Outer packaging material for electricity storage device, method for producing same, and electricity storage device

By using a laminated structure of a base material layer, a barrier layer and a hot-weld resin layer composed of two or more layers in the outer packaging material for power storage devices, the work hardening index of the base material is adjusted, and forming in the prior art is solved The problem of poor performance achieves high energy density and excellent molding performance.

CN119013826APending Publication Date: 2024-11-22DAI NIPPON PRINTING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380032513.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-06
Filing Date
2023-04-04
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing film-shaped outer packaging materials for electrical storage devices are prone to cracks and pinholes during the molding process, and the mechanical strength and insulation of the polyamide film are poor, making it difficult to meet the needs of high energy density.

Method used

A base material layer composed of two or more layers is adopted, including a polyester film, and a barrier layer and a hot-weld resin layer are added thereto, so that the molding performance is improved by adjusting the work hardening index of the base material layer.

Benefits of technology

The molding performance of the outer packaging material for electrical storage devices is achieved, which avoids the occurrence of cracks and pinholes, and improves the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005070408080000261
    Figure BDA0005070408080000261
  • Figure BDA0005070408080000262
    Figure BDA0005070408080000262
  • Figure BDA0005070408080000263
    Figure BDA0005070408080000263
Patent Text Reader

Abstract

The present invention pertains to an outer packaging material for an electricity storage device, the outer packaging material comprising a laminate comprising at least two or more base material layers, a barrier layer, and a heat-fusible resin layer in this order, the base material layer comprising one or more polyester films, and the heat-fusible resin layer comprising one or more polyester films. The work hardening indexes in the longitudinal direction and the width direction of the base material layer are both 2.5-4.5, and the difference between the work hardening indexes in the longitudinal direction and the width direction is 1.4 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an outer packaging material for an electric storage device, a method for producing the same, and an electric storage device. Background Art

[0002] Currently, various types of power storage devices have been developed, but in all of these power storage devices, packaging materials have become indispensable components in order to encapsulate power storage device components such as electrodes and electrolytes. In the past, metal packaging materials were often used as packaging materials for power storage devices.

[0003] On the other hand, in recent years, with the high performance of electric vehicles, hybrid electric vehicles, personal computers, cameras, mobile phones, etc., the storage devices are required to have not only various shapes, but also thinner and lighter weight. However, the currently commonly used metal packaging materials for storage devices have the disadvantages of being difficult to adapt to the diversification of shapes and also having limitations in lightness.

[0004] Therefore, as an outer packaging material for storage battery devices that is easy to process into various shapes and can be thinned and lightened, a film-like outer packaging material having a base material layer / aluminum foil layer / thermo-fusible resin layer stacked in sequence has been proposed (see, for example, Patent Document 1).

[0005] In the case of such a film-like packaging member, a recess is usually formed by cold rolling, and storage device elements such as electrodes and electrolyte are arranged in the space formed by the recess. By thermally fusing the heat-fusible resin layers to each other, a storage device is obtained in which the storage device elements are accommodated inside the outer packaging material.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2008-287971 Summary of the invention

[0009] Problems to be solved by the invention

[0010] In order to further improve the energy density of the storage device, the film-shaped packaging material needs to form a deep concave portion for accommodating the storage device element. However, when the film-shaped packaging material is molded and the concave portion is formed, there is a problem that cracks and pinholes are easily generated.

[0011] Among them, as the base material layer of the film-like outer packaging material, for example, polyamide film, polyester film, etc. are used. In order to improve the molding performance of the outer packaging material, polyamide film is preferably used.

[0012] However, although polyamide films have better moldability than polyester films, they are inferior in mechanical strength and insulation properties. Therefore, a technology that uses a polyester film as a base layer and can improve the moldability of an outer packaging material for a storage device is desired.

[0013] Moreover, if the base material layer of the film-like outer packaging material is composed of two or more layers and the materials and physical properties of each layer contained in the base material layer are adjusted, the overall performance of the outer packaging material (molding performance, etc.) will also be adjusted to an appropriate level.

[0014] The main object of the present invention is to provide a packaging material for a power storage device having excellent moldability, comprising a laminate having at least a base layer composed of two or more layers including a polyester film, a barrier layer, and a heat-fusible resin layer in this order.

[0015] Technical solutions to solve problems

[0016] The inventors of the present invention have conducted intensive research to solve the above-mentioned problems. As a result, it was found that in an outer packaging material for a storage device having a laminated body having at least a substrate layer including a polyester film and composed of two or more layers, a barrier layer, and a heat-fusible resin layer in sequence, by setting the work hardening index of the entire substrate layer in the length direction and the width direction and the difference in the work hardening index in the length direction and the width direction within a specific range, the outer packaging material for a storage device exhibits excellent molding performance.

[0017] The present invention is an invention completed through further repeated studies based on the above-mentioned knowledge. That is, this specification provides the invention of the following forms.

[0018] A packaging material for a storage device, wherein the substrate layer is composed of two or more layers, the substrate layer includes one or more polyester films, the work hardening index of the substrate layer in the length direction and the width direction are both greater than 2.5 and less than 4.5, and the difference between the work hardening index in the length direction and the width direction is less than 1.4.

[0019] Effects of the Invention

[0020] According to the present invention, there is provided an outer packaging material for an electrical storage device having excellent moldability and comprising a laminated body including at least a base layer including a polyester film and composed of two or more layers, a barrier layer, and a heat-fusible resin layer in this order. Furthermore, according to the present invention, there is provided a method for manufacturing an outer packaging material for an electrical storage device and an electrical storage device. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of an example of the cross-sectional structure of the outer packaging material for an electric storage device of the present invention.

[0022] Figure 2It is a schematic diagram of an example of the cross-sectional structure of the outer packaging material for an electric storage device of the present invention.

[0023] Figure 3 It is a schematic diagram of an example of the cross-sectional structure of the outer packaging material for an electric storage device of the present invention.

[0024] Figure 4 It is a schematic diagram of an example of the cross-sectional structure of the outer packaging material for an electric storage device of the present invention.

[0025] Figure 5 It is a schematic diagram for explaining a method of housing an electric storage device element in a packaging body formed of the outer packaging material for an electric storage device of the present invention. DETAILED DESCRIPTION

[0026] The outer packaging material for a storage device of the present invention is characterized in that it is composed of a laminated body having at least a substrate layer, a barrier layer and a heat-fusible resin layer in sequence, the substrate layer is composed of two or more layers, the substrate layer includes one or more polyester films, the work hardening index of the substrate layer in the longitudinal direction (MD direction) and the width direction is 2.5 or more and 4.5 or less, and the difference between the work hardening index in the longitudinal direction and the width direction is 1.4 or less. The outer packaging material for a storage device of the present invention has excellent molding performance despite containing a polyester film.

[0027] The outer packaging material for the power storage device of the present invention will be described in detail below. It should be noted that, in the present invention, the numerical range represented by "~" means "above..., below...". For example, the expression "2~15mm" means "above 2mm, below 15mm". In the numerical range represented by segments in the present invention, the upper limit value or lower limit value recorded in a certain numerical range can be replaced by the upper limit value or lower limit value of the numerical range recorded in other segments. In addition, the upper limit value and the upper limit value, the upper limit value and the lower limit value, or the lower limit value and the lower limit value recorded independently can also be combined to form a numerical range. In addition, within the numerical range recorded in this specification, the upper limit value or the lower limit value recorded in a certain numerical range can also be replaced by the value shown in the embodiment.

[0028] It should be noted that, in the outer packaging material for the storage device, regarding the barrier layer 3 described later, the MD (Machine Direction: processing direction / longitudinal direction) and TD (Transverse Direction: transverse direction) in its manufacturing process can usually be distinguished. For example, when the barrier layer 3 is made of a metal foil such as an aluminum alloy foil or a stainless steel foil, a linear stripe called a rolling mark will be formed on the surface of the metal foil along the rolling direction (RD: Rolling Direction) of the metal foil. Since the rolling mark extends along the rolling direction, the rolling direction of the metal foil can be determined by observing the surface of the metal foil. In addition, in the manufacturing process of the laminate, the MD of the laminate is usually consistent with the RD of the metal foil. Therefore, by observing the surface of the metal foil of the laminate to determine the rolling direction (RD) of the metal foil, the MD of the laminate can be determined. And since the TD of the laminate is perpendicular to the MD of the laminate, the TD of the laminate can also be determined.

[0029] In addition, when the MD of the outer packaging material for the storage device cannot be confirmed by the rolling marks of the metal foil such as aluminum alloy foil and stainless steel foil, it can be determined by the following method. As a method for confirming the MD of the outer packaging material for the storage device, there is a method of observing the cross section of the heat-fusible resin layer of the outer packaging material for the storage device with an electron microscope and confirming the island structure. In this method, the direction parallel to the cross section where the average value of the diameter of the shape of the "island" perpendicular to the thickness direction of the heat-fusible resin layer is the largest can be determined as MD. Specifically, the cross section from the length direction of the heat-fusible resin layer and the cross sections (a total of 10 cross sections) starting from the direction parallel to the cross section in the length direction and changing 10 degrees each time until the cross section perpendicular to the length direction are observed using electron micrographs to confirm the island structure. Next, the shape of each "island" in each cross section is observed separately. The shape of each "island" is determined by the straight-line distance connecting the leftmost end and the rightmost end in the vertical direction perpendicular to the thickness of the hot-melt resin layer as the island diameter y. In each cross-section, the average value of the island diameter y of the top 20 island diameter y values ​​in descending order in the "island" shape is calculated, and the direction parallel to the cross-section where the average value of the island diameter y of the "island" shape is the largest is determined as MD.

