Substrate coating composition
Through the composition of acrylic resin, polyester resin and melamine resin, the problem of hard curing of the base coating at low temperature in the prior art is solved, the mechanical properties of the coating film are improved, and economical coating technology and excellent coating are achieved. Film performance, suitable for body coating.
Patent Information
- Application Number
- CN202380034068.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-21
- Filing Date
- 2023-04-18
- Publication Date
- 2024-11-22
AI Technical Summary
The existing base coating composition is difficult to cure at a low temperature below 130°C, resulting in insufficient mechanical properties of the coating film and unable to meet the needs of vehicle body coating.
The composition of acrylic resin, polyester resin and melamine resin is used to improve the mechanical properties of the coating film by adjusting the hydroxyl group value, acid value and weight average molecular weight, and curing is achieved below 130°C.
It realizes an economical coating process at low temperatures, improves the gloss, impact resistance, water resistance and cold chip resistance of the coating film, and is suitable for use as body coating.
Smart Images

Figure BDA0005083156980000111 
Figure BDA0005083156980000121 
Figure BDA0005083156980000122
Abstract
Description
Technical Field
[0001] The present invention relates to a base coating composition. Background Art
[0002] Generally, the coating film on the vehicle body should not deteriorate or rust, and should have the durability to maintain the gloss or color of the coating film. Therefore, in terms of the vehicle painting process, the vehicle body that has undergone the pretreatment process is usually electroplated, followed by an intermediate (primer) coating to improve adhesion and smoothness, and a base coating is performed on the intermediate-coated vehicle body to improve the aesthetics of the vehicle body. Thereafter, a clear coating is applied to protect the color of the base coating and improve the appearance, and to protect the base coating from external influences.
[0003] In the coating of the base coating and the coating of the clear coating, usually, after the base coating composition is coated and dried, the clear coating composition is coated, and the clear coating and the base coating are cured together when the clear coating is cured. Therefore, the existing base coating composition is designed based on the high temperature curing condition. However, in order to reduce the cost of the coating process, the requirements for shortening the process and curable compositions at low temperatures tend to increase. In this regard, Korean Patent No. 10-0158534 (Patent Document 1) discloses a two-liquid acrylic polyurethane composition, which is composed of an additive, a main mixture containing an alcohol solvent, and a curing agent mixture containing polyisocyanate and ester solvents, and the additive is composed of acrylic polyol, ester solvent, smoothing agent, slip agent and wax. However, as shown in Patent Document 1, although under the existing low temperature baking conditions, especially under the heat curing conditions below 130°C, the base coating composition that can be used has a coating coating for automobile maintenance and a component coating composition, but the mechanical properties of the prepared coating film are insufficient, so that there are limitations in the application of the coating for the body.
[0004] Therefore, it is necessary to develop a base coating composition that can be cured at a low temperature of 130° C. or lower and has excellent mechanical properties for a coating film prepared therefrom and is suitable for use as a vehicle body coating.
[0005] [Prior art literature]
[0006] (Patent Document 1) Korean Patent No. 10-0158534 (August 5, 1998) Summary of the invention
[0007] Technical issues
[0008] The present invention aims to provide a base coating composition which can be cured at a low temperature below 130°C and can prepare a coating film with excellent mechanical properties.
[0009] Solution to the problem
[0010] In one embodiment, the present invention provides a base coating composition, which includes an acrylic resin, a polyester resin and a melamine resin, wherein the hydroxyl value of the acrylic resin is 70 to 85 mgKOH / g and the weight average molecular weight is 40,000 to 50,000 g / mol, and the acid value of the polyester resin is 10 to 30 mgKOH / g and the hydroxyl value is 250 to 300 mgKOH / g.
[0011] Effects of the Invention
[0012] According to a base coating composition of the present invention, the thermal curing temperature of the coating process can be performed at a low temperature of 130°C or lower, which is lower than the temperature of the prior art, thereby saving the cost required for the coating process, which is very economical. In addition, the coating film prepared by the composition has excellent mechanical properties, especially gloss, impact resistance, water resistance, cold cracking resistance, etc., which is conducive to use as a car body coating. DETAILED DESCRIPTION
[0013] Hereinafter, the present invention will be described in detail.
[0014] In this specification, "weight average molecular weight (Mw)" and "number average molecular weight (Mn)" are measured by a commonly known method in the technical field to which the present invention belongs, for example, by a method such as gel permeation chromatography (GPC).
[0015] In the present specification, the "glass transition temperature (Tg)" is measured by a generally known method in the technical field to which the present invention belongs, for example, it can be measured by differential scanning calorimetry (DSC) or the like.
[0016] In this specification, functional group values such as "acid value (Av)" and "hydroxyl value (OHv)" are measured by a commonly known method in the technical field to which the present invention belongs, for example, by titration or the like.
[0017] According to one embodiment of the present invention, a base coating composition is provided, which includes an acrylic resin, a polyester resin and a melamine resin, wherein the acrylic resin has a hydroxyl value of 70 to 85 mgKOH / g and a weight average molecular weight of 40,000 to 50,000 g / mol, and the polyester resin has an acid value of 10 to 30 mgKOH / g and a hydroxyl value of 250 to 300 mgKOH / g.
