Clear coating composition

The acid value and hydroxyl value are adjusted through the composition of the first acrylic resin, the second acrylic resin, the polyester resin and the melamine resin, and the acid value and hydroxyl value are achieved, and the curing is achieved at a low temperature below 130°C, which solves the problem of insufficient mechanical properties of the transparent coating composition. , suitable for body coating and reduces process costs.

CN119013359APending Publication Date: 2024-11-22KCC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380033403.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-14
Filing Date
2023-04-11
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When the existing transparent coating compositions cure at low temperatures, the mechanical properties are insufficient, making them difficult to be suitable for vehicle body coating, and the process cost is high.

Method used

The composition of the first acrylic resin, the second acrylic resin, the polyester resin and the melamine resin is used to adjust the acid value, hydroxyl value and the curing reaction speed to achieve curing at a low temperature below 130°C, and improve the mechanical properties of the coating film. .

Benefits of technology

The transparent coating composition cured at low temperature has excellent mechanical properties, especially gloss, impact resistance, water resistance and cold chip resistance, which is suitable for use as vehicle body coating, while reducing process costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005077574490000121
    Figure BDA0005077574490000121
  • Figure BDA0005077574490000131
    Figure BDA0005077574490000131
  • Figure BDA0005077574490000132
    Figure BDA0005077574490000132
Patent Text Reader

Abstract

The present invention relates to a clear coating composition comprising a first acrylic resin, a second acrylic resin, a polyester resin and a melamine resin, the first acrylic resin having an acid value of 6 to 13 mgKOH / g and a hydroxyl value of 135 to 155 mgKOH / g, and the second acrylic resin having an acid value of 15 to 25 mgKOH / g and a hydroxyl value of 100 to 130 mgKOH / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a low temperature curable transparent coating composition. Background Art

[0002] Generally, the coating film on the vehicle body should not deteriorate or rust, and should have the durability to maintain the gloss or color of the coating film. Therefore, in terms of the vehicle painting process, the vehicle body that has undergone the pretreatment process is usually electroplated, followed by an intermediate (primer) coating to improve adhesion and smoothness, and a base coating is performed on the intermediate-coated vehicle body to improve the aesthetics of the vehicle body. Thereafter, a clear coating is applied to protect the color of the base coating and improve the appearance, and to protect the base coating from external influences.

[0003] In the coating of the base coating and the coating of the clear coating, usually, after the base coating composition is coated and dried, the clear coating composition is coated, and the clear coating and the base coating are cured together when the clear coating is cured (150°C). Therefore, the existing clear coating composition is designed based on high temperature curing conditions. However, in order to reduce the cost of the coating process, the requirements for shortening the process and curable compositions at low temperatures tend to increase. In this regard, Korean Patent No. 10-0158534 (Patent Document 1) discloses a two-component acrylic polyurethane composition, which is composed of an additive, a main mixture containing an alcohol solvent, and a curing agent mixture containing a polyisocyanate and an ester solvent, and the additive is composed of an acrylic polyol, an ester solvent, a smoothing agent, a slip agent and a wax. However, as shown in Patent Document 1, although the clear coating compositions that can be used under existing low-temperature baking conditions, especially under heat curing conditions below 130° C., include automobile repair coatings and parts coating compositions, the mechanical properties of the prepared coating films are insufficient, which limits their applicability as vehicle body coatings.

[0004] Therefore, it is necessary to research and develop a clear coating composition that can be cured at a low temperature of 130° C. or less and has excellent mechanical properties for a coating film prepared therefrom and is suitable for use as a vehicle body coating.

[0005] [Prior art literature]

[0006] Korean Patent No. 10-0158534 (August 5, 1998) Summary of the invention

[0007] Technical issues

[0008] The present invention aims to provide a transparent coating composition which can be cured at a low temperature below 130°C and can prepare a coating film with excellent mechanical properties.

[0009] Solution to the problem

[0010] In one embodiment, the present invention provides a transparent coating composition, which includes a first acrylic resin, a second acrylic resin, a polyester resin and a melamine resin, wherein the acid value of the first acrylic resin is 6 to 13 mgKOH / g, and the hydroxyl value is 135 to 155 mgKOH / g, and the acid value of the second acrylic resin is 15 to 25 mgKOH / g, and the hydroxyl value is 100 to 130 mgKOH / g.

[0011] Effects of the Invention

[0012] According to the clear coating composition of the present invention, the coating process can be carried out at a lower temperature than the prior art, 130°C or lower, in terms of the thermal curing temperature of the coating process, thereby saving the cost required for the coating process, which is very economical. In addition, the coating film prepared by the composition has excellent mechanical properties, especially gloss, impact resistance, water resistance, cold crack resistance, etc., which is advantageous for use as a vehicle body coating. DETAILED DESCRIPTION

[0013] Hereinafter, the present invention will be described in detail.

[0014] In this specification, "weight average molecular weight (Mw)" and "number average molecular weight (Mn)" are measured by a commonly known method in the technical field to which the present invention belongs, for example, by a method such as gel permeation chromatography (GPC).

[0015] In the present specification, the "glass transition temperature (Tg)" is measured by a generally known method in the technical field to which the present invention belongs, for example, it can be measured by differential scanning calorimetry (DSC) or the like.

[0016] In this specification, functional group values ​​such as "acid value (Av)" and "hydroxyl value (OHv)" are measured by a commonly known method in the technical field to which the present invention belongs, for example, by titration or the like.

[0017] A transparent coating composition according to one embodiment of the present invention includes a first acrylic resin, a second acrylic resin, a polyester resin and a melamine resin, wherein the first acrylic resin has an acid value of 6 to 13 mgKOH / g and a hydroxyl value of 135 to 155 mgKOH / g, and the second acrylic resin has an acid value of 15 to 25 mgKOH / g and a hydroxyl value of 100 to 130 mgKOH / g.