[0030] 1. Laminated structure of packaging materials for power storage devices

[0031] For example, the outer packaging material 10 for an electric storage device of the present invention Figure 1As shown, it is composed of a laminated body having a base material layer 1, a barrier layer 3 and a heat-fusible resin layer 4 in this order. In the outer packaging material 10 for a storage device, the base material layer 1 is the outermost layer, and the heat-fusible resin layer 4 is the innermost layer. When assembling a storage device using the outer packaging material 10 for a storage device and a storage device element, the storage device element is accommodated in a space formed by heat-fusion bonding of the peripheral portions of the heat-fusible resin layers 4 of the outer packaging material 10 for a storage device in a state where the heat-fusible resin layers 4 of the storage device outer packaging material 10 are facing each other. In the laminated body constituting the outer packaging material 10 for a storage device of the present invention, with the barrier layer 3 as a reference, the side closer to the heat-fusible resin layer 4 than the barrier layer 3 is the inner side, and the side closer to the base material layer 1 than the barrier layer 3 is the outer side.

[0032] In the present invention, the substrate layer 1 is composed of two or more layers. Figures 1 to 4 The schematic diagram shows that the substrate layer 1 is formed of a laminate including a first substrate layer 11 and a second substrate layer 12. In the present invention, when the substrate layer 1 includes the first substrate layer 11 and the second substrate layer 12, the first substrate layer 11 is located on the outside (opposite to the barrier layer side), and the second substrate layer 12 is located on the inside (barrier layer side). The substrate layer 1 includes one or more polyester films, and as described later, the first substrate layer 11 is preferably formed of a polyester film.

[0033] The first substrate layer 11 and the second substrate layer 12 may be in contact with each other. In addition, although not shown in the figure, there may be an adhesive layer between the first substrate layer 11 and the second substrate layer 12. It should be noted that when there is an adhesive layer between the first substrate layer 11 and the second substrate layer 12, the substrate layer 1 forms a three-layer structure in which the first substrate layer 11, the adhesive layer, and the second substrate layer 12 are stacked in sequence. As described later, in the present invention, the most preferred composition of the substrate layer 1 is a stacked structure in which the first substrate layer 11 is formed of a biaxially stretched polyethylene terephthalate film, the second substrate layer 12 is formed of a stretched nylon film, and the first substrate layer 11 and the second substrate layer 12 are bonded by an adhesive layer (thickness of, for example, about 2 to 5 μm).

[0034] For example, the outer packaging material 10 for an electric storage device Figure 2 to Figure 4 As shown, for the purpose of improving the interlayer adhesion between the substrate layer 1 and the barrier layer 3, an adhesive layer 2 may be provided between the two as required. Figure 3 and Figure 4 As shown in FIG. 1 , for the purpose of improving the interlayer adhesion between the barrier layer 3 and the heat-fusible resin layer 4, a bonding layer 5 may be provided between the two as required. Figure 4As shown, a surface covering layer 6 may be provided on the outside of the substrate layer 1 (the opposite side of the heat-fusible resin layer 4) as required. It should be noted that when the surface covering layer 6 is present on the outside of the substrate layer 1, the substrate layer 1 is formed to include a structure of the surface covering layer 6, specifically, a three-layer structure in which the surface covering layer 6, the first substrate layer 11, and the second substrate layer 12 are stacked in sequence, or a four-layer structure in which the surface covering layer 6, the first substrate layer 11, the adhesive layer, and the second substrate layer 12 are stacked in sequence.

[0035] From the perspective of reducing costs and improving energy density, the thickness of the laminate constituting the outer packaging material 10 for a storage device may be preferably, but not particularly limited to, about 190 μm or less, about 155 μm or less, or about 120 μm or less. From the perspective of maintaining the function of the outer packaging material for a storage device such as protecting the storage device element, the thickness of the laminate constituting the outer packaging material for a storage device 10 may be preferably about 35 μm or more, about 45 μm or more, or about 60 μm or more. In addition, the preferred range of the laminate body constituting the outer packaging material 10 for the storage device is, for example, about 35 to 190 μm, about 35 to 155 μm, about 35 to 120 μm, about 45 to 190 μm, about 45 to 155 μm, about 45 to 120 μm, about 60 to 190 μm, about 60 to 155 μm, about 60 to 120 μm, and particularly preferably about 60 to 155 μm.

[0036] In the outer packaging material 10 for a storage device, the ratio of the total thickness of the base material layer 1, the adhesive layer 2 provided as required, the barrier layer 3, the bonding layer 5 provided as required, the heat-fusible resin layer 4, and the surface covering layer 6 provided as required to the thickness (total thickness) of the laminate constituting the outer packaging material 10 for a storage device is preferably 90% or more, more preferably 95% or more, and further preferably 98% or more. As a specific example, when the outer packaging material 10 for a storage device of the present invention includes the base material layer 1, the adhesive layer 2, the barrier layer 3, the bonding layer 5, and the heat-fusible resin layer 4, the ratio of the total thickness of the above-mentioned layers to the thickness (total thickness) of the laminate constituting the outer packaging material 10 for a storage device is preferably 90% or more, more preferably 95% or more, and further preferably 98% or more. In addition, when the outer packaging material 10 for the storage device of the present invention is a laminate comprising a substrate layer 1, an adhesive layer 2, a barrier layer 3 and a thermally fusible resin layer 4, the ratio of the total thickness of the above-mentioned layers to the thickness (total thickness) of the laminate constituting the outer packaging material 10 for the storage device can be, for example, 80% or more, preferably 90% or more, more preferably 95% or more, and further preferably 98% or more.

[0037] 2. Forming each layer of the outer packaging material for the power storage device

[0038] [Base material layer 1]

[0039] In the present invention, the substrate layer 1 is a layer provided for the purpose of functioning as a substrate of an outer packaging material for a storage device. The substrate layer 1 is located on the outer layer side of the outer packaging material for a storage device. The substrate layer 1 may be the outermost layer (a layer constituting the outer surface), and in the case where, for example, a surface covering layer 6 described later is provided, the surface covering layer 6 may also be the outermost layer (a layer constituting the outer surface).

[0040] In the present invention, the substrate layer 1 is composed of two or more layers. Figures 1 to 4 As shown, it is preferred that a laminated body including a first substrate layer 11 and a second substrate layer 12 is provided. In addition, the substrate layer 1 includes one or more layers of polyester film. It is preferred that the first substrate layer 11 is formed of a polyester film.

[0041] In the outer packaging material 10 for the storage battery device of the present invention, the work hardening index of the substrate layer 1 as a whole in the length direction (MD direction) and the width direction is greater than 2.5 and less than 4.5, and the difference (absolute value) between the work hardening index in the length direction and the width direction is less than 1.4.

[0042] The work hardening index of the substrate layer 1 is a value calculated from the stress at an elongation of 5% and the stress at an elongation of 60% obtained by a tensile test, determined by the method described in the evaluation method "(14) Work hardening index of the entire substrate layer" in the later described embodiment.

[0043] The laminate used for the outer packaging material for storage devices includes a substrate layer, a barrier layer and a heat-fusible resin layer, wherein the thickness of the substrate layer is often designed to be the thinnest. In the case of deep drawing of the outer packaging material for storage devices, the stress applied in the thickness direction determines the neutral axis according to the work hardening state of each layer, and determines which positions in the thickness direction the stress is concentrated. By making the overall work hardening state of the substrate layer 1, that is, the work hardening index, be above 2.5, the offset of the neutral axial barrier layer and the heat-fusible resin layer side is suppressed, making the barrier layer susceptible to uniform stress, and as a result, the breakage of the barrier layer and the generation of pinholes during the deep drawing process can be suppressed. Therefore, the work hardening index of the substrate layer 1 as a whole needs to be above 2.5. From the perspective of avoiding the neutral axis from deviating to the outermost layer side, the work hardening index of the substrate layer 1 in either the length direction (MD direction) or the width direction (TD direction) needs to be below 4.5.

[0044] In order to make the work hardening index of the substrate layer 1 in the longitudinal direction (MD direction) and the width direction (TD direction) reach 2.5 or more and 4.5 or less, it is preferred that, for example, the breaking strength of the substrate layer 1 in the longitudinal direction (MD direction) and the width direction (TD direction) is 180 MPa or more, more preferably 200 MPa or more, 220 MPa or more, or 230 MPa or more. Moreover, the tensile elongation at break in the longitudinal direction (MD direction) and the width direction (TD direction) of the substrate layer 1 is preferably 80% or more, more preferably 90% or more, 95% or more, or 100% or more. The breaking strength and tensile elongation at break of the substrate layer 1 are values ​​obtained by tensile testing determined by the method described in the evaluation method "(13) Breaking strength and tensile elongation at break of the entire substrate layer" in the examples described later.