[0018] As described above, when using an acrylic resin having a hydroxyl value and a weight-average molecular weight within a specific range, by adjusting the curing reaction rate and the crosslinking density with the fast-reactive melamine resin, not only the appearance characteristics of the coating film can be improved, but also the mechanical properties such as impact resistance and water resistance can be improved, and the coating film can be cured at a low temperature below 130°C.
[0019] For example, the fast-reactive imino-containing melamine resin undergoes a cross-linking reaction with the hydroxyl value of the acrylic resin, thereby being cured at a low temperature below 130°C. A weight average molecular weight within a specific range has the effect of improving the mechanical properties of the prepared coating film, such as durability.
[0020] Furthermore, when a polyester resin having an acid value and a hydroxyl value within a specific range is used, the surface tension is adjusted during the curing reaction of the fast-reactive melamine resin and the acrylic resin, thereby improving the smoothness of the coating film and forming a soft coating film, which has the effect of improving mechanical properties such as chip resistance and scratch resistance.
[0021] <Acrylic resin>
[0022] The acrylic resin, as the main resin (principal resin) of the base coating composition according to the present invention, has a function of improving the appearance characteristics such as durability and glossiness of the prepared coating film.
[0023] The acrylic resin may be directly synthesized according to a known method or a commercially available product. The acrylic resin may be prepared by polymerizing, for example, one or more of a first vinyl monomer and a first (meth)acrylate monomer.
[0024] As the first vinyl monomer, one or more selected from the group consisting of, for example, styrene, methylstyrene, dimethylstyrene, fluorostyrene, ethoxystyrene, methoxystyrene, phenylene vinyl ketone, vinyl tert-butylbenzoate, vinyl cyclohexanoate, vinyl acetate, vinyl pyrrolidone, vinyl chloride, vinyl alcohol, acetoxystyrene, tert-butylstyrene and vinyltoluene can be used.
[0025] The first (meth)acrylate-based monomer may include one or more selected from the group consisting of a (meth)acrylate monomer not containing a hydroxyl group and a (meth)acrylate monomer containing a hydroxyl group.
[0026] The (meth)acrylate monomer not containing a hydroxyl group may include one or more selected from the group consisting of, for example, (meth)acrylic acid, methyl(meth)acrylic acid, (meth)acrylate, methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, isopropyl(meth)acrylate, butyl(meth)acrylate, isobutyl(meth)acrylate, tert-butyl(meth)acrylate, pentyl(meth)acrylate, hexyl(meth)acrylate, heptyl(meth)acrylate, isooctyl(meth)acrylate, octyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, isodecyl(meth)acrylate, decyl(meth)acrylate, dodecyl(meth)acrylate, isobornyl(meth)acrylate and lauryl(meth)acrylate.
[0027] The hydroxyl group-containing (meth)acrylate monomer may be, for example, a hydroxyalkyl-containing (meth)acrylate, and specifically may include one or more selected from the group consisting of 2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate.
[0028] Acrylic resin can be prepared by, for example, free radical polymerization, and physical properties such as weight average molecular weight (Mw), hydroxyl value (OHv), acid value (Av) can be adjusted by initiator and polymerization time.
[0029] The solid content (NV) of the acrylic resin may be 40 to 60% by weight or 45 to 55% by weight relative to the total weight of the resin. When the solid content of the acrylic resin is within the range, the storage stability of the resin and the storage stability of the base coating composition can be improved, and the workability is excellent. If the solid content of the acrylic resin is less than the range, the viscosity becomes too low, which has the problem of insufficient workability of the base coating composition containing it. If it exceeds the range, the viscosity of the acrylic resin is too high, which reduces the stability during the reaction and deteriorates the dispersion stability, so that agglomeration may occur over time.
[0030] The viscosity of the acrylic resin at 25°C may be 450 to 650 cps or 470 to 630 cps. When the viscosity of the acrylic resin at 25°C is within the above range, the viscosity of the base coating composition is appropriate, which has the effect of improving workability. If the viscosity of the acrylic resin at 25°C is less than the above range, the viscosity of the composition is too low, and the prepared coating film is not formed, resulting in low fluidity, adhesion and scratch resistance of the paint. When it exceeds the above range, the appearance characteristics of the prepared coating film may be reduced due to insufficient workability of the composition.
[0031] The acid value (Av) of the acrylic resin may be 10 to 30 mgKOH / g or 15 to 25 mgKOH / g. When the acid value of the acrylic resin is within the range, the reactivity of the composition containing the acrylic resin is adjusted, thereby improving the appearance characteristics of the coating film prepared therefrom. When the acid value of the acrylic resin is less than the range, the appearance of the prepared coating film may deteriorate due to the low curing reaction rate. If the acid value exceeds the range, the viscosity of the composition may increase as the cohesiveness of the resin increases, and the workability and room temperature storage properties may be reduced.
[0032] The hydroxyl value (OHv) of the acrylic resin may be 70 to 85 mgKOH / g or 75 to 80 mgKOH / g. When the hydroxyl value of the acrylic resin is within the range, the durability and weather resistance of the coating film are improved. If the hydroxyl value of the acrylic resin is less than the range, the coating film formed by the cross-linking reaction with the curing agent is insufficient, so that the mechanical properties such as the hardness of the coating film are reduced. If it exceeds the range, the coating film becomes brittle due to over-curing, thereby reducing elasticity, and the appearance characteristics of the prepared coating film may be insufficient.