[0018] As described above, when two acrylic resins having different acid values ​​and hydroxyl values ​​are used, the appearance characteristics and mechanical properties of the coating film can be improved by adjusting the curing reaction rate and the crosslinking density, and curing can be performed at a low temperature of 130° C. or less.

[0019] For example, the different acid values ​​of the two acrylic resins have the following effects, namely, by adjusting the curing reaction rate and surface tension of the clear coating composition of the present invention, it can be cured at a low temperature of below 130°C, and the different hydroxyl values ​​of the two acrylic resins have the effect of adjusting the crosslinking density of the coating film to improve the adhesion and mechanical properties.

[0020] <First acrylic resin>

[0021] The first acrylic resin, as the main resin (primary resin) of the clear coating composition according to the present invention, has a function of improving the appearance characteristics such as durability and glossiness of the prepared coating film.

[0022] The first acrylic resin may be directly synthesized according to a known method or a commercially available product. The first acrylic resin may be prepared by polymerizing, for example, one or more of a first vinyl monomer and a first (meth)acrylate-based monomer.

[0023] As the first vinyl monomer, one or more selected from the group consisting of, for example, styrene, methylstyrene, dimethylstyrene, fluorostyrene, ethoxystyrene, methoxystyrene, phenylene vinyl ketone, vinyl tert-butylbenzoate, vinyl cyclohexanoate, vinyl acetate, vinyl pyrrolidone, vinyl chloride, vinyl alcohol, acetoxystyrene, tert-butylstyrene and vinyltoluene can be used.

[0024] The first (meth)acrylate-based monomer may include one or more selected from the group consisting of a (meth)acrylate monomer not containing a hydroxyl group and a (meth)acrylate monomer containing a hydroxyl group.

[0025] The (meth)acrylate monomer not containing a hydroxyl group may include one or more selected from the group consisting of, for example, (meth)acrylic acid, methyl(meth)acrylic acid, (meth)acrylate, methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, isopropyl(meth)acrylate, butyl(meth)acrylate, isobutyl(meth)acrylate, tert-butyl(meth)acrylate, pentyl(meth)acrylate, hexyl(meth)acrylate, heptyl(meth)acrylate, isooctyl(meth)acrylate, octyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, isodecyl(meth)acrylate, decyl(meth)acrylate, dodecyl(meth)acrylate, isobornyl(meth)acrylate and lauryl(meth)acrylate.

[0026] The hydroxyl group-containing (meth)acrylate monomer may be, for example, a hydroxyalkyl-containing (meth)acrylate, and specifically may include one or more selected from the group consisting of 2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate.

[0027] The first acrylic resin can be prepared by, for example, a free radical polymerization method, and the physical properties, that is, the weight average molecular weight (Mw), hydroxyl value (OHv), acid value (Av), etc., can be adjusted according to the initiator and the polymerization time.

[0028] The solid content (NV) of the first acrylic resin may be 50 to 70% by weight or 55 to 65% by weight relative to the total weight of the resin. When the solid content of the first acrylic resin is within the above range, the storage stability of the resin and the storage stability of the transparent coating composition can be improved, and the workability is excellent. If the solid content of the first acrylic resin is less than the above range, the viscosity becomes too low, which has the problem of insufficient workability of the transparent coating composition containing it. If it exceeds the above range, the viscosity of the first acrylic resin is too high, which reduces the stability during the reaction and deteriorates the dispersion stability, so that agglomeration may occur over time.

[0029] The viscosity of the first acrylic resin at 25° C. may be 1000 to 2350 cps or 1050 to 2300 cps. When the viscosity of the first acrylic resin at 25° C. is within the above range, the viscosity of the transparent coating composition is appropriate, which has the effect of improving workability. If the viscosity of the first acrylic resin at 25° C. is less than the above range, the viscosity of the composition is too low, and the prepared coating film is not formed, resulting in low fluidity, adhesion and scratch resistance of the paint. When it exceeds the above range, the appearance characteristics of the prepared coating film may be reduced due to insufficient workability of the composition.

[0030] The acid value (Av) of the first acrylic resin may be 6 mgKOH / g to 13 mgKOH / g or 8 to 10 mgKOH / g. When the acid value of the first acrylic resin is within the range, the reactivity of the composition containing it is adjusted, so that the appearance characteristics of the coating film prepared therefrom can be improved. When the acid value of the first acrylic resin is less than the range, the appearance and mechanical properties of the prepared coating film may deteriorate due to the low curing reaction rate. If it exceeds the range, the viscosity of the composition may increase as the cohesion of the resin increases, and the workability and room temperature storage properties may be reduced.

[0031] The hydroxyl value (OHv) of the first acrylic resin may be 135 to 155 mgKOH / g or 140 to 150 mgKOH / g. When the hydroxyl value of the first acrylic resin is within the range, the durability and weather resistance of the coating film are improved. If the hydroxyl value of the first acrylic resin is less than the range, the coating film formed by the cross-linking reaction with the curing agent is insufficient, so that the mechanical properties such as the hardness of the coating film are reduced. If it exceeds the range, due to the formation of over-curing, the coating film becomes brittle, thereby reducing elasticity, and the problem of insufficient appearance characteristics of the prepared coating film may occur.

[0032] The glass transition temperature (Tg) of the first acrylic resin may be 10 to 13° C. or 11 to 12° C. When the glass transition temperature of the first acrylic resin is within the above range, the hardness and solvent resistance of the coating film are improved. If the glass transition temperature of the first acrylic resin is less than the above range, the hardness and solvent resistance of the prepared coating film are insufficient due to the reduction of the drying speed and crosslinking density of the coating film. When the glass transition temperature exceeds the above range, the appearance characteristics and chipping resistance of the prepared coating film are insufficient due to the brittleness of the coating film.