[0045] In order to make the breaking strength of the base material layer 1 reach 180 MPa or more and the tensile breaking elongation reach 80% or more, for example, the polyester film contained in the base material layer 1 can be stretched at a high ratio during the manufacturing process. Specifically, it is most preferred to stretch in two axial directions, and the stretching can be performed sequentially or simultaneously at an area stretching ratio of 11.0 times or more by a known method. When the work hardening index of the polyester film described later is 1.6 or more, the deep drawing formability is excellent. On the other hand, the higher the work hardening index, the greater the elastic deformation caused by bending during deep drawing, and therefore the warping after forming is often greater. Therefore, it is preferred to control the work hardening index to a minimum according to the required warping degree.

[0046] From the perspective of showing a better effect of the present invention, the work hardening index of the substrate layer 1 as a whole is preferably about 2.6 or more. In addition, the work hardening index of the substrate layer 1 as a whole is preferably 4.0 or less. The preferred range of the work hardening index of the substrate layer 1 as a whole can be about 2.5 to 4.5, about 2.5 to 4.0, about 2.6 to 4.5, and about 2.6 to 4.0.

[0047] In the present invention, from the perspective of in-plane uniformity, the difference between the work hardening index in the length direction (MD direction) and the width direction (TD direction) of the substrate layer 1 is 1.4 or less. Since the difference between the work hardening index in the length direction and the width direction is 1.4 or less, the in-plane uniformity is high, the load is applied evenly after the drawing process, local deformation is not likely to occur, and the drawing formability is excellent. The difference in the work hardening index is preferably 1.2 or less.

[0048] Next, the polyester film included in the base material layer 1 will be described in detail.

[0049] The polyester film contained in the substrate layer 1 has a work hardening index of 1.6 or more and 3.0 or less in both the longitudinal direction (MD direction) and the width direction (TD direction), and the difference between the work hardening indexes in the longitudinal direction and the width direction is preferably 0.5 or less. In addition, the polyester film preferably has an intrinsic viscosity of 0.66 dl / g or more and 1.00 dl / g or less, more preferably 0.66 dl / g or more and 0.95 dl / g or less. In addition, the rigid amorphous component content of the polyester film is preferably 5% or more and 60% or less.

[0050] The work hardening index of the polyester film is a value calculated from the stress at an elongation of 5% and the stress at an elongation of 60% obtained by a tensile test and determined by the method described in the evaluation method "(10) Work hardening index" in the Examples described later.

[0051] As described above, when the outer packaging material for the storage device is deep-drawn, the stress applied in the thickness direction determines the neutral axis according to the work hardening state of each layer, and determines the positions in the thickness direction where the stress is concentrated. By making the work hardening state of the polyester film contained in the substrate layer 1, that is, the work hardening index be 1.6 or more, the neutral axis is not easily deviated to the barrier layer and the heat-fusible resin layer side, and the barrier layer is easily subjected to uniform stress, resulting in the suppression of the breakage of the barrier layer and the generation of pinholes during the deep drawing process. Therefore, in the substrate layer 1 of the present invention, the polyester film preferably has a work hardening index of at least 1.6. From the perspective of avoiding the neutral axis from deviating to the outermost layer side, the work hardening index of the polyester film is preferably less than 3.0 in either the length direction (MD direction) or the width direction.

[0052] In order to make the work hardening index of the polyester film in the longitudinal direction (MD direction) and the width direction (TD direction) reach 1.6 or more and 3.0 or less, the tensile breaking strength of the film in the longitudinal direction (MD direction) and the width direction (TD direction) is preferably, for example, 200 MPa or more.

[0053] In order to make the tensile strength of the polyester film reach 200MPa or more, the polyester film can be stretched at a high ratio during the manufacturing process. Specifically, it is most preferred to stretch in two axial directions, and the stretching can be performed sequentially or simultaneously at an area stretching ratio of 11.0 times or more by a known method. When the work hardening index is 1.6 or more, the stretching formability is improved. On the other hand, if the work hardening index is too high, the elastic deformation caused by bending during deep drawing will increase, so the warping after forming often increases. Therefore, it is preferred to control the work hardening index to a minimum according to the desired warping degree.

[0054] From the perspective of showing a better effect of the present invention, the work hardening index of the polyester film is, for example, 1.6 or more, preferably 1.8 or more, and more preferably 2.0 or more. In addition, the work hardening index of the polyester film is 3.0 or less, preferably 2.9 or less. As a preferred range of the work hardening index of the polyester film, there can be cited about 1.6 to 3.0, about 1.6 to 2.9, about 1.8 to 3.0, about 1.8 to 2.9, about 2.0 to 3.0, and about 2.0 to 2.9.

[0055] In the present invention, from the perspective of in-plane uniformity, the difference (absolute value) between the work hardening index of the polyester film in the length direction (MD direction) and the width direction (TD direction) is preferably 0.5 or less. Since the difference between the work hardening index in the length direction (MD direction) and the width direction is 0.5 or less, the in-plane uniformity is high, and it is easy to achieve uniform load application after deep drawing and suppress local deformation. The difference in work hardening index is preferably 0.3 or less.

[0056] In the present invention, from the perspective of in-plane uniformity, the difference between the work hardening index of the polyester film in the longitudinal direction (MD direction) and the width direction (TD direction) is preferably 0.5 or less. Since the difference between the work hardening index in the longitudinal direction (MD direction) and the width direction is 0.5 or less, the in-plane uniformity is high, and it is easy to achieve uniform load application after deep drawing and suppress local deformation. The difference in work hardening index is preferably 0.3 or less.

[0057] In the present invention, the tensile elongation at break of at least one of the length direction (MD direction) and the width direction (TD direction) of the polyester film is preferably 65% ​​or more. One of the deformation behaviors of the material during the drawing process is elongation. The greater the elongation of the film, the larger the part that can be stretched and deformed in the deformation behavior, and the better the drawing process performance. Therefore, it is preferred that the tensile elongation at break in at least one of the length direction and the width direction is 65% or more, and more preferably the tensile elongation at break in both the length direction and the width direction is 65% or more. In order to make the tensile elongation at break in the length direction and the width direction 65% or more, it can be adjusted by making the stretching ratio in both directions less than 4.0 times. Although the situation in which there is a direction with a stretching ratio exceeding 4.0 times is beneficial to improving the work hardening index, the tensile elongation at break in the stretching direction will be less than 65%, making the deep drawing formability low, which is not conducive to deep drawing. The tensile elongation at break of the polyester film in both the longitudinal direction and the width direction is preferably 65% ​​or more, more preferably 70% or more, further preferably 75% or more, further preferably 90% or more, further preferably 100% or more, and further preferably 110% or more; and preferably 150% or less, more preferably 140% or less, and further preferably 130% or less. Preferred ranges of the tensile elongation at break include about 65-150%, about 65-140%, about 65-130%, about 70-150%, about 70-140%, about 70-130%, about 75-150%, about 75-140%, about 75-130%, about 90-150%, about 90-140%, about 90-130%, about 100-150%, about 65-140%, and about 65-130%. The tensile elongation at break of the polyester film was measured by the method described in the evaluation method "(6) Tensile elongation at break" in the Examples described later.

[0058] In the present invention, the polyester film preferably has a rigid amorphous component amount of 5% or more and 60% or less relative to the component amount of the entire film. The rigid amorphous component amount is measured by the method described in the evaluation method "(8) Rigid amorphous component amount" of the embodiment described later. Since the rigid amorphous component amount is within this range, a particularly significant performance in the thickness direction, namely puncture resistance, can be obtained. The drawing process performed on the outer packaging material for the storage device is generally a process in which the four corners are fixed with a mold and extruded in the thickness direction. By controlling the rigid amorphous component amount relative to the entire film within this range, excellent drawing processing performance will be exhibited in the above-mentioned drawing process. Since the rigid amorphous component amount is less than 60%, the situation in which the amorphous component occupies most of the main composition of the film is suppressed, and the dimensional stability of the film tends to improve. On the other hand, since the rigid amorphous component amount is more than 5%, it is easy to improve the puncture resistance as a performance in the thickness direction.

[0059] From the perspective of achieving better effects of the present invention, the amount of the rigid amorphous component of the polyester film is, for example, 5% or more, preferably 6% or more, more preferably 8% or more, further preferably 15% or more, further preferably 28% or more, further preferably 30% or more, and further preferably 35% or more. Furthermore, the amount of the rigid amorphous component of the polyester film is 60% or less, preferably 58% or less, more preferably 55% or less, and further preferably 53% or less. Preferred ranges of the rigid amorphous component content of the polyester film include about 5 to 60%, about 5 to 58%, about 5 to 55%, about 5 to 53%, about 6 to 60%, about 6 to 58%, about 6 to 55%, about 6 to 53%, about 8 to 60%, about 8 to 58%, about 8 to 55%, about 8 to 53%, about 15 to 60%, about 15 to 58%, about 15 to 55%, about 15 to 53%, about 28 to 60%, about 28 to 58%, about 28 to 55%, about 28 to 53%, about 30 to 60%, about 30 to 58%, about 30 to 55%, about 30 to 53%, about 35 to 60%, about 35 to 58%, about 35 to 55%, and about 35 to 53%.