[0033] The glass transition temperature (Tg) of the acrylic resin may be 20 to 40° C. or 25 to 35° C. When the glass transition temperature of the acrylic resin is within the above range, the hardness and solvent resistance of the coating film are improved. If the glass transition temperature of the acrylic resin is less than the above range, the hardness and solvent resistance of the prepared coating film are insufficient due to the decrease in the drying speed and crosslinking density of the coating film. When the glass transition temperature exceeds the above range, the coating film becomes brittle, which may result in insufficient appearance characteristics and crack resistance of the prepared coating film.
[0034] The weight average molecular weight (Mw) of acrylic resin can be 40000 to 50000 g / mol or 42000 to 44000 g / mol. When the weight average molecular weight of acrylic resin is within the range, the prepared coating film can have long-term physical properties such as excellent durability and weather resistance. If the weight average molecular weight of acrylic resin is less than the range, the weather resistance and scratch resistance of the prepared coating film are insufficient due to the small molecular weight. If it exceeds the range, the fluidity is reduced as the molecular weight increases, thereby the workability of the base coating composition comprising it is poor, and the surface smoothness is not excellent, and the problem of being difficult to prepare a coating film with excellent appearance may occur.
[0035] The composition may include an acrylic resin in an amount of 22 to 33% by weight or 24 to 30% by weight based on the total weight of the base coating composition. When the acrylic resin is included within the above content range, it has the effect of improving the adhesion and durability of the coating film. If the content of the acrylic resin is less than the above range, the adhesion, glossiness and durability of the coating film may be reduced due to poor drying properties. If the content of the acrylic resin exceeds the above range, the coating workability and paint fluidity of the composition may be insufficient due to rapid drying, thereby reducing the appearance and scratch resistance of the coating film.
[0036] <Polyester resin>
[0037] The polyester resin has the function of imparting flexibility to the base coating composition, increasing the crosslinking density, and improving mechanical properties such as cold crack resistance, impact resistance, and scratch resistance of the prepared coating film.
[0038] The polyester resin can be prepared by reacting a carboxylic acid compound with a diol compound. For example, the polyester resin can be prepared by reacting one or more carboxylic acid compounds selected from adipic acid (AA), isophthalic acid (IPA), trimellitic anhydride (TMA), alicyclic acid, phthalic anhydride, isophthalic acid, terephthalic acid, succinic acid, adipic acid, fumaric acid, maleic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride and derivatives thereof with one or more diol compounds selected from 1,6-hexanediol (1,6-HD), neopentyl glycol (NPG), trimethylolpropane (TMP), ethylene glycol, propylene glycol, diethylene glycol, butanediol, 1,4-hexanediol and 3-methylpentanediol.
[0039] Polyester resin can be prepared by condensation reaction of acid and alcohol, and physical properties such as weight average molecular weight (Mw), hydroxyl value (OHv), acid value (Av) can be adjusted by adjusting the ratio of acid and alcohol.
[0040] The solid content (NV) of the polyester resin may be 60 to 70% by weight or 63 to 67% by weight relative to the total weight of the resin. When the solid content of the polyester resin is within the above range, the storage stability of the resin and the storage stability of the base coating composition can be improved, and the workability is excellent. If the solid content of the polyester resin is less than the above range, the viscosity becomes too low, which has the problem of insufficient workability of the base coating composition containing it. If it exceeds the above range, the viscosity of the polyester resin is too high, which reduces the stability during the reaction and deteriorates the dispersion stability, so that aggregation may occur over time.
[0041] The viscosity of the polyester resin at 25°C may be 800 to 1800 cps or 850 to 1780 cps. When the viscosity of the polyester resin at 25°C is within the above range, the viscosity of the base coating composition is appropriate, which has the effect of improving workability. If the viscosity of the polyester resin at 25°C is less than the above range, the viscosity of the composition is too low, and the prepared coating film is not formed, resulting in low fluidity, adhesion and scratch resistance of the paint. When it exceeds the above range, the workability of the composition is insufficient, and the appearance characteristics of the prepared coating film may be reduced.
[0042] The acid value (Av) of the polyester resin may be 10 to 30 mgKOH / g or 15 to 25 mgKOH / g. When the acid value of the polyester resin is within the above range, the weather resistance of the coating film is improved. If the acid value of the polyester resin is less than the above range, the coating film is not formed sufficiently through the cross-linking reaction with the curing agent, so that the mechanical properties such as the hardness of the coating film are reduced. If it exceeds the above range, the coating film becomes brittle (brittle) due to over-curing, thereby reducing the elasticity, and the appearance characteristics, water resistance and scratch resistance of the prepared coating film may be insufficient.
[0043] The hydroxyl value (OHv) of the polyester resin may be 250 to 300 mgKOH / g or 260 to 280 mgKOH / g. When the hydroxyl value of the polyester resin is within the range, the reactivity with the melamine resin may be improved, so that the crosslinking density of the coating film is increased, which has the effect of improving mechanical properties, appearance and chemical resistance. If the hydroxyl value of the polyester resin is less than the range, the crosslinking density is insufficient due to insufficient reactivity with the melamine resin, and the durability and chemical resistance of the prepared coating film are low. If it exceeds the range, the coating film becomes brittle due to over-curing, and the appearance and scratch resistance may be reduced.