[0033] The weight average molecular weight (Mw) of the first acrylic resin may be 10000 to 20000 g / mol or 14000 to 16000 g / mol. When the weight average molecular weight of the first acrylic resin is within the range, the prepared coating film may have excellent long-term physical properties such as durability and weather resistance. If the weight average molecular weight of the first acrylic resin is less than the range, the weather resistance and scratch resistance of the prepared coating film are insufficient due to the small molecular weight. If the weight average molecular weight of the first acrylic resin is less than the range, the fluidity may be reduced as the molecular weight increases, thereby the workability of the transparent coating composition containing the first acrylic resin is poor, and the surface smoothness is not excellent, and the problem of difficulty in preparing a coating film with excellent appearance may occur.

[0034] The composition may include the first acrylic resin in an amount of 33 to 50% by weight or 37 to 46% by weight based on the total weight of the clear coating composition. When the first acrylic resin is included within the above content range, it has the effect of improving the adhesion and durability of the coating film. If the content of the first acrylic resin is less than the above range, the adhesion, glossiness and durability of the coating film may be reduced due to poor drying properties. If it exceeds the above range, the coating workability and paint fluidity of the composition may be insufficient due to rapid drying, thereby reducing the appearance and scratch resistance of the coating film.

[0035] <Second acrylic resin>

[0036] The second acrylic resin, as an auxiliary resin of the clear coating composition according to the present invention, has a function of improving the appearance characteristics such as durability and glossiness of the prepared coating film.

[0037] The second acrylic resin is the same as the first acrylic resin except for the following description.

[0038] The solid content (NV) of the second acrylic resin may be 40 to 60% by weight or 45 to 55% by weight relative to the total weight of the resin. When the solid content of the second acrylic resin is within the above range, the storage stability of the resin and the storage stability of the clear coating composition can be improved, and the workability is excellent. If the solid content of the second acrylic resin is less than the above range, the viscosity becomes too low, which has the problem of insufficient workability of the clear coating composition containing it. If it exceeds the above range, the viscosity of the second acrylic resin is too high, so that the stability during the reaction is reduced and the dispersion stability is deteriorated, so that aggregation may occur over time.

[0039] The viscosity of the second acrylic resin at 25° C. may be 50 to 110 cps or 60 to 100 cps. When the viscosity of the second acrylic resin at 25° C. is within the above range, the viscosity of the clear coating composition is appropriate, which has the effect of improving workability. If the viscosity of the second acrylic resin at 25° C. is less than the above range, the viscosity of the composition is too low, and the prepared coating film is not formed, resulting in low fluidity, adhesion and scratch resistance of the paint. If it exceeds the above range, the appearance characteristics of the prepared coating film may be reduced due to insufficient workability of the composition.

[0040] The acid value (Av) of the second acrylic resin may be 15 to 25 mgKOH / g or 17 to 21 mgKOH / g. When the acid value of the second acrylic resin is within the range, the reactivity of the composition containing it is adjusted, so that the appearance characteristics of the coating film prepared therefrom can be improved. When the acid value of the second acrylic resin is less than the range, the appearance of the prepared coating film may deteriorate due to the low curing reaction rate. If it exceeds the range, the viscosity of the composition may increase as the cohesiveness of the resin increases, and the problem of reduced workability and room temperature storage may occur.

[0041] The hydroxyl value (OHv) of the second acrylic resin may be 100 to 130 mgKOH / g or 110 to 120 mgKOH / g. When the hydroxyl value of the second acrylic resin is within the range, the durability and weather resistance of the coating film are improved. If the hydroxyl value of the second acrylic resin is less than the range, the coating film formed by the cross-linking reaction with the curing agent is insufficient, so that the mechanical properties such as the hardness of the coating film are reduced. If it exceeds the range, the coating film becomes brittle due to over-curing, thereby reducing elasticity, and the problem of insufficient appearance characteristics of the prepared coating film may occur.

[0042] The glass transition temperature (Tg) of the second acrylic resin may be -7 to -3°C or -6 to -4°C. When the glass transition temperature of the second acrylic resin is within the above range, the hardness and solvent resistance of the coating film are improved. If the glass transition temperature of the second acrylic resin is less than the above range, the drying speed and crosslinking density of the coating film are reduced, and the hardness and solvent resistance of the prepared coating film are insufficient. If it exceeds the above range, the coating film becomes brittle, which may cause the appearance characteristics and crack resistance of the coating film to be insufficient.

[0043] The weight average molecular weight (Mw) of the second acrylic resin can be 7000 to 9000 g / mol or 7500 to 8500 g / mol. When the weight average molecular weight of the second acrylic resin is within the range, the prepared coating film can have excellent long-term physical properties such as durability and weather resistance. If the weight average molecular weight of the second acrylic resin is less than the range, the weather resistance and scratch resistance of the prepared coating film are insufficient due to the small molecular weight. If it exceeds the range, the fluidity will be reduced as the molecular weight increases, so that the workability of the transparent coating composition containing it is poor, and the surface smoothness is not excellent, and the problem of being difficult to prepare a coating film with excellent appearance may occur.

[0044] The second acrylic resin may be included in an amount of 0.1 to 2% by weight or 0.2 to 1.5% by weight based on the total weight of the clear coating composition. When the second acrylic resin is included within the above content range, it has the effect of improving the adhesion and durability of the coating film. If the content of the second acrylic resin is less than the above range, the adhesion, glossiness and durability of the coating film may be reduced due to poor drying properties. If it exceeds the above range, the coating workability and paint fluidity of the composition may be insufficient due to rapid drying, thereby reducing the appearance and scratch resistance of the coating film.

[0045] <Polyester resin>

[0046] The polyester resin has the functions of imparting flexibility to the clear coating composition, increasing the crosslinking density, and improving the mechanical properties of the prepared coating film, such as cold crack resistance, impact resistance, and scratch resistance.