[0060] The bulk state of the film depends not only on the crystallization performance of the raw materials used, but also on the film forming conditions. For example, in the case of using polyethylene terephthalate, in order to set the amount of rigid amorphous components to 5% or more, a method of setting the plane orientation coefficient fn of the film to 0.165 or more can be cited. Among them, the plane orientation coefficient of the film is measured by the method described in the evaluation method "(5) Plane orientation coefficient fn of polyester film" in the embodiment described later. In order to set the plane orientation coefficient of the film to 0.165 or more, a method of setting the area stretching ratio in the biaxial stretching process to 12.25 times or more can be cited. In addition, it is preferred to control the amount of rigid amorphous components by the heat treatment temperature after the stepwise biaxial stretching. The important point is that the maximum temperature (heat treatment temperature) applied during the film forming process is set to 200°C or less. On the other hand, when the heat treatment temperature is set to 230°C or more, the amount of rigid amorphous components tends to increase because the resin begins to melt, but since the heat crystallization of the film is promoted, the crystallinity described later is increased, and as the main composition of the film, the crystallinity will also be higher than that of rigid amorphous. Therefore, it is important that the heat treatment temperature is below 200° C. In the case where the heat treatment temperature of the film exceeds 200° C. and is below 230° C., the amount of the rigid amorphous component will be less than 5%.

[0061] From the perspective of showing a better effect of the present invention, the crystallinity of the polyester film is preferably 15% to 40%. It is possible to control the crystallinity by stretching oriented crystallization or thermally induced crystallization to improve the mechanical strength of the film. When the crystallinity is lower than 15%, the surface orientation of the film may be insufficient and the work hardening index may not be controlled within the scope of the present invention; when the crystallinity exceeds 40%, the amount of rigid amorphous component may not be controlled within the scope of the present invention. In order to set the crystallinity to 15% to 40%, it can be adjusted by, for example, using a homopolymer polyester resin, setting the film surface orientation coefficient to 0.165 to 0.170, and the heat treatment temperature to 150°C to 200°C, but it can also be mixed with other resins. The crystallinity of the polyester film is measured by the method described in the evaluation method "(7) Crystallinity" in the later examples.

[0062] From the perspective of showing a better effect of the present invention, the crystallinity of the polyester is, for example, 15% or more, preferably 16% or more, more preferably 18% or more, and further preferably 20% or more. The crystallinity of the polyester film is 40% or less, preferably 39% or less, more preferably 35% or less, and further preferably 32% or less. Preferred ranges of the crystallinity of the polyester film include about 15 to 40%, about 15 to 39%, about 15 to 35%, about 15 to 32%, about 16 to 40%, about 16 to 39%, about 16 to 35%, about 16 to 32%, about 18 to 40%, about 18 to 39%, about 18 to 35%, about 18 to 32%, about 20 to 40%, about 20 to 39%, about 20 to 35%, and about 20 to 32%.

[0063] The intrinsic viscosity of the polyester film is preferably 0.66 dl / g or more and 1.00 or less, more preferably 0.66 dl / g or more and 0.95 dl / g or less. The intrinsic viscosity is a value measured by the method described in the evaluation method "(4) Intrinsic viscosity" of the embodiment described later. Since the intrinsic viscosity is within this range, the degree of entanglement of the molecular chain is improved, and tolerance to deformation in the thickness direction, especially puncture resistance, can be obtained. When the intrinsic viscosity is less than 0.66 dl / g, the degree of entanglement of the molecular chain is insufficient, and the drawing performance is easily reduced; on the other hand, since the intrinsic viscosity is less than 0.95 dl / g, or even less than 1.00 dl / g, the discharge amount will not decrease with the increase of the filtration pressure during the melt film forming process, and the production efficiency is very high. The intrinsic viscosity can be adjusted by the raw materials used in the melt film forming. When it is necessary to increase the intrinsic viscosity of the film, the intrinsic viscosity of the raw materials used in the film forming can be increased. When both the molecular chain entanglement effect and production efficiency are taken into consideration, the intrinsic viscosity is preferably 0.69 dl / g or more and 0.88 dl / g or less.

[0064] The intrinsic viscosity of the polyester film is preferably 0.66 dl / g or more and 0.95 dl / g or less. The intrinsic viscosity is a value measured by the method described in the evaluation method "(4) Intrinsic viscosity" of the embodiment described later. Since the intrinsic viscosity is within this range, the degree of entanglement of the molecular chain is improved, and tolerance to deformation in the thickness direction, especially puncture resistance, can be obtained. When the intrinsic viscosity is less than 0.66 dl / g, the degree of entanglement of the molecular chain is insufficient, and the deep drawing performance is easily reduced; on the other hand, when the intrinsic viscosity exceeds 0.95 dl / g, the discharge amount has to be reduced due to the increase in filtration pressure during the melt film forming process, and the production efficiency is poor. The intrinsic viscosity can be adjusted by the raw materials used in the melt film forming. When it is necessary to increase the intrinsic viscosity of the film, the intrinsic viscosity of the raw materials used in the film forming can be increased. When both the entanglement effect of the molecular chain and the production efficiency are taken into consideration, the intrinsic viscosity is preferably 0.69 dl / g or more and 0.88 dl / g or less.

[0065] From the perspective of better performance of the effect of the present invention, the thermal shrinkage rate of the polyester film at a temperature of 150°C in both the length direction (MD direction) and the width direction (TD direction) is preferably 3.5% or more and 14.0% or less. In the lamination process in which the substrate layer 1 is heated at about 150°C, such as the extrusion lamination process in which the molten resin is directly laminated onto the film, the thermal shrinkage rate at 150°C is preferably 3.5% or more in order to suppress wrinkling during the extrusion lamination process. On the other hand, when the thermal shrinkage rate of the temperature applied during the lamination process exceeds 14%, the film may be deformed too much due to the thermal shrinkage during the lamination process, thereby causing defects. From the perspective of taking into account both wrinkling and thermal deformation during the lamination process, the thermal shrinkage rate of the polyester film at a temperature of 150°C in the length direction and the width direction is preferably 10% or less. In order to control the heat shrinkage rate at 150°C in the longitudinal direction and the width direction to be 3.5% or more and 14.0% or less, the area ratio of the film is set to 12.25 times or more and the heat treatment temperature is set to 160°C or more and 200°C or less. The heat shrinkage rate at 150°C in the longitudinal direction and the width direction of the polyester film is measured by the method described in the evaluation method "(11) Heat shrinkage rate at 150°C in the longitudinal direction and the width direction of the polyester film" in the examples described later.

[0066] From the perspective of achieving a better effect of the present invention, the polyester film preferably has a melting point (melting endothermic peak temperature (Tm)) of 235°C or more as determined by a differential scanning calorimeter. When the polyester film is used as a base material layer of an outer packaging material for a storage device, a container is formed by heat-sealing the heat-fusible resin layers to each other. Therefore, it is necessary to suppress the melting of the outer packaging material due to the heat of the heat seal. When the melting endothermic peak temperature Tm is lower than 235°C, it is necessary to lower the heating temperature during heat sealing, and the time required to form a container by heat sealing becomes longer, and the mass production efficiency may be poor. Therefore, in order to make the melting endothermic peak temperature Tm above 235°C, it is most preferred to use a homopolymer polyester. It should be noted that from the perspective of the ease of processing of the polyester film, the melting point is preferably below 320°C. The melting point of the polyester film is measured by the method described in the evaluation method "(9) Glass transition temperature Tg, melting point (melting endothermic peak temperature Tm)" in the later described embodiment.

[0067] From the perspective of achieving better effects of the present invention, the melting point of the polyester film is 235° C. or higher, preferably 238° C. or higher, more preferably 240° C. or higher, and further preferably 245° C. or higher. Furthermore, the melting point of the polyester film is, for example, 320° C. or lower, preferably 300° C. or lower, more preferably 290° C. or lower, and further preferably 270° C. or lower. Preferred ranges of the melting point of the polyester film include 235 to 320°C, 235 to 300°C, 235 to 290°C, 235 to 270°C, 238 to 320°C, 238 to 300°C, 238 to 290°C, 238 to 270°C, 240 to 320°C, 240 to 300°C, 240 to 290°C, 240 to 270°C, 245 to 320°C, 245 to 300°C, 245 to 290°C, and 245 to 270°C.

[0068] When the polyester film is a mixture of two or more polyesters and exhibits two or more melting points, the highest melting point temperature may be 235° C. or higher. Examples of the mixture with polyester include, but are not particularly limited to, polyethylene naphthalate, polycarbonate, and polybutylene terephthalate.