[0044] The glass transition temperature (Tg) of the polyester resin may be 5 to 20° C. or 10 to 14° C. When the glass transition temperature of the polyester resin is within the above range, the glossiness and hardness of the coating film are improved. If the glass transition temperature of the polyester resin is less than the above range, the drying speed of the base coating composition is delayed, and the solvent resistance and crack resistance of the prepared coating film are insufficient. If it exceeds the above range, the coating film becomes brittle, which may cause the appearance characteristics and hardness of the coating film to be insufficient.
[0045] The weight average molecular weight (Mw) of the polyester resin may be 2000 to 4000 g / mol or 2500 to 3500 g / mol. When the weight average molecular weight of the polyester resin is within the range, the smoothness of the base coating composition can be improved, a soft coating film can be formed, and the scratch resistance and hardness can be improved. If the weight average molecular weight of the polyester resin is less than the range, the mechanical properties of the prepared coating film are low due to the small molecular weight. If it exceeds the range, as the molecular weight increases, the fluidity decreases, making the coating film brittle, and the problem of reduced smoothness and low scratch resistance may occur.
[0046] The composition may contain the polyester resin in an amount of 3 to 6 wt % or 4 to 5 wt % based on the total weight of the base coating composition. When the polyester resin contained is within the above content range, it has the effect of improving the scratch resistance of the appearance and the smoothness of the coating film. If the content of the polyester resin in the composition is less than the above range, the appearance and scratch resistance may be reduced due to the low crosslinking density. If it exceeds the above range, the viscosity of the composition is too high, the workability and drying properties may be reduced, and the appearance and mechanical properties may be reduced.
[0047] <Melamine resin>
[0048] The melamine resin, as a curing agent, undergoes a cross-linking reaction with the components of the base coating composition to cure the composition, thereby increasing the hardness of the prepared coating film.
[0049] The melamine resin may be an alkylated melamine resin, and a product directly synthesized according to a known method or a commercially available product may be used.
[0050] The melamine resin may include one or more selected from the group consisting of, for example, methoxymethylmelamine, methylmelamine, butylmelamine, isobutoxymelamine, butoxymelamine, hexamethylolmelamine, hexamethoxymethylmelamine, hexabutoxymethylmelamine, hexamethoxybutoxymethylmelamine, aminomethoxymethylmelamine and imino group-containing alkylated melamine.
[0051] Examples of commercially available melamine resins include CYMEL-325, CYMEL-303, CYMEL-1161, and CYMEL-1168 from CYTEC, LUWIPAL 012 and LUWIPAL 072 from BASF, and SETAMINE US-138 from NUPLEX.
[0052] The solid content (NV) of the melamine resin may be 60 to 80% by weight or 65 to 75% by weight relative to the total weight of the resin. When the solid content of the melamine resin is within the range, the workability of the base coating composition is improved. If the solid content of the melamine resin is less than the range, the viscosity becomes too low and the fluidity is low, which has the problem of insufficient workability of the base coating composition containing it. If it exceeds the range, the viscosity is too high, which reduces the stability during the reaction and deteriorates the dispersion stability. Therefore, coagulants may be generated in the base coating composition over time.
[0053] The viscosity of the melamine resin at 25° C. may be 1000 to 1800 cps or 1100 to 1700 cps. When the viscosity of the melamine resin at 25° C. is within the above range, the gloss and appearance are excellent. If the viscosity of the melamine resin at 25° C. is less than the above range, the coating film may not be formed due to the low viscosity, resulting in low adhesion and scratch resistance of the coating film. When the viscosity exceeds the above range, the workability of the composition may deteriorate, resulting in insufficient appearance characteristics of the prepared coating film.
[0054] Moreover, the acid value (Av) of the melamine resin may be 0.1 to 3 mgKOH / g or 0.1 to 2 mgKOH / g. When the acid value of the melamine resin is less than the above range, the hardness and appearance characteristics of the prepared coating film may be low due to the low curing reaction rate. If it exceeds the above range, the water resistance may be low as the hydrophilicity increases.
[0055] The composition may contain melamine resin in an amount of 5 to 20% by weight or 8 to 15% by weight based on the total weight of the base coating composition. When the content of melamine resin is within the range, the crosslinking density can be increased, thereby increasing the adhesion and hardness of the prepared coating film. If the content of melamine resin is less than the range, the hardness and appearance characteristics may be reduced due to low curability. If the content exceeds the range, the coating film may become brittle due to excessive curability, and the adhesion, impact resistance and scratch resistance may be reduced.
[0056] <Acrylic anti-sagging agent>
[0057] In order to adjust the sagging property of the base coating composition, an acrylic anti-sagging agent may be included.
[0058] The acrylic anti-sagging agent can be directly synthesized according to a known method or a commercially available product. The acrylic anti-sagging agent can be prepared by polymerizing, for example, one or more of a second vinyl monomer and a second (meth)acrylate monomer.
[0059] As another example, the acrylic anti-sagging agent may also be prepared by reacting a second vinyl monomer, a second (meth)acrylate monomer, and benzylamine, and may have a chemical structure having a needle-shaped diurea group.