[0047] The polyester resin can be prepared by reacting a carboxylic acid compound with a diol compound. For example, the polyester resin can be prepared by reacting one or more carboxylic acid compounds selected from adipic acid (AA), isophthalic acid (IPA), trimellitic anhydride (TMA), alicyclic acid, phthalic anhydride, isophthalic acid, terephthalic acid, succinic acid, adipic acid, fumaric acid, maleic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride and derivatives thereof with one or more diol compounds selected from 1,6-hexanediol (1,6-HD), neopentyl glycol (NPG), trimethylolpropane (TMP), ethylene glycol, propylene glycol, diethylene glycol, butanediol, 1,4-hexanediol and 3-methylpentanediol.

[0048] Polyester resin can be prepared by condensation reaction of acid and alcohol, and physical properties such as weight average molecular weight (Mw), hydroxyl value (OHv), acid value (Av) can be adjusted by adjusting the ratio of acid and alcohol.

[0049] The solid content (NV) of the polyester resin may be 60 to 80% by weight or 65 to 75% by weight relative to the total weight of the resin. When the solid content of the polyester resin is within the above range, the storage stability of the resin and the storage stability of the clear coating composition can be improved, and the workability is excellent. If the solid content of the polyester resin is less than the above range, the viscosity becomes too low, which has the problem of insufficient workability of the clear coating composition containing it. If it exceeds the above range, the viscosity of the polyester resin is too high, which reduces the stability during the reaction and deteriorates the dispersion stability, so that aggregation may occur over time.

[0050] The viscosity of the polyester resin at 25°C may be 1700 to 2750 cps or 1750 to 2700 cps. When the viscosity of the polyester resin at 25°C is within the above range, the viscosity of the clear coating composition is appropriate, which has the effect of improving workability. If the viscosity of the polyester resin at 25°C is less than the above range, the viscosity of the composition is too low, and the prepared coating film is not formed, resulting in low fluidity, adhesion and scratch resistance of the paint. When it exceeds the above range, the workability of the composition is insufficient, and the appearance characteristics of the prepared coating film may be reduced.

[0051] The acid value (Av) of the polyester resin may be 15 to 30 mgKOH / g or 20 to 25 mgKOH / g. When the acid value of the polyester resin is within the above range, the weather resistance of the coating film is improved. If the acid value of the polyester resin is less than the above range, the coating film is not formed sufficiently through the cross-linking reaction with the curing agent, so that the mechanical properties such as the hardness of the coating film are reduced. If it exceeds the above range, the coating film becomes brittle (brittle) due to over-curing, thereby reducing the elasticity, and the appearance characteristics, water resistance and scratch resistance of the prepared coating film may be insufficient.

[0052] The hydroxyl value (OHv) of the polyester resin may be 120 to 155 mgKOH / g or 130 to 145 mgKOH / g. When the hydroxyl value of the polyester resin is within the range, the reactivity with the melamine resin may be improved, so that the crosslinking density of the coating film is increased, which has the effect of improving mechanical properties, appearance and chemical resistance. If the hydroxyl value of the polyester resin is less than the range, the crosslinking density is insufficient due to insufficient reactivity with the melamine resin, and the durability and chemical resistance of the prepared coating film are low. If it exceeds the range, the coating film becomes brittle due to over-curing, and the appearance and scratch resistance may be reduced.

[0053] The glass transition temperature (Tg) of the polyester resin may be 0.1 to 2° C. or 0.4 to 1.2° C. When the glass transition temperature of the polyester resin is within the above range, the glossiness and hardness of the coating film are improved. If the glass transition temperature of the polyester resin is less than the above range, the drying speed of the clear coating composition is delayed, and the solvent resistance and chipping resistance of the prepared coating film are insufficient. If it exceeds the above range, the coating film becomes brittle, which may cause the appearance characteristics and hardness of the coating film to be insufficient.

[0054] The weight average molecular weight (Mw) of the polyester resin may be 4000 to 6000 g / mol or 4500 to 5500 g / mol. When the weight average molecular weight of the polyester resin is within the above range, the smoothness of the transparent coating composition can be improved, a soft coating film can be formed, and the scratch resistance and hardness can be improved. If the weight average molecular weight of the polyester resin is less than the above range, the mechanical properties of the prepared coating film are low due to the small molecular weight. If it exceeds the above range, as the molecular weight increases, the fluidity decreases, making the coating film brittle, and the problem of reduced smoothness and low scratch resistance may occur.

[0055] The composition may contain the polyester resin in an amount of 2 to 9 wt % or 3 to 8 wt % based on the total weight of the clear coating composition. When the polyester resin is contained within the above content range, the scratch resistance of the appearance and the smoothness of the coating film are improved. If the content of the polyester resin in the composition is less than the above range, the appearance and scratch resistance may be reduced due to the low crosslinking density. If the content exceeds the above range, the viscosity of the composition is too high, the workability and drying properties may be reduced, and the appearance and mechanical properties may be reduced.

[0056] <Melamine resin>

[0057] The melamine resin, as a curing agent, cures the composition by cross-linking reaction with the components of the clear coating composition, and has the effect of increasing the hardness of the prepared coating film.

[0058] The melamine resin may be an alkylated melamine resin, and a product directly synthesized according to a known method or a commercially available product may be used.

[0059] The melamine resin may include one or more selected from the group consisting of, for example, methoxymethylmelamine, methylmelamine, butylmelamine, isobutoxymelamine, butoxymelamine, hexamethylolmelamine, hexamethoxymethylmelamine, hexabutoxymethylmelamine, hexamethoxybutoxymethylmelamine, and iminomethoxymethylmelamine.

[0060] Examples of commercially available melamine resins include CYMEL-325, CYMEL-303, CYMEL-1161, and CYMEL-1168 from CYTEC, and LUWIPAL 012 and LUWIPAL 072 from BASF.