[0069] The polyester film is mainly composed of polyester. Polyester is a general term for polymer compounds whose main chemical bonds in the main chain are ester bonds. Moreover, polyester can usually be obtained by polycondensation reaction of dicarboxylic acids or their derivatives with diols or their derivatives. Since it is mainly composed of polyester, it can achieve resistance to electrolyte corrosion. In addition, "mainly composed" as described in the present invention refers to a proportion of more than 60% by mass and less than 100% by mass relative to the whole object, and this example refers to the proportion relative to the polyester film. Among them, the dicarboxylic acid unit (structural unit) or the diol unit (structural unit) refers to a divalent organic group excluding the part removed by polycondensation, and is expressed by the following general formula.

[0070] Dicarboxylic acid unit (structural unit): -CO-R-CO

[0071] Diol unit (structural unit): -O-R'-O-

[0072] Wherein, R and R' are divalent organic groups and R and R' may be the same or different.

[0073] Examples of diols or derivatives thereof that can be used for polyesters include, in addition to ethylene glycol, aliphatic dihydroxy compounds such as 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, and neopentyl glycol; polyoxyalkylene glycols such as diethylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; alicyclic dihydroxy compounds such as 1,4-cyclohexanediol and spiroglycol; aromatic dihydroxy compounds such as bisphenol A and bisphenol S; and derivatives of the above compounds.

[0074] In addition, as dicarboxylic acids or derivatives thereof that can be used for polyester, in addition to terephthalic acid, aromatic dicarboxylic acids such as isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, diphenyl dicarboxylic acid, diphenylsulfon dicarboxylic acid, diphenoxyethane dicarboxylic acid, and sodium dicarboxylate-5-sulfonate, aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, dimer acid, maleic acid, and fumaric acid, alicyclic dicarboxylic acids such as 1,4-cyclohexane dicarboxylic acid, oxocarboxylic acids such as p-hydroxybenzoic acid, and derivatives of the above acids can be cited. As derivatives of dicarboxylic acids, for example, esters such as dimethyl terephthalate, diethyl terephthalate, 2-hydroxyethyl methyl terephthalate, dimethyl 2,6-naphthalenedicarboxylate, dimethyl isophthalate, dimethyl adipate, diethyl maleate, and dimethyl dicarboxylate can be cited.

[0075] The polyester film may be a single-layer structure or a multilayer structure of more than two layers. In the case of a multilayer structure, from the perspective of suppressing warping after film formation, a symmetrical structure such as B layer / A layer / B layer with the center layer as the base point is preferably adopted. Once warping occurs after film formation, operability will deteriorate in subsequent processes such as battery manufacturing processes. In addition, in the present invention, a five-layer structure such as B / A / B / A / B may also be used. In the case of a multilayer structure, from the perspective of warping after film formation, a three-layer laminated structure of B / A / B is preferably used. In the present invention, if it is a double-layer structure such as A layer / B layer with different molecular orientations, warping may occur immediately after film formation. However, as long as it does not hinder the effect of the present invention, an asymmetric structure such as an A / B double-layer structure may also be used.

[0076] In order to improve the drawing performance of the polyester film, the dynamic friction coefficient μd of the contact surface on the mold side is preferably set to 0.3 or less. By setting the dynamic friction coefficient in the above range, the deformation resistance during drawing can be reduced and the processing performance can be improved. The dynamic friction coefficient of the polyester film is measured by the method described in the evaluation method "(12) Dynamic friction coefficient of polyester film" of the embodiment described later. The technical means for making the dynamic friction coefficient below 0.3 can be, but is not particularly limited to, for example, the outermost layer has inorganic particles with an average particle size of 0.005μm or more and 10μm or less, and / or a layer with 0.3% by mass or more and 5% by mass or less of organic particles. More preferably, it is 0.5% by mass or more and 3% by mass. However, if the particles are added in excess, the tensile elongation at break of the outer packaging material may be reduced. Therefore, it is important to add particles within a range that does not hinder the effect of the present invention. It should be noted that in the present invention, particles with an average primary particle size of 0.005μm or more are used. The particle size described in this example refers to the number average particle size, which refers to the particle size observed in the cross section of the film. When the shape is not a perfect circle, the value converted to a perfect circle of equal area is used as the particle size. The number average particle size Dn can be obtained by the following steps (1) to (4).

[0077] (1) First, a film cross section is cut using a microtome without crushing the film in the thickness direction, and a magnified observation image is obtained using a scanning electron microscope. In this case, the cutting is performed in a direction parallel to the TD direction (transverse direction) of the film.

[0078] (2) Next, the cross-sectional area S of each particle observed in the cross section of the image is calculated, and the particle diameter d is calculated by the following formula.

[0079] d=2×(S / π) 1 / 2

[0080] (3) Using the obtained particle diameter d and the number n of resin particles, Dn is calculated from the following formula.

[0081] Dn=Σd / n

[0082] Wherein, Σd is the sum of the particle sizes of the particles in the observation plane, and n is the total number of particles in the observation plane.

[0083] (4) Change the position and perform the above (1) to (3) at 5 positions, and take the average value as the number average particle size of the particles. 2 The above area is an observation point.

[0084] As inorganic particles, for example, wet or dry silica, colloidal silica, aluminum silicate, titanium oxide, calcium carbonate, calcium phosphate, barium sulfate, aluminum oxide, mica, kaolin, clay, etc. can be used. In addition, as organic particles, particles with styrene, silicone, acrylic acid, methacrylic acid, polyester and divinyl compounds, etc. as components can be used. Among them, inorganic particles such as wet or dry silica, aluminum oxide, calcium carbonate and particles with styrene, silicone, acrylic acid, methacrylic acid, polyester, divinylbenzene, etc. as components are preferably used. In addition, these inorganic particles and organic particles can also be used in combination of two or more. In addition, in order to control the maximum surface height, it is also preferred to apply unevenness processing such as embossing and sandblasting to the film surface.

[0085] From the perspective of molding (shape) followability after being used as a substrate layer of an outer packaging material for a storage device and warping after molding, the thickness of the polyester film is preferably 5 μm or more and 40 μm or less, more preferably 9 μm or more and 30 μm or less. The most preferred thickness is 12 μm or more and 28 μm or less. Although it depends on the required drawing, when it is less than 5 μm, the moldability may be poor, and when it is more than 40 μm, the rigidity becomes high and warping may occur after molding.

[0086] For example, in order to improve the adhesion with the adjacent layer, it is preferred to implement corona treatment, plasma treatment, ozone treatment, and surface treatment such as setting an anchoring agent layer on the polyester film surface. As a method for forming an anchoring agent layer, a method of coating a resin on the film surface (composite melt extrusion method, hot melt coating method, online and offline coating method of solvent-soluble or water-soluble and / or water-dispersible resin other than water, etc.) can be cited. Among them, from the perspective of forming a uniform coating film and production efficiency, it is preferred to coat the film preparation on one side of the film surface before the oriented crystallization is completed, and stretch and heat-treat it in at least one direction to complete the online coating method of oriented crystallization. In addition, in the case of setting an anchoring agent layer, as a resin, it is possible to use, but not particularly limited to, for example, acrylic resin, polyurethane resin, polyester resin, olefin resin, fluororesin, vinyl resin, chlorine-containing resin, styrene resin, various grafted resins, epoxy resin, silicone resin, etc., and a mixture of these resins can also be used. From the perspective of adhesion, polyester resin, acrylic resin or polyurethane resin is preferably used. When polyester resin is used as aqueous coating liquid, water-soluble or water-dispersible polyester resin is used. To form such water-solubility or water-dispersibility, it is preferably copolymerized with a compound containing a sulfonate group or a compound containing a carboxylate group. When acrylic resin is used as aqueous coating liquid, since it is necessary to form a state of being dissolved or dispersed in water, a surfactant (for example, polyether compounds, etc., can be cited but not limited to) is sometimes used as an emulsifier. In addition, in the case of an anchoring agent layer, in order to further improve adhesion, the resin can be used in combination with various crosslinking agents. As crosslinking agent resins, melamine-based, epoxy-based, and oxazoline-based resins are generally used.

[0087] In the present invention, the substrate layer 1 may include at least one layer of polyester film. As described above, the substrate layer 1 is composed of two or more layers. Therefore, when the substrate layer 1 is composed only of polyester film, the substrate layer 1 includes two or more layers of polyester film. In addition, the substrate layer 1 may include a layer (other layer) different from the polyester film in addition to the polyester film. The material forming the other layer is not particularly limited, as long as it has the function of a substrate, that is, at least has insulation properties. The other layer can be formed by, for example, using a resin, and the resin may also contain additives described later.

[0088] The other layers may be, for example, a resin film formed by a resin, or a coating formed by applying a resin. The resin film may be an unstretched film or a stretched film. As the stretched film, a uniaxially stretched film and a biaxially stretched film may be cited, preferably a biaxially stretched film. As the stretching method for forming the biaxially stretched film, for example, a sequential biaxial stretching method, a blow molding method, a simultaneous biaxial stretching method, etc. may be cited. As the method for applying the resin, a roll coating method, a gravure coating method, an extrusion coating method, etc. may be cited.

[0089] As the resin forming the other layers, for example, polyamide, polyolefin, epoxy resin, acrylic resin, fluororesin, polyurethane, silicone resin, phenolic resin and the like and modified products of these resins can be cited. In addition, the resin forming the other layers can also be a copolymer of these resins, or a modified product of a copolymer. In addition, it can also be a mixture of these resins.