[0060] As the second vinyl monomer, one or more selected from the group consisting of, for example, styrene, methylstyrene, dimethylstyrene, fluorostyrene, ethoxystyrene, methoxystyrene, phenylene vinyl ketone, vinyl tert-butylbenzoate, vinyl cyclohexanoate, vinyl acetate, vinyl pyrrolidone, vinyl chloride, vinyl alcohol, acetoxystyrene, tert-butylstyrene and vinyltoluene can be used.
[0061] The second (meth)acrylate-based monomer may include one or more selected from the group consisting of a (meth)acrylate monomer not containing a hydroxyl group and a (meth)acrylate monomer containing a hydroxyl group.
[0062] The (meth)acrylate monomer not containing a hydroxyl group may include one or more selected from the group consisting of, for example, (meth)acrylic acid, methyl(meth)acrylic acid, (meth)acrylate, methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, isopropyl(meth)acrylate, butyl(meth)acrylate, isobutyl(meth)acrylate, tert-butyl(meth)acrylate, pentyl(meth)acrylate, hexyl(meth)acrylate, heptyl(meth)acrylate, isooctyl(meth)acrylate, octyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, isodecyl(meth)acrylate, decyl(meth)acrylate, dodecyl(meth)acrylate, isobornyl(meth)acrylate and lauryl(meth)acrylate.
[0063] The hydroxyl group-containing (meth)acrylate monomer may be, for example, a hydroxyalkyl-containing (meth)acrylate, and specifically may include one or more selected from the group consisting of, for example, 2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate.
[0064] The acrylic anti-sagging agent can be prepared by, for example, a free radical polymerization method, and the physical properties such as the weight average molecular weight (Mw), hydroxyl value (OHv), and acid value (Av) can be adjusted by the initiator and the polymerization time.
[0065] The solid content (NV) of the acrylic anti-sagging agent may be 50 to 70% by weight or 55 to 65% by weight relative to the total weight of the resin. When the solid content of the acrylic anti-sagging agent is within the range, the storage stability of the resin and the storage stability of the base coating composition can be improved, and the workability is excellent. If the solid content of the acrylic anti-sagging agent is less than the range, the viscosity becomes too low, which has the problem of insufficient workability of the base coating composition containing it. If it exceeds the range, the viscosity is too high, so that the stability during the reaction is reduced and the dispersion stability is deteriorated, so coagulation may occur over time.
[0066] The viscosity of the acrylic anti-sagging agent at 25°C may be 10,000 to 18,000 cps or 11,000 to 17,000 cps. When the viscosity of the acrylic anti-sagging agent at 25°C is within the above range, the viscosity of the base coating composition is appropriate, which has the effect of improving workability. If the viscosity of the acrylic anti-sagging agent at 25°C is less than the above range, the viscosity of the composition is too low, and the prepared coating film is not formed, resulting in low fluidity, adhesion and scratch resistance of the paint. When it exceeds the above range, the appearance characteristics of the prepared coating film may be reduced due to insufficient workability of the composition.
[0067] The composition may contain an acrylic anti-sagging agent in an amount of 4 to 9 wt % or 5 to 8 wt % based on the total weight of the base coating composition. When the acrylic anti-sagging agent is contained within the above content range, it has the effect of improving the sagging property of the base coating composition. If the content of the acrylic anti-sagging agent is less than the above range, the base coating composition containing it may have insufficient sagging property due to poor drying performance, thereby reducing workability. If the content exceeds the above range, the coating workability and paint fluidity of the composition may be reduced due to rapid drying, and the viscosity of the base coating composition may be increased, thereby deteriorating the storage stability and appearance.
[0068] <Toner>
[0069] The base coating composition according to one embodiment of the present invention may further include a toner. The toner has a function of imparting color to the prepared coating film.
[0070] The toner is not particularly limited as long as it is a pigment that can be generally used in a coating composition, and for example, inorganic pigments and organic pigments can be used. As another example, the pigments include metal oxides such as titanium dioxide, carbon black, zinc oxide, ultramarine, and red iron oxide; sulfides of lithopone, lead, cadmium, iron, cobalt, and aluminum, and their hydrochlorides or lactates; azo pigments; and copper phthalocyanine pigments.
[0071] The solid content (NV) of the toner may be 65 to 85 wt % or 70 to 80 wt % relative to the total weight of the toner. When the solid content of the toner is within the above range, the workability of the base coating composition is improved.
[0072] The viscosity of the toner at 25° C. may be 880 to 2270 cps or 900 to 2000 cps. When the viscosity of the toner at 25° C. is within the above range, the viscosity of the base coating composition is appropriate, thereby improving workability and appearance.
[0073] The composition may contain the toner in an amount of 33 to 50% by weight or 37 to 45% by weight based on the total weight of the base coating composition. When the toner content in the base coating composition is within the range, problems such as insufficient hiding power of the prepared coating film, low stability of the composition, and low dispersibility of the toner can be prevented.
[0074] <Additives>
[0075] The base coating composition according to one embodiment of the present invention may further include additives such as a UV absorber, a leveling agent, a surface smoothing agent, and a curing catalyst.
[0076] The UV absorber has the function of blocking the UV rays reaching the prepared coating film, thereby improving the weather resistance of the coating film. The UV absorber has a solid content (NV) of 80 to 100 wt %, a specific gravity of 1.0 to 1.2 g / cm3, and a ignition point of 45 to 49°C.