[0061] The solid content (NV) of the melamine resin may be 50 to 70% by weight or 55 to 65% by weight relative to the total weight of the resin. When the solid content of the melamine resin is within the above range, the workability of the clear coating composition is improved. If the solid content of the melamine resin is less than the above range, the viscosity becomes too low and the fluidity is low, which has the problem of insufficient workability of the clear coating composition containing it. If it exceeds the above range, the viscosity is too high, which reduces the stability during the reaction and deteriorates the dispersion stability, so that coagulation may be generated in the clear coating composition over time.

[0062] The viscosity of the melamine resin at 25° C. may be 350 to 600 cps or 400 to 550 cps. When the viscosity of the melamine resin at 25° C. is within the above range, the gloss and appearance are excellent. If the viscosity of the melamine resin at 25° C. is less than the above range, the coating film may not be formed due to the low viscosity, resulting in low adhesion and scratch resistance of the coating film. When the viscosity exceeds the above range, the workability of the composition may deteriorate, resulting in a problem of insufficient appearance characteristics of the prepared coating film.

[0063] Moreover, the acid value (Av) of the melamine resin may be 0.1 to 3 mgKOH / g or 0.1 to 2 mgKOH / g. When the acid value of the melamine resin is less than the above range, the hardness and appearance characteristics of the prepared coating film may be low due to the low curing reaction rate. If it exceeds the above range, the water resistance may be low as the hydrophilicity increases.

[0064] The composition may contain melamine resin in an amount of 20 to 33% by weight or 23 to 30% by weight based on the total weight of the clear coating composition. When the content of melamine resin is within the above range, the crosslinking density can be increased, thereby increasing the adhesion and hardness of the prepared coating film. If the content of melamine resin is less than the above range, the hardness and appearance characteristics may be reduced due to low curability. If the content exceeds the above range, the coating film may become brittle due to excessive curability, and the adhesion, impact resistance and scratch resistance may be reduced.

[0065] <Acrylic anti-sagging agent>

[0066] In order to adjust the sag property of the clear coating composition, an acrylic anti-sagging agent may be included.

[0067] The acrylic anti-sagging agent can be directly synthesized according to a known method or a commercially available product. The acrylic anti-sagging agent can be prepared by polymerizing, for example, one or more of a second vinyl monomer and a second (meth)acrylate monomer.

[0068] As another example, the acrylic anti-sagging agent may also be prepared by reacting a second vinyl monomer, a second (meth)acrylate monomer, and benzylamine, and may have a chemical structure having a needle-shaped diurea group.

[0069] As the second vinyl monomer, one or more selected from the group consisting of, for example, styrene, methylstyrene, dimethylstyrene, fluorostyrene, ethoxystyrene, methoxystyrene, phenylene vinyl ketone, vinyl tert-butylbenzoate, vinyl cyclohexanoate, vinyl acetate, vinyl pyrrolidone, vinyl chloride, vinyl alcohol, acetoxystyrene, tert-butylstyrene and vinyltoluene can be used.

[0070] The second (meth)acrylate-based monomer may include one or more selected from the group consisting of a (meth)acrylate monomer not containing a hydroxyl group and a (meth)acrylate monomer containing a hydroxyl group.

[0071] The (meth)acrylate monomer not containing a hydroxyl group may include one or more selected from the group consisting of, for example, (meth)acrylic acid, methyl(meth)acrylic acid, (meth)acrylate, methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, isopropyl(meth)acrylate, butyl(meth)acrylate, isobutyl(meth)acrylate, tert-butyl(meth)acrylate, pentyl(meth)acrylate, hexyl(meth)acrylate, heptyl(meth)acrylate, isooctyl(meth)acrylate, octyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, isodecyl(meth)acrylate, decyl(meth)acrylate, dodecyl(meth)acrylate, isobornyl(meth)acrylate and lauryl(meth)acrylate.

[0072] The hydroxyl group-containing (meth)acrylate monomer may be, for example, a hydroxyalkyl-containing (meth)acrylate, and specifically may include one or more selected from the group consisting of, for example, 2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate.

[0073] The acrylic anti-sagging agent can be prepared by, for example, a free radical polymerization method, and the physical properties such as the weight average molecular weight (Mw), hydroxyl value (OHv), and acid value (Av) can be adjusted by the initiator and the polymerization time.

[0074] The solid content (NV) of the acrylic anti-sagging agent may be 50 to 70% by weight or 55 to 65% by weight relative to the total weight of the resin. When the solid content of the acrylic anti-sagging agent is within the above range, the storage stability of the resin and the storage stability of the clear coating composition can be improved, and the workability is excellent. If the solid content of the acrylic anti-sagging agent is less than the above range, the viscosity becomes too low, which has the problem of insufficient workability of the clear coating composition containing it. If it exceeds the above range, the viscosity of the acrylic resin is too high, which reduces the stability during the reaction and deteriorates the dispersion stability, so that agglomeration may occur over time.

[0075] The viscosity of the acrylic anti-sagging agent at 25°C may be 5500 to 13500 cps or 6000 to 13000 cps. When the viscosity of the acrylic anti-sagging agent at 25°C is within the above range, the viscosity of the base coating composition is appropriate, which has the effect of improving workability. If the viscosity of the acrylic anti-sagging agent at 25°C is less than the above range, the viscosity of the composition is too low, and the prepared coating film is not formed, resulting in low fluidity, adhesion and scratch resistance of the paint. When it exceeds the above range, the appearance characteristics of the prepared coating film may be reduced due to insufficient workability of the composition.

[0076] The composition may contain an acrylic anti-sagging agent in an amount of 5 to 9% by weight or 6 to 8% by weight based on the total weight of the clear coating composition. When the acrylic anti-sagging agent is contained within the above content range, it has an effect of improving the sagging property of the clear coating composition. If the content of the acrylic anti-sagging agent is less than the above range, the sag property of the clear coating composition containing it is insufficient due to poor drying property, thereby reducing workability. If the content exceeds the above range, the coating workability and paint fluidity of the composition may be reduced due to rapid drying, and the viscosity of the clear coating composition may be increased, thereby deteriorating the storage stability and appearance.