[0090] From the perspective of showing better effects of the present invention, polyamide is preferably used as the resin forming the other layer. That is, when the substrate layer 1 of the present invention further includes other layers different from the polyester film, the substrate layer 1 is preferably a laminate of a polyester film and a polyamide film.

[0091] Specific examples of polyamides include aliphatic polyamides such as nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, and copolymers of nylon 6 and nylon 66; hexamethylenediamine-isophthalic acid-terephthalic acid copolymer polyamides such as nylon 6I, nylon 6T, nylon 6IT, and nylon 6I6T (I represents isophthalic acid, and T represents terephthalic acid) containing structural units derived from terephthalic acid and / or isophthalic acid; polyamide MXD6 (polyadipic acid Polyamides containing aromatic compounds such as polyamide (m-xylene diamine); alicyclic polyamides such as polyamide PACM6 (polybis(4-aminocyclohexyl)methane adipamide); polyamides obtained by copolymerizing a lactam component and / or an isocyanate component such as 4,4'-diphenylmethane-diisocyanate; polyesteramide copolymers and polyetheresteramide copolymers as copolymers of a copolymerized polyamide and a polyester or a polyalkylene ether glycol; and copolymers of the above compounds. These polyamides may be used alone or in combination of two or more.

[0092] The polyamide film is preferably a stretched polyamide film, more preferably a stretched nylon film, and further preferably a biaxially stretched nylon film.

[0093] The substrate layer 1 may be a laminated body in which each film is laminated using an adhesive, etc., or a laminated body in which two or more layers of films are formed by co-extruding resins. In addition, the laminated body in which two or more layers of resin films are formed by co-extruding resins may be formed directly as the substrate layer 1 without being stretched, or may be formed by uniaxial stretching or biaxial stretching.

[0094] In addition, since polyester is unlikely to change color even when an electrolyte solution adheres to the surface, for example, the polyester film is preferably located on the outermost layer side of the base material layer 1 (the first base material layer 11 ).

[0095] In the present invention, the substrate layer 1 is preferably a laminate in which the first substrate layer 11 is a polyester film and the second substrate layer 12 is a polyamide film, and particularly preferably a laminate in which the polyester film as the first substrate layer 11 and the polyamide film as the second substrate layer 12 are bonded by an adhesive layer.

[0096] In the present invention, the preferred composition of the substrate layer 1 is a laminated structure in which the first substrate layer 11 is formed of a polyester film, the second substrate layer 12 is formed of a polyamide film, and the first substrate layer 11 and the second substrate layer 12 are bonded by an adhesive layer (thickness is, for example, about 2 to 5 μm). A more preferred composition of the substrate layer 1 is a laminated structure in which the first substrate layer 11 is formed of a polyethylene terephthalate film, the second substrate layer 12 is formed of a nylon film, and the first substrate layer 11 and the second substrate layer 12 are bonded by an adhesive layer (thickness is, for example, about 2 to 5 μm). A further preferred composition of the substrate layer 1 is a laminated structure in which the first substrate layer 11 is formed of a biaxially stretched polyethylene terephthalate film, the second substrate layer 12 is formed of a stretched nylon film, and the first substrate layer 11 and the second substrate layer 12 are bonded by an adhesive layer (thickness is, for example, about 2 to 5 μm). These laminated structures are all three-layer structures in which the first substrate layer 11, the adhesive layer, and the second substrate layer 12 are laminated in order from the outside to the inside.

[0097] As for the preferred adhesive for bonding the first substrate layer 11 and the second substrate layer 12, the same products as the adhesive described in the adhesive layer 2 described later can be cited. It should be noted that there is no particular limitation on the method for laminating two or more layers of resin films, and a known method can be adopted, for example, dry lamination, sandwich lamination, extrusion lamination, hot lamination, etc., preferably dry lamination. When lamination is performed by dry lamination, a polyurethane adhesive is preferably used as an adhesive. In this case, the thickness of the adhesive can be, for example, about 2 to 5 μm. In addition, as described above for the polyester film, an anchoring agent layer can be formed by laminating the resin film used for the substrate layer. The anchoring agent layer can be the same product as the adhesive described in the adhesive layer 2 described later. In this case, the thickness of the anchoring agent layer can be, for example, about 0.01 to 1.0 μm.

[0098] In addition, additives such as lubricants, flame retardants, antiblocking agents, antioxidants, light stabilizers, tackifiers, and antistatic agents may be present on at least one of the surface and the interior of the base layer 1. The additives may be used alone or in combination of two or more.

[0099] In the present invention, from the perspective of improving the moldability of the outer packaging material for the storage device, it is preferred that a lubricant is present on the surface of the substrate layer 1. As a lubricant, preferably, but not particularly limited to, an amide-based lubricant can be cited. As specific examples of amide-based lubricants, for example, saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, hydroxymethylamides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid ester amides, aromatic bisamides, etc. can be cited. As specific examples of saturated fatty acid amides, lauramide, palmitamide, stearamide, behenamide, hydroxystearamide, etc. can be cited. As specific examples of unsaturated fatty acid amides, oleamide, erucamide, etc. can be cited. As specific examples of substituted amides, N-oleoyl palmitamide, N-stearyl stearamide, N-stearyl oleamide, N-oleoyl stearamide, N-stearyl erucamide, etc. can be cited. In addition, as specific examples of hydroxymethylamides, hydroxymethyl stearamide, etc. can be cited. Specific examples of saturated fatty acid bisamides include methylene bisstearamide, ethylene biscaprylamide, ethylene bislaurylamide, ethylene bisstearamide, ethylene bishydroxystearamide, ethylene bisbehenamide, hexamethylene bisstearamide, hexamethylene bisbehenamide, hexamethylene hydroxystearamide, N,N'-distearyl adipamide, N,N'-distearyl sebacamide, etc. Specific examples of unsaturated fatty acid bisamides include ethylene bisoleamide, ethylene biserucamide, hexamethylene bisoleamide, N,N'-dioleoyl adipamide, N,N'-dioleoyl sebacamide, etc. Specific examples of fatty acid ester amides include stearamide stearic acid ethyl ester, etc. In addition, specific examples of aromatic bisamides include m-xylene bisstearamide, m-xylene bishydroxystearamide, N,N'-distearyl isophthalic acid amide, etc. The lubricants may be used alone or in combination of two or more.

[0100] When a lubricant is present on the surface of the base material layer 1, the amount of lubricant present is preferably, but not particularly limited to, about 3 mg / m 2 More preferably, 4 to 15 mg / m 2 About 5 to 14 mg / m 2 about.

[0101] The lubricant present on the surface of the base layer 1 may be a product obtained by exuding the lubricant contained in the resin constituting the base layer 1 , or may be a product obtained by applying the lubricant on the surface of the base layer 1 .

[0102] There is no particular restriction on the thickness (total thickness) of the substrate layer 1, as long as it can function as a substrate. From the perspective of showing a better effect of the present invention, it is preferably about 10 μm or more, and more preferably about 15 μm or less. Based on the same perspective, it is preferably about 60 μm or less, more preferably about 50 μm or less, and further preferably about 45 μm or less. As the preferred range of the thickness of the substrate layer 1, about 10 to 60 μm, about 10 to 50 μm, about 10 to 45 μm, about 15 to 60 μm, about 15 to 50 μm, and about 15 to 45 μm can be cited. As the thickness of the resin film (polyester film, other layers) constituting each layer of the substrate layer 1, it can be cited that it is preferably about 2 to 25 μm, more preferably about 5 to 25 μm, and further preferably about 10 to 25 μm.

[0103] For example, the thickness of the first substrate layer 11 is preferably greater than about 9 μm, more preferably greater than about 10 μm, and preferably less than about 40 μm, more preferably less than about 30 μm, and further preferably less than about 25 μm. Preferred ranges include about 9 to 40 μm, about 9 to 30 μm, about 9 to 25 μm, about 10 to 40 μm, about 10 to 30 μm, and about 10 to 25 μm.

[0104] In addition, the thickness of the second substrate layer 12 is preferably greater than about 10 μm, more preferably greater than about 12 μm, further preferably greater than about 15 μm, and is preferably less than about 40 μm, more preferably less than about 35 μm, further preferably less than about 30 μm. Preferred ranges include about 10 to 40 μm, about 10 to 35 μm, about 10 to 30 μm, about 12 to 40 μm, about 12 to 35 μm, about 12 to 30 μm, about 15 to 40 μm, about 15 to 35 μm, and about 15 to 30 μm.

[0105] [Adhesive layer 2]

[0106] In the packaging material for a power storage device of the present invention, the adhesive layer 2 is a layer provided between the base layer 1 and the barrier layer 3 as necessary for the purpose of improving the adhesion between the two layers.