[0077] The ultraviolet absorber may be a benzotriazole ultraviolet absorber, for example, α-[3-[3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl]-ω-hydroxypoly(oxy-1,2-ethanediyl) (α-[3-[3-(2H-Benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl]-ω-hydroxypoly(oxy-1,2-ethanediyl) ydroxypoly(oxy-1,2-ethanediyl)), α-[3-[3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl]-ω-[3-[3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl]-ω-[3-[3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl] Benzotriazole ultraviolet absorbers such as benzotriazole-2-yl]-1-oxopropoxy]poly(oxy-1,2-ethanediyl) and 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy-methylester.
[0078] The leveling agent has the function of imparting leveling and wettability to the prepared coating film. The leveling agent can be a cationic surfactant, an anionic surfactant or a nonionic surfactant, for example, a nonionic surfactant can be included. The solid content (NV) of the leveling agent is 45 to 55% by weight, the specific gravity is 1.0 to 1.3, and the viscosity at 25°C can be 40 to 60 cps.
[0079] The surfactant has the function of affecting the smoothness of the prepared coating film and improving the appearance characteristics. The surfactant has a solid content (NV) of 50 to 54% by weight, a viscosity of 110 to 120 cSt, and a specific gravity of 0.8 to 1.0.
[0080] The curing catalyst has the function of preventing unstable curing of the base coating composition, thereby improving the mechanical properties of the coating film prepared therefrom. For example, curing catalysts such as amino-containing phosphate compounds or dodecylbenzenesulfonic acid compounds can be cited. The solid content (NV) of the curing catalyst can be 72 to 76% by weight, the specific gravity at 25° C. can be 0.9 to 1.0, and the acid value (Av) can be 120 to 140 mgKOH / g.
[0081] The content of the additive is not particularly limited as long as it is within the range that can be generally included in the base coating composition. For example, the composition may include the additive in an amount of 1 to 8 wt % or 2 to 7 wt % based on the total weight of the base coating composition.
[0082] <Solvent>
[0083] The base coating composition according to one embodiment of the present invention may further include a solvent. The solvent may have the function of adjusting the viscosity of the composition, improving the drying property, and improving the appearance characteristics and spreadability of the prepared coating film.
[0084] The solvent is not particularly limited as long as it is a solvent that can be generally used in the base coating composition, and may include one or more selected from the group consisting of, for example, aromatic hydrocarbon solvents, acetate solvents, alcohol solvents, and propionate solvents. Specifically, the solvent may include aromatic hydrocarbon solvents such as toluene, xylene, and xylene; acetate solvents such as 1-methoxy-2-propyl acetate, methyl acetate, ethyl acetate, n-propyl acetate, n-butyl acetate, methyl glutarate, methyl succinate, methyl adipate, dimethyl glutarate, dimethyl succinate, dimethyl adipate, propylene glycol methyl ether acetate (PMA), butyl carbitol acetate, and butyl cellosolve acetate; alcohol solvents such as n-butanol, propanol, 1-methoxy-2-propanol, and 2-butoxyethanol; ketone solvents such as acetone, methyl ethyl ketone, methyl butyl ketone, and methyl isobutyl ketone; and propionate solvents such as ethyl ethoxypropionate. Furthermore, commercially available products of aromatic hydrocarbon solvents include Kocosol#100, Kocosol#150, and the like.
[0085] Based on the gross weight of the base coating composition, the composition may include a solvent in an amount of 1 to 50% by weight or 5 to 25% by weight. When the solvent is included within the range, the viscosity of the composition can be appropriately adjusted to improve workability and dryness. If the solvent content in the base coating composition is less than the range, the workability of the composition may be insufficient due to the high solids content in the composition. If the solids content of the prepared base coating composition is low, the fluidity increases, and the appearance of the prepared coating and the problem of insufficient adhesion may occur.
[0086] The base coating composition according to one embodiment of the present invention may be a one-component type including a main part and a curing agent part.
[0087] Based on the gross weight of the composition, the solid content of the base coating composition of the present invention can be 50 to 60% by weight or 52 to 58% by weight. When the solid content of the base coating composition of the present invention is within the range, there is an advantage that the coating workability of the composition is suitable. If the solid content of the base coating composition of the present invention is insufficient in the range, there is a problem that the solid content reduces and causes the curing reactivity to be low. If it exceeds the range, due to the high solid content, the workability of the base coating composition may be reduced.
[0088] The base coating composition of the present invention may have a viscosity of 30 to 50 seconds, 32 to 48 seconds, or 35 to 45 seconds based on Ford Cup No. 4 at 25° C. If the viscosity of the base coating composition of the present invention is less than the above range, problems such as dripping from a vertical surface may occur, and if it exceeds the above range, the viscosity of the composition is high, and the appearance characteristics of the coating film prepared therefrom may be reduced or a load may be applied to the coating machine, which may cause a malfunction of the coating machine.
[0089] As mentioned above, the thermal curing temperature of the coating process of the base coating composition according to the present invention can be performed at a low temperature of 130°C or less, which is lower than the temperature of the prior art, and the cost required for the coating process can be saved, which is very economical. In addition, the coating film prepared by the base coating composition according to the present invention has excellent mechanical properties, especially gloss, impact resistance, water resistance, cold crack resistance, etc., which is conducive to use as a car body coating.