[0077] <Additives>

[0078] The clear coating composition according to one embodiment of the present invention may further contain additives such as a moisture absorbent, a leveling agent, a defoamer, an antioxidant, an ultraviolet absorber, and a catalyst. The additives are not particularly limited as long as they are additives that can be generally added to a clear coating composition.

[0079] Moisture absorbents have the function of absorbing moisture and improving storage properties.

[0080] The leveling agent has the function of imparting leveling and wettability to the prepared coating film. The leveling agent can be a cationic surfactant, an anionic surfactant or a nonionic surfactant, for example, it can include a nonionic surfactant.

[0081] The defoamer has the function of inhibiting the generation of bubbles when preparing the coating, inhibiting or even eliminating the phenomenon of pinholes or popping caused when forming the coating film. Moreover, the defoamer is not particularly limited as long as it is a defoamer that can be generally used in the coating composition. For example, commercially available products of the defoamer include BYK-011, BYK-015, BYK-072, Air Product's DF-21, Munzing's agitan 281, and San Nopco's Foamster-324.

[0082] The antioxidant has the function of preventing oxidation of the prepared coating and improving storage properties. The antioxidant has a solid content (NV) of 9.5 to 10.5% by weight, a specific gravity of 0.85 to 0.95, and an acid value of 47 to 49 mgKOH / g.

[0083] The UV absorber has the function of blocking the UV rays reaching the prepared coating film, thereby ultimately improving the weather resistance of the coating film. The UV absorber has a solid content (NV) of 80 to 100% by weight, a specific gravity of 1.0 to 1.2, an acid value of 47 to 49 mgKOH / g, and a viscosity of 2500 to 3500 cps at 25°C.

[0084] The ultraviolet absorber may be a benzotriazole ultraviolet absorber, for example, α-[3-[3-(2H-Benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl]-ω-hydroxypoly(oxy-1,2-ethanediyl) y-1,2-ethanediyl)), α-[3-[3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl]-ω-[3-[3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropoxy]poly(oxy-1,2-ethanediyl) Benzotriazole ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers such as 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropoxy]poly(oxy-1,2-ethanediyl) and 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxymethylester.

[0085] The catalyst has the function of preventing the unstable solidification of the clear coating composition and improving the curing property, thereby improving the mechanical properties of the coating film prepared therefrom. For example, catalysts such as amino-containing phosphate compounds or dodecylbenzenesulfonic acid compounds can be cited. The solid content (NV) of the catalyst can be 72 to 76% by weight, the specific gravity can be 0.95 to 1.0, and the acid value (Av) can be 120 to 140 mgKOH / g.

[0086] The content of the additive is not particularly limited as long as it is within the range that can be generally included in a clear coating composition. For example, the composition may contain the additive in an amount of 1 to 10 wt % or 2 to 8 wt % based on the total weight of the clear coating composition.

[0087] <Solvent>

[0088] The transparent coating composition according to one embodiment of the present invention may further include a solvent. The solvent may have the function of adjusting the viscosity of the composition, improving the drying property, and improving the appearance characteristics and spreadability of the prepared coating film.

[0089] The solvent is not particularly limited as long as it is a solvent that can be generally used in a clear coating composition, and may include one or more selected from the group consisting of, for example, aromatic hydrocarbon solvents, acetate solvents, alcohol solvents, and propionate solvents. Specifically, the solvent may include aromatic hydrocarbon solvents such as toluene, xylene, and xylene; acetate solvents such as 1-methoxy-2-propyl acetate, methyl acetate, ethyl acetate, n-propyl acetate, n-butyl acetate, methyl glutarate, methyl succinate, methyl adipate, dimethyl glutarate, dimethyl succinate, dimethyl adipate, propylene glycol methyl ether acetate (PMA), butyl carbitol acetate, and butyl cellosolve acetate; alcohol solvents such as n-butanol, propanol, 1-methoxy-2-propanol, and 2-butoxyethanol; ketone solvents such as acetone, methyl ethyl ketone, methyl butyl ketone, and methyl isobutyl ketone; and propionate solvents such as ethyl ethoxypropionate. Furthermore, commercially available products of aromatic hydrocarbon solvents include Kocosol#100, Kocosol#150, and the like.

[0090] The composition may contain a solvent in an amount of 1 to 50% by weight or 3 to 30% by weight based on the total weight of the clear coating composition. When the solvent is contained within the above range, the viscosity of the composition can be appropriately adjusted, thereby improving workability and drying properties. If the content of the solvent in the clear coating composition is less than the above range, the workability of the composition is insufficient due to the high solid content in the composition. If the content exceeds the above range, the solid content of the prepared clear coating composition is low, the fluidity is increased, and the appearance and adhesion of the prepared coating film may be insufficient.

[0091] The solid content of the clear coating composition of the present invention may be 50 to 60% by weight or 52 to 58% by weight. When the solid content of the clear coating composition of the present invention is within the above range, it has the advantage of making the coating workability of the composition appropriate. If the solid content of the clear coating composition of the present invention is less than the above range, there is a problem of reduced solid content leading to low curing reactivity. If it exceeds the above range, due to the high solid content, the workability of the clear coating composition may be reduced.

[0092] The clear coating composition of the present invention may have a viscosity of 35 to 55 seconds, 40 to 50 seconds, or 42 to 47 seconds based on Ford Cup No. 4. If the viscosity of the clear coating composition of the present invention is less than the above range, problems such as dripping from a vertical surface may occur, and if it exceeds the above range, the viscosity of the composition is high, the appearance characteristics of the coating film prepared therefrom may be reduced, or a load may be applied to a coating machine, which may cause a malfunction of the coating machine.