[0107] The adhesive layer 2 is formed by an adhesive capable of bonding the substrate layer 1 to the barrier layer 3. The adhesive used in forming the adhesive layer 2 may be, but is not particularly limited to, any of a chemical reaction type, a solvent volatilization type, a hot melt type, a hot pressing type, and the like. In addition, it may be a two-component curing adhesive (two-component adhesive), a one-component curing adhesive (one-component adhesive), or a resin that does not undergo a curing reaction. In addition, the adhesive layer 2 may be a single layer or a multilayer.

[0108] As the bonding components contained in the bonding agent, specific examples include polyesters such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, and copolyesters; polyethers; polyurethanes; epoxy resins; phenolic resins; polyamides such as nylon 6, nylon 66, nylon 12, and copolyamides; polyolefin resins such as polyolefins, cyclic polyolefins, acid-modified polyolefins, and acid-modified cyclic polyolefins; polyvinyl acetate; cellulose; (meth) acrylic resins; polyimides; polycarbonates; amino resins such as urea resins and melamine resins; rubbers such as chloroprene rubber, nitrile rubber, and styrene-butadiene rubber; silicone resins, etc. These bonding components can be used alone or in combination of two or more. Among these bonding components, polyurethane bonding agents can also be preferably used. In addition, the resins forming these bonding components can be used with appropriate curing agents to improve bonding strength. The curing agent can be selected from a suitable compound such as polyisocyanate, polyfunctional epoxy resin, oxazoline group-containing polymer, polyamine resin, acid anhydride, etc., depending on the functional group of the bonding component.

[0109] As a polyurethane adhesive, for example, a polyurethane adhesive including a main agent containing a polyol compound and an auxiliary agent containing an isocyanate compound can be cited. Preferably, a two-component curing polyurethane adhesive with a polyol such as polyester polyol, polyether polyol and acryl polyol as a main agent and an aromatic or aliphatic polyisocyanate as an auxiliary agent can be cited. In addition, as a polyurethane adhesive, for example, a polyurethane adhesive containing a polyurethane compound and an isocyanate compound obtained by reacting a polyol compound with an isocyanate compound in advance can be cited. In addition, as a polyurethane adhesive, for example, a polyurethane adhesive containing a polyurethane compound and a polyol compound obtained by reacting a polyol compound with an isocyanate compound in advance can be cited. In addition, as a polyurethane adhesive, for example, a polyurethane adhesive cured by reacting a polyurethane compound obtained by reacting a polyol compound with an isocyanate compound in advance with moisture in the air can be cited. As a polyol compound, it is preferred to use a polyester polyol having a hydroxyl group in the side chain in addition to the hydroxyl group at the end of the repeating unit. As auxiliary agent, aliphatic, alicyclic, aromatic, aromatic aliphatic isocyanate compounds can be cited. As isocyanate compounds, for example, hexamethylene diisocyanate (HDI), xylene diisocyanate (XDI), isophorone diisocyanate (IPDI), hydrogenated XDI (H6XDI), hydrogenated MDI (H12MDI), toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), etc. can be cited. In addition, polyfunctional isocyanate modified bodies of one or more of these diisocyanates can also be cited. In addition, as polyisocyanate compounds, polymers (such as trimers) can also be used. Such polymers can include adducts, biuret bodies, urate bodies, etc. By making the adhesive layer 2 be formed by a polyurethane adhesive, it is possible to bring excellent electrolyte corrosion resistance to the outer packaging material for the storage device, even if the electrolyte is attached to the side, the peeling of the substrate layer 1 can also be suppressed.

[0110] In addition, as long as it does not hinder adhesion, the bonding agent layer 2 also allows the addition of other components, and can contain coloring agent, thermoplastic elastomer, tackifier, filler, etc. By making the bonding agent layer 2 contain coloring agent, it is possible to color the outer packaging material for the storage device. As coloring agent, known materials such as pigments and dyes can be used. In addition, coloring agent can only use one, or can mix two or more to use.

[0111] The type of pigment is not particularly limited as long as it is within the range that does not impair the adhesion of the adhesive layer 2. Examples of organic pigments include azo, phthalocyanine, quinacridone, anthraquinone, dioxazine, indigothioindigo, pyrenone-perylene, isoindolenine, and benzimidazolone pigments, and examples of inorganic pigments include carbon black, titanium oxide, cadmium, lead, chromium oxide, and iron pigments. In addition, examples include fine powder of mica, fish scale foil, and the like.

[0112] Among the colorants, carbon black is also preferred in order to make the appearance of the outer packaging material for an electric storage device black, for example.

[0113] The average particle size of the pigment may be, but is not particularly limited to, about 0.05 to 5 μm, preferably about 0.08 to 2 μm. The average particle size of the pigment is the median particle size measured by a laser diffraction / scattering particle size distribution measuring device.

[0114] The content of the pigment in the adhesive layer 2 is not particularly limited as long as the outer packaging material for the electric storage device can be colored, and is, for example, about 5 to 60% by mass, preferably about 10 to 40% by mass.

[0115] The thickness of the adhesive layer 2 is not particularly limited as long as the substrate layer 1 and the barrier layer 3 can be bonded, and is, for example, about 1 μm or more, about 2 μm or more. In addition, the thickness of the adhesive layer 2 is, for example, about 10 μm or less, about 5 μm or less. In addition, the preferred range of the thickness of the adhesive layer 2 includes about 1 to 10 μm, about 1 to 5 μm, about 2 to 10 μm, and about 2 to 5 μm.

[0116] [Coloring Layer]

[0117] The coloring layer is a layer (not shown) provided between the base layer 1 and the barrier layer 3 as required. In the case of having a binder layer 2, the coloring layer may be provided between the base layer 1 and the binder layer 2, or between the binder layer 2 and the barrier layer 3. In addition, the coloring layer may be provided outside the base layer 1. By providing the coloring layer, the outer packaging material for the power storage device can be colored.

[0118] The colored layer can be formed by, for example, applying ink containing a colorant to the surface of the base layer 1 or the surface of the barrier layer 3. As the colorant, known materials such as pigments and dyes can be used. In addition, the colorant can be used alone or in combination of two or more.

[0119] Specific examples of the colorant contained in the colored layer include the same colorants as exemplified in the section [Adhesive Layer 2].

[0120] [Barrier layer 3]

[0121] In the packaging material for a power storage device, the barrier layer 3 is a layer that at least suppresses the penetration of moisture.

[0122] As the barrier layer 3, for example, metal foil, vapor-deposited film, resin layer, etc. with barrier properties can be cited. As the vapor-deposited film, metal vapor-deposited film, inorganic oxide vapor-deposited film, carbon-containing inorganic oxide vapor-deposited film, etc. can be cited; as the resin layer, polyvinylidene chloride, polymers with chlorotrifluoroethylene (CTFE) as the main component, polymers with tetrafluoroethylene (TFE) as the main component, polymers with fluoroalkyl groups, and polymers with fluoroalkyl units as the main component, etc., fluororesins, ethylene-vinyl alcohol copolymers, etc. can be cited. In addition, as the barrier layer 3, resin films having at least one layer of these vapor-deposited films and resin layers can also be cited. The barrier layer 3 can also be provided with multiple layers. The barrier layer 3 preferably includes a layer formed by a metal material. As the metal material constituting the barrier layer 3, specifically aluminum alloy, stainless steel, titanium steel, steel plate, etc. can be cited. When used in the form of metal foil, it is preferably included at least one of aluminum alloy foil and stainless steel foil.

[0123] From the perspective of improving the formability of the outer packaging material for the storage device, the aluminum alloy foil is preferably a soft aluminum alloy foil formed by, for example, an aluminum alloy that has been annealed, and from the perspective of further improving the formability, it is preferably an aluminum alloy foil containing iron. In the aluminum alloy foil containing iron (100% by mass), the iron content is preferably 0.1 to 9.0% by mass, and more preferably 0.5 to 2.0% by mass. By making the iron content 0.1% or more, an outer packaging material for a storage device with better formability can be obtained. By making the iron content 9.0% or less, an outer packaging material for a storage device with better flexibility can be obtained. As soft aluminum alloy foil, for example, aluminum alloy foil having a composition specified in JIS H4160: 1994A8021H-O, JIS H4160: 1994A8079H-O, JIS H4000: 2014A8021P-O or JIS H4000: 2014A8079P-O can be cited. In addition, silicon, magnesium, copper, manganese, etc. can be added as needed. Softening can be achieved by annealing treatment, etc.

[0124] In addition, examples of stainless steel foil include austenitic, ferrite, austenitic / ferrite, martensitic, and precipitation-hardened stainless steel foils. From the perspective of providing a packaging material for a power storage device with better formability, the stainless steel foil is preferably made of austenitic stainless steel.

[0125] Specific examples of the austenitic stainless steel constituting the stainless steel foil include SUS304, SUS301, and SUS316L. Among them, SUS304 is particularly preferred.