[0090] The present invention will be described in more detail below by way of examples, but these examples are only used to help understand the present invention, and the scope of the present invention is not limited to these examples in any way.
[0091] [Example]
[0092] Preparation of Base Coating Compositions of Examples and Comparative Examples
[0093] The components were stirred and mixed in the amounts shown in Tables 1 to 4 to prepare base coating compositions having a viscosity of 40 seconds based on Ford Cup No. 4.
[0094]
Table 1
[0095]
[0096]
[0097]
Table 2
[0098]
[0099]
[0100]
Table 3
[0101]
Table 4
[0102]
[0103]
[0104]
[0105] The physical properties, manufacturers and / or product names of the components used in the Examples and Comparative Examples are shown in Table 5 below.
[0106]
Table 5
[0107]
[0108]
[0109] Test example: Evaluation of properties of prepared coating films
[0110] The base coating composition prepared in the examples and comparative examples was bell sprayed on the electroplated sample at a thickness of 35 μm, and cured in an oven at 130° C. for 20 minutes to prepare a final coating film.
[0111] The appearance characteristics and physical properties of the final coating film were measured by the method described below, and the results are shown in Tables 6 to 9.
[0112] (1) Painting workability
[0113] The coating workability was evaluated by observing the spray state when the coating was discharged and the wettability with respect to the base material.
[0114] The observed conditions were evaluated as excellent (◎), good (○), fair (△), or poor (×).
[0115] (2) Coating appearance
[0116] The gloss (LU), brightness (SH) and orange peel (OP) of the prepared final coating film were measured using Wave Scan DOI (BYK Gardner), which is an automotive appearance tester. The comprehensive appearance evaluation value (CF) was calculated using the following mathematical formula 1 using the measured physical properties.
[0117] [Mathematical formula 1]
[0118] CF=LU×0.15+SH×0.35+OP×0.5
[0119] CF was measured and calculated in a horizontal and vertical manner. As the horizontal / vertical value of CF, when CF was greater than or equal to 65, it was evaluated as excellent (◎), when CF was greater than or equal to 60 and less than 65, it was evaluated as good (○), when CF was greater than or equal to 55 and less than 60, it was evaluated as fair (△), and when CF was less than 55, it was evaluated as poor (×).
[0120] (3) Glossiness
[0121] In order to measure the gloss (GLOSS, %) reflected from the coating film, a gloss meter (BYK Gardner) was used to measure the gloss at 20° of the final coating film.
[0122] According to the measurement results, when the glossiness is greater than or equal to 90%, it is evaluated as excellent (◎), when the glossiness is greater than or equal to 89% and less than 90%, it is evaluated as good (○), when the glossiness is greater than or equal to 87% and less than 89%, it is evaluated as average (△), and when the glossiness is less than 87%, it is evaluated as poor (×).
[0123] (4) Adhesion
[0124] After curing the base coating compositions of Examples and Comparative Examples, adhesion was evaluated using a checkerboard method.
[0125] Specifically, by the checkerboard method, after the recoating coating film is scratched with a knife blade to form 100 squares with a width of 2 mm and a length of 2 mm, the squares are separated using a tape to measure the adhesion. At this time, when 100% of the 100 squares are completely connected, the measured adhesion is evaluated as excellent (◎), when the remaining squares are greater than or equal to 70% and less than 100%, the measured adhesion is evaluated as good (○), when the remaining squares are greater than or equal to 50% and less than 70%, the measured adhesion is evaluated as general (△), and when the remaining squares are less than 50%, the measured adhesion is evaluated as poor (×).
[0126] (5) Impact resistance
[0127] The final coating film was evaluated for impact resistance according to ASTM D 2794. A DuPont impact tester was used to drop a 500 g weight onto the sample at a height varying from 30 cm to 50 cm, and the appearance of the coating film was observed.
[0128] The observation results show that when the falling height of the heavy object is greater than or equal to 50 cm, if the coating film does not show cracks or peeling, it is evaluated as excellent (◎); when the falling height of the heavy object is greater than or equal to 30 cm and less than 50 cm, if the coating film shows cracks or peeling, it is evaluated as good (○); when the falling height of the heavy object is greater than or equal to 20 cm and less than 30 cm, if the coating film shows cracks or peeling, it is evaluated as fair (△); when the falling height of the heavy object is less than 20 cm, if the coating film shows cracks or peeling, it is evaluated as poor (×).
[0129] (6) Water resistance
[0130] The final coating film was deposited in a constant temperature water bath at 40° C. for 240 hours and left at room temperature for 1 hour. The adhesion was evaluated by the checkerboard method and the color change was confirmed with the naked eye.
[0131] Specifically, the adhesion was measured in the same manner as the checkerboard method described in Item (4). The same evaluation criteria were applied to evaluate the water resistance of the coating film.
[0132] (7) Paint fluidity
[0133] A sample with a primer coating film formed thereon was vertically suspended on a steel plate with a hole having a diameter of 5 mm for electroplating coating, and the base coating composition of the embodiment and the comparative example was applied by the same method as described above. After drying and curing, the surface of the prepared coating film was observed to evaluate the paint fluidity of the composition.