[0093] As mentioned above, the heat curing temperature of the coating process of the clear coating composition according to the present invention can be performed at a low temperature of 130°C or less, which is lower than the temperature of the prior art, and the cost required for the coating process can be saved, which is very economical. In addition, the coating film prepared by the clear coating composition according to the present invention has excellent mechanical properties, especially gloss, impact resistance, water resistance, cold crack resistance, etc., which is advantageous for use as a vehicle body coating.

[0094] The present invention will be described in more detail below by way of examples, but these examples are only used to help understand the present invention, and the scope of the present invention is not limited to these examples in any way.

[0095] [Example]

[0096] Preparation of Clear Coating Compositions of Examples and Comparative Examples

[0097] The components were stirred and mixed in the amounts shown in Tables 1 to 3 to prepare a clear coating composition having a viscosity of 43 seconds based on Ford Cup No. 4.

[0098]

Table 1

[0099]

[0100]

Table 2

[0101]

[0102]

Table 3

[0103]

[0104]

[0105] The physical properties, manufacturers and / or product names of the components used in the Examples and Comparative Examples are shown in Table 4 below.

[0106]

Table 4

[0107]

[0108]

[0109] Test example: Evaluation of properties of prepared coating films

[0110] The sample was coated with a primer coating (manufacturer: KCC, product name: FU2290) and cured at 140°C for 20 minutes to form a primer coating film with a thickness of 40 μm. Then, a base coating (manufacturer: KCC, product name: WT3062) was applied on the primer coating film by bell spray, and hot air was blown at 80°C for 3 minutes to evaporate the residual water in the coating to form a base coating film with a thickness of 15 μm. Then, the clear coating composition prepared in the examples and comparative examples was applied on the base coating film and cured at 130°C for 20 minutes to form a clear coating film with a thickness of 40 μm, thereby preparing a final coating film.

[0111] The appearance characteristics and physical properties of the final coating film were measured by the method described below, and the results are shown in Tables 5 to 7.

[0112] (1) Painting workability

[0113] The coating workability was evaluated by observing the spray state when the coating was discharged and the wettability with respect to the base material.

[0114] The observed conditions were evaluated as excellent (◎), good (○), fair (△), or poor (×).

[0115] (2) Coating appearance

[0116] The gloss (LU), brightness (SH) and orange peel (OP) of the prepared final coating film were measured using Wave Scan DOI (BYK Gardner), which is an automotive appearance tester. The comprehensive appearance evaluation value (CF) was calculated using the following mathematical formula 1 using the measured physical properties.

[0117] [Mathematical formula 1]

[0118] CF=LU×0.15+SH×0.35+OP×0.5

[0119] CF was measured and calculated in a horizontal and vertical manner. As the horizontal / vertical value of CF, when CF was greater than or equal to 65, it was evaluated as excellent (◎), when CF was greater than or equal to 60 and less than 65, it was evaluated as good (○), when CF was greater than or equal to 55 and less than 60, it was evaluated as fair (△), and when CF was less than 55, it was evaluated as poor (×).

[0120] (3) Glossiness

[0121] In order to measure the gloss (GLOSS, %) reflected from the coating film, a gloss meter (BYK Gardner) was used to measure the gloss at 20° of the final coating film.

[0122] According to the measurement results, when the glossiness is greater than or equal to 90%, it is evaluated as excellent (◎), when the glossiness is greater than or equal to 89% and less than 90%, it is evaluated as good (○), when the glossiness is greater than or equal to 87% and less than 89%, it is evaluated as average (△), and when the glossiness is less than 87%, it is evaluated as poor (×).

[0123] (4) Adhesion

[0124] After the base coating composition and the clear coating compositions of Examples and Comparative Examples were applied and cured, adhesion was evaluated using a checkerboard method.

[0125] Specifically, by the checkerboard method, after the recoating coating film is scratched with a knife blade to form 100 squares with a width of 2 mm and a length of 2 mm, the squares are separated using a tape to measure the adhesion. At this time, when 100% of the 100 squares are completely connected, the measured adhesion is evaluated as excellent (◎), when the remaining squares are greater than or equal to 70% and less than 100%, the measured adhesion is evaluated as good (○), when the remaining squares are greater than or equal to 50% and less than 70%, the measured adhesion is evaluated as general (△), and when the remaining squares are less than 50%, the measured adhesion is evaluated as poor (×).

[0126] (5) Impact resistance

[0127] The final coating film was evaluated for impact resistance according to ASTM D 2794. A DuPont impact tester was used to drop a 500 g weight onto the sample at a height varying from 30 cm to 50 cm, and the appearance of the coating film was observed.

[0128] The observation results show that when the falling height of the heavy object is greater than or equal to 50 cm, if the coating film does not show cracks or peeling, it is evaluated as excellent (◎); when the falling height of the heavy object is greater than or equal to 30 cm and less than 50 cm, if the coating film shows cracks or peeling, it is evaluated as good (○); when the falling height of the heavy object is greater than or equal to 20 cm and less than 30 cm, if the coating film shows cracks or peeling, it is evaluated as fair (△); when the falling height of the heavy object is less than 20 cm, if the coating film shows cracks or peeling, it is evaluated as poor (×).

[0129] (6) Water resistance

[0130] The final coating film was deposited in a constant temperature water bath at 40° C. for 240 hours and left at room temperature for 1 hour. The adhesion was evaluated by the checkerboard method and the color change was confirmed with the naked eye.

[0131] Specifically, the adhesion was measured in the same manner as the checkerboard method described in Item (4). The same evaluation criteria were applied to evaluate the water resistance of the coating film.

[0132] (7) Paint fluidity

[0133] A sample having a base coating film was vertically suspended on a steel plate having a hole having a diameter of 5 mm, and the clear coating composition of the examples and comparative examples was applied. After drying and curing, the surface of the prepared coating film was observed to evaluate the coating fluidity of the composition.