[0126] In the case of a metal foil, the thickness of the barrier layer 3 may be such that it can at least function as a barrier layer to inhibit water penetration, and for example, it may be about 9 to 200 μm. The thickness of the barrier layer 3 is preferably about 85 μm or less, more preferably about 50 μm or less, further preferably about 40 μm or less, and particularly preferably about 35 μm or less. In addition, the thickness of the barrier layer 3 is preferably about 10 μm or more, more preferably about 20 μm or more, and further preferably about 25 μm or more. In addition, as a preferred range of the thickness of the barrier layer 3, about 10 to 85 μm, about 10 to 50 μm, about 10 to 40 μm, about 10 to 35 μm, about 20 to 85 μm, about 20 to 50 μm, about 20 to 40 μm, about 20 to 35 μm, about 25 to 85 μm, about 25 to 50 μm, about 25 to 40 μm, and about 25 to 35 μm. When the barrier layer 3 is formed of an aluminum alloy foil, the above range is particularly preferred. In addition, when the barrier layer 3 is formed of an aluminum alloy foil, from the perspective of giving the outer packaging material 10 for a storage device high formability (plasticity) and high rigidity, the thickness of the barrier layer 3 is preferably about 45 μm or more, more preferably about 50 μm or more, and preferably about 85 μm or less, more preferably about 75 μm or less, and more preferably about 70 μm or less. As a preferred range, it is about 45 to 85 μm, about 45 to 75 μm, about 45 to 70 μm, about 50 to 85 μm, about 50 to 75 μm, about 50 to 70 μm, about 55 to 85 μm, about 55 to 75 μm, about 55 to 70 μm. By making the outer packaging material 10 for a storage device have high formability, deep drawing is easily achieved, and it is expected to achieve a high capacity of the storage device. In addition, when the capacity of the power storage device is increased, the weight of the power storage device will increase. However, by increasing the rigidity of the outer packaging material 10 for the power storage device, it is expected to achieve high sealing of the power storage device. In addition, when the barrier layer 3 is formed of a stainless steel foil, the thickness of the stainless steel foil is preferably about 60 μm or less, more preferably about 50 μm or less, further preferably about 40 μm or less, further preferably about 30 μm or less, and particularly preferably about 25 μm or less. In addition, the thickness of the stainless steel foil is preferably about 10 μm or more, more preferably about 15 μm or more. In addition, as a preferred range of the thickness of the stainless steel foil, there can be cited about 10 to 60 μm, about 10 to 50 μm, about 10 to 40 μm, about 10 to 30 μm, about 10 to 25 μm, about 15 to 60 μm, about 15 to 50 μm, about 15 to 40 μm, about 15 to 30 μm, and about 15 to 25 μm.

[0127] In addition, in the case where the barrier layer 3 is a metal foil, in order to prevent dissolution and corrosion, it is preferred that at least the surface on the opposite side to the substrate layer has a corrosion-resistant protective film. The barrier layer 3 may have a corrosion-resistant protective film on both sides thereof. In the present invention, the corrosion-resistant protective film refers to a film that is subjected to a hot water modification treatment such as boehmite treatment, a chemical conversion treatment, anodizing treatment, a plating treatment of nickel or chromium, or an anti-corrosion treatment of a coating agent on the surface of the barrier layer to make the barrier layer have corrosion resistance (such as acid resistance, alkali resistance, etc.). The corrosion-resistant protective film specifically refers to a protective film that improves the acid resistance of the barrier layer (acid-resistant protective film), a protective film that improves the alkali resistance of the barrier layer (alkali-resistant protective film), etc. As a treatment for forming a corrosion-resistant protective film, one or more treatments may be performed. In addition, not only one layer but also multiple layers may be provided. In addition, among these treatments, the hot water modification treatment and the anodizing treatment are treatments in which the surface of the metal foil is dissolved by a treatment agent to form a metal compound with excellent corrosion resistance. It should be noted that these treatments may also be included in the definition of chemical conversion treatment. In addition, when the barrier layer 3 includes a corrosion-resistant protective film, the barrier layer 3 including the corrosion-resistant protective film is formed.

[0128] The corrosion-resistant protective film prevents peeling between the barrier layer (such as aluminum alloy foil) and the substrate layer during the molding process of the outer packaging material for the storage device; prevents the generation of hydrogen fluoride due to the reaction of the electrolyte and water, which leads to the dissolution and corrosion of the barrier layer surface, especially when the barrier layer is an aluminum alloy foil, prevents the dissolution and corrosion of aluminum oxide present on the barrier layer surface, and improves the adhesion (wettability) of the barrier layer surface, prevents peeling between the substrate layer and the barrier layer during heat sealing, and prevents peeling between the substrate layer and the barrier layer during molding.

[0129] As the corrosion-resistant protective film formed by chemical conversion treatment, various corrosion-resistant protective films are known, mainly including corrosion-resistant protective films containing at least one of phosphate, chromate, fluoride, triazine thiol compound and rare earth oxide. As the chemical conversion treatment using phosphate and chromate, for example, chromic acid-chromic acid passivation treatment, phosphoric acid-chromic acid passivation treatment, phosphoric acid-chromate treatment, chromate treatment, etc. can be mentioned, and as the chromium compound used for these treatments, for example, chromium nitrate, chromium fluoride, chromium sulfate, chromium acetate, chromium oxalate, chromium hydrogen phosphate, acetoacetic chromate, chromium chloride, potassium chromium sulfate, etc. can be mentioned. In addition, as the phosphorus compound used for these treatments, sodium phosphate, potassium phosphate, ammonium phosphate, polyphosphoric acid, etc. can be mentioned. In addition, as chromic acid passivation treatment, etching chromic acid passivation treatment, electrolytic chromic acid passivation treatment, coating type chromic acid passivation treatment, etc. can be mentioned, preferably coating type chromic acid passivation treatment. The coating type chromic acid passivation treatment is to first degrease the surface of at least the inner layer side of the barrier layer (e.g., aluminum alloy foil) by a known treatment method such as alkali immersion, electrolytic cleaning, acid cleaning, electrolytic acid cleaning, acid activation, etc., and then apply a treatment liquid containing a phosphate metal salt such as Cr (chromium) phosphate, Ti (titanium) phosphate, Zr (zirconium) phosphate, Zn (zinc) phosphate, and a mixture of these metal salts as a main component, or a treatment liquid containing a phosphate nonmetallic salt and a mixture of these nonmetallic salts as a main component, or a treatment liquid formed by a mixture of the above salts or their mixtures with a synthetic resin, etc., on the degreased surface by a known coating method such as roll coating, gravure printing, dipping, etc., and then dry the treatment liquid. The treatment liquid can use various solvents such as water, alcohol solvents, hydrocarbon solvents, ketone solvents, ester solvents, ether solvents, etc., preferably water. In addition, as the resin component used at this time, there can be mentioned high molecular compounds such as phenolic resin and acrylic resin, and there can be mentioned chromic acid passivation treatment using aminophenol polymers having repeating units represented by the following general formulas (1) to (4). It should be noted that in the aminophenol polymer, the repeating units represented by the following general formulas (1) to (4) can contain one type alone or any combination of two or more. The acrylic resin is preferably polyacrylic acid, acrylic acid-methacrylate copolymer, acrylic acid-maleic acid copolymer, acrylic acid-styrene copolymer or derivatives such as sodium salts, ammonium salts, and amine salts of the above acids. Particularly preferred are derivatives of polyacrylic acid such as ammonium salts, sodium salts, or amine salts of polyacrylic acid. In the present invention, polyacrylic acid refers to a polymer of acrylic acid. In addition, the acrylic resin is also preferably a copolymer of acrylic acid and a dicarboxylic acid or a dicarboxylic acid anhydride, and is also preferably an ammonium salt, sodium salt, or amine salt of a copolymer of acrylic acid and a dicarboxylic acid or a dicarboxylic acid anhydride. The acrylic resin can be used alone or in combination of two or more.

[0130] [Chemical formula 1]

[0131]

[0132] [Chemical formula 2]

[0133]

[0134] [Chemical formula 3]

[0135]

[0136] [Chemical formula 4]

[0137]

[0138] In the general formulae (1) to (4), X represents a hydrogen atom, a hydroxyl group, an alkyl group, a hydroxyalkyl group, an allyl group or a benzyl group. 1 and R 2 represents the same or different hydroxyl groups, alkyl groups or hydroxyalkyl groups. 1 and R 2 The alkyl group represented by , for example, can be a linear or branched alkyl group having 1 to 4 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, etc. 1 and R 2 The hydroxyalkyl group represented by the above-mentioned group includes, for example, hydroxymethyl, 1-hydroxyethyl, 2-hydroxyethyl, 1-hydroxypropyl, 2-hydroxypropyl, 3-hydroxypropyl, 1-hydroxybutyl, 2-hydroxybutyl, 3-hydroxybutyl, 4-hydroxybutyl, and other linear or branched alkyl groups having 1 to 4 carbon atoms substituted with one hydroxyl group. 1 and R 2 The alkyl group and the hydroxyalkyl group shown may be the same or different. In the general formulae (1) to (4), X is preferably a hydrogen atom, a hydroxyl group or a hydroxyalkyl group. The number average molecular weight of the aminophenol polymer having repeating units represented by the general formulae (1) to (4) is, for example, preferably in the range of 5 to 1,000,000, and more preferably in the range of 1,000 to 20,000. The aminophenol polymer can be prepared by, for example, polycondensing a phenol compound or a naphthol compound with formaldehyde to produce a polymer having