[0134] Specifically, it was observed that the paint was condensed at the lower end of the hole, and the thickness (μm) of the coating film at the starting point where the flow was observed to occur was recorded as the critical film thickness of flow. At this time, the lower the value of the measured critical film thickness of flow, the worse the fluidity of the paint is judged to be. In this case, when the critical film thickness of flow is greater than or equal to 40μm, it is evaluated as excellent (◎), when the critical film thickness of flow is greater than or equal to 35μm and less than 40μm, it is evaluated as good (○), when the critical film thickness of flow is greater than or equal to 30μm and less than 35μm, it is evaluated as general (△), and when the critical film thickness of flow is less than 30μm, it is evaluated as poor (×).
[0135] (8) Resistance to cold cracking
[0136] After the final coating film was left at -20°C for 3 hours, it was struck with 50 g of crushed stone (4 mm in diameter) at a 45° angle at a pressure of 4 bar. Thereafter, foreign matter such as peeled coating film remaining on the final coating film was removed.
[0137] For the damaged parts of the final coating film, when there are 10 or less damaged parts of 1 mm or less, it is evaluated as excellent (◎), when there are 10 or less damaged parts of more than 1 mm and less than 2 mm, it is evaluated as good (○), when there are 10 or less damaged parts of more than 2 mm and less than 3 mm, it is evaluated as fair (△), and when there are more than 10 damaged parts of more than 2 mm and less than 3 mm, it is evaluated as poor (×).
[0138] (9) Re-coating adhesion
[0139] After the base coating compositions of Examples and Comparative Examples were re-coated and cured in the same manner as above to prepare re-coated coating films, adhesion was evaluated using the checkerboard method.
[0140] Specifically, by the checkerboard method, after the recoating coating film is scratched with a knife blade to form 100 squares with a width of 2 mm and a length of 2 mm, the squares are separated using a tape to measure the adhesion. At this time, when 100% of the 100 squares are completely connected, the measured adhesion is evaluated as excellent (◎), when the remaining squares are greater than or equal to 70% and less than 100%, the measured adhesion is evaluated as good (○), when the remaining squares are greater than or equal to 50% and less than 70%, the measured adhesion is evaluated as general (△), and when the remaining squares are less than 50%, the measured adhesion is evaluated as poor (×).
[0141]
Table 6
[0142]
[0143]
[0144]
Table 7
[0145]
[0146]
Table 8
[0147]
[0148]
Table 9
[0149]
[0150] As shown in Tables 6 to 9, it can be seen that the base coating composition of the embodiment has excellent coating workability and paint fluidity, and the coating film prepared therefrom also has excellent mechanical properties such as appearance characteristics, glossiness, re-coating adhesion, impact resistance, water resistance and cold crack resistance.
[0151] Various embodiments of the present invention will be described below.
[0152] (1) A base coating composition, comprising an acrylic resin, a polyester resin and a melamine resin, wherein the acrylic resin has a hydroxyl value of 70 to 85 mgKOH / g and a weight average molecular weight of 40,000 to 50,000 g / mol, and the polyester resin has an acid value of 10 to 30 mgKOH / g and a hydroxyl value of 250 to 300 mgKOH / g.
[0153] (2) A base coating composition, wherein the acrylic resin has an acid value of 10 to 30 mgKOH / g and a glass transition temperature of 20 to 40°C.
[0154] (3) A base coating composition, wherein the polyester resin has a glass transition temperature of 5 to 20° C. and a weight average molecular weight of 2000 to 4000 g / mol.
[0155] (4) A base coating composition, wherein the melamine resin has a viscosity of 1000 to 1800 cps at 25°C and an acid value of 0.1 to 3 mgKOH / g.
[0156] (5) A base coating composition comprising, based on the total weight of the base coating composition, 22 to 33 wt % of an acrylic resin, 3 to 6 wt % of a polyester resin, and 5 to 20 wt % of a melamine resin.
Claims
1. A base coating composition, in, Including acrylic resin, polyester resin and melamine resin, The hydroxyl value of the acrylic resin is 70 to 85 mgKOH / g, and the weight average molecular weight is 40,000 to 50,000 g / mol. The polyester resin has an acid value of 10 to 30 mgKOH / g and a hydroxyl value of 250 to 300 mgKOH / g.
2. The base coating composition according to claim 1, in, The acrylic resin has an acid value of 10 to 30 mgKOH / g and a glass transition temperature of 20 to 40°C.
3. The base coating composition according to claim 1, in, The polyester resin has a glass transition temperature of 5 to 20° C. and a weight average molecular weight of 2000 to 4000 g / mol.
4. The base coating composition according to claim 1, in, The melamine resin has a viscosity of 1000 to 1800 cps at 25° C. and an acid value of 0.1 to 3 mgKOH / g.
5. The base coating composition according to claim 1, in, The base coating composition comprises 22 to 33 weight percent of acrylic resin, 3 to 6 weight percent of polyester resin and 5 to 20 weight percent of melamine resin based on the total weight of the base coating composition.
Citation Information
Patent Citations
Coating composition and coating object
CN104673073A
Coating composition
CN105518091A
Aqueous paint composition for vehicle primer coating and vehicle coating method using same
CN108603072A
Transparent coating composition
CN112029349A
Method for forming a multilayer paint film