[0134] Specifically, it was observed that the paint was condensed at the lower end of the hole, and the thickness (μm) of the coating film at the starting point where the flow was observed to occur was recorded as the critical film thickness of flow. At this time, the lower the value of the measured critical film thickness of flow, the worse the fluidity of the paint is judged to be. In this case, when the critical film thickness of flow is greater than or equal to 40μm, it is evaluated as excellent (◎), when the critical film thickness of flow is greater than or equal to 35μm and less than 40μm, it is evaluated as good (○), when the critical film thickness of flow is greater than or equal to 30μm and less than 35μm, it is evaluated as general (△), and when the critical film thickness of flow is less than 30μm, it is evaluated as poor (×).

[0135] (8) Resistance to cold fracture

[0136] After the final coating film was left at -20°C for 3 hours, it was struck with 50 g of crushed stone (4 mm in diameter) at a 45° angle at a pressure of 4 bar. Thereafter, foreign matter such as peeled coating film remaining on the final coating film was removed.

[0137] For the damaged parts of the final coating film, when there are 10 or less damaged parts of 1 mm or less, it is evaluated as excellent (◎), when there are 10 or less damaged parts of more than 1 mm and less than 2 mm, it is evaluated as good (○), when there are 10 or less damaged parts of more than 2 mm and less than 3 mm, it is evaluated as fair (△), and when there are more than 10 damaged parts of more than 2 mm and less than 3 mm, it is evaluated as poor (×).

[0138] (9) Re-coating adhesion

[0139] After recoating and curing the base coating composition and the clear coating compositions of Examples and Comparative Examples to prepare recoated coating films, adhesion was evaluated using a checkerboard method.

[0140] Specifically, by the checkerboard method, after the recoating coating film is scratched with a knife blade to form 100 squares with a width of 2 mm and a length of 2 mm, the squares are separated using a tape to measure the adhesion. At this time, when 100% of the 100 squares are completely connected, the measured adhesion is evaluated as excellent (◎), when the remaining squares are greater than or equal to 70% and less than 100%, the measured adhesion is evaluated as good (○), when the remaining squares are greater than or equal to 50% and less than 70%, the measured adhesion is evaluated as general (△), and when the remaining squares are less than 50%, the measured adhesion is evaluated as poor (×).

[0141]

Table 5

[0142]

[0143]

Table 6

[0144]

[0145]

Table 7

[0146]

[0147] As shown in Tables 5 to 7, it can be seen that the base coating composition of the embodiment has excellent coating workability and paint fluidity, and the coating film prepared therefrom also has excellent mechanical properties such as appearance characteristics, glossiness, re-coating adhesion, impact resistance, water resistance and cold crack resistance.

[0148] Various embodiments of the present invention will be described below.

[0149] (1) A transparent coating composition, comprising a first acrylic resin, a second acrylic resin, a polyester resin and a melamine resin, wherein the first acrylic resin has an acid value of 6 to 13 mgKOH / g and a hydroxyl value of 135 to 155 mgKOH / g, and the second acrylic resin has an acid value of 15 to 25 mgKOH / g and a hydroxyl value of 100 to 130 mgKOH / g.

[0150] (2) A transparent coating composition, wherein the first acrylic resin has a glass transition temperature of 10 to 13° C. and a weight average molecular weight of 10,000 to 20,000 g / mol, and the second acrylic resin has a glass transition temperature of −7 to −3° C. and a weight average molecular weight of 7,000 to 9,000 g / mol.

[0151] (3) A transparent coating composition, wherein the polyester resin has an acid value of 15 to 30 mgKOH / g, a hydroxyl value of 120 to 155 mgKOH / g, a glass transition temperature of 0.1 to 2° C., and a weight average molecular weight of 4000 to 6000 g / mol.

[0152] (4) A transparent coating composition, wherein the solid content of the melamine resin is 50 to 70% by weight based on the total weight of the resin, the viscosity at 25° C. is 350 to 600 cps, and the acid value is 0.1 to 3.0 mgKOH / g.

[0153] (5) A transparent coating composition, comprising, based on the total weight of the transparent coating composition, 33 to 50 wt % of a first acrylic resin, 0.1 to 2 wt % of a second acrylic resin, 2 to 9 wt % of a polyester resin, and 20 to 33 wt % of a melamine resin.

Claims

1. A clear coating composition, wherein: comprising a first acrylic resin, a second acrylic resin, a polyester resin and a melamine resin, The first acrylic resin has an acid value of 6 to 13 mgKOH / g and a hydroxyl value of 135 to 155 mgKOH / g. The second acrylic resin has an acid value of 15 to 25 mgKOH / g and a hydroxyl value of 100 to 130 mgKOH / g.

2. The clear coating composition according to claim 1, wherein The first acrylic resin has a glass transition temperature of 10 to 13° C. and a weight average molecular weight of 10,000 to 20,000 g / mol. The second acrylic resin has a glass transition temperature of -7 to -3°C and a weight average molecular weight of 7000 to 9000 g / mol.

3. The clear coating composition according to claim 1, wherein The polyester resin has an acid value of 15 to 30 mgKOH / g, a hydroxyl value of 120 to 155 mgKOH / g, a glass transition temperature of 0.1 to 2° C., and a weight average molecular weight of 4000 to 6000 g / mol.

4. The clear coating composition according to claim 1, wherein The melamine resin has a solid content of 50 to 70% by weight, based on the total weight of the resin, a viscosity of 350 to 600 cps at 25° C., and an acid value of 0.1 to 3.0 mgKOH / g.

5. The clear coating composition according to claim 1, wherein The transparent coating composition comprises, based on the total weight of the composition, 33 to 50 wt % of a first acrylic resin, 0.1 to 2 wt % of a second acrylic resin, 2 to 9 wt % of a polyester resin and 20 to 33 wt % of a melamine resin.

Citation Information

Patent Citations

  • Resin composition for transparent varnich and transparent varnish composition using the same

    KR1020120110603A

  • Clear paint composition

    WO2020262869A2

  • KR20210108800A