicating the yellowness of the complex is 0 to 5, and the content of the amino acid relative to the total mass of the complex is greater than 0 mass % and 10.0 mass % or less.

2. The composite body according to claim 1, characterized in that The amino acid is a glycine compound.

3. The composite body according to claim 1, characterized in that The hydrotalcite compound is represented by the following formula (1): (M 2+ ) 1-X (M 3+ ) X (OH)2(A n- ) X / n ·mH2O···(1) In formula (1), M 2+ is a divalent metal cation, M 3+ A is a trivalent metal cation. n- It is an n-valent anion, X is a number satisfying 0.17<X<0.36, n is an integer of 1 to 6, and m is a number satisfying 0<m<1.

80.

4. The composite body according to claim 1, characterized in that The thickness of the primary particle of the composite is 20 nm or less, and the aspect ratio is 100 or more.

5. A coating liquid comprising the composite according to claim 1 and a polymer.

6. The coating solution according to claim 5, characterized in that The polymer is a water-soluble polymer.

7. The coating solution according to claim 6, characterized in that The water-soluble polymer is polyvinyl alcohol.

8. A film having a coating layer formed using the coating solution according to claim 5.

9. The film according to claim 8, characterized in that The coating layer has a thickness of 1 μm or more and 1000 μm or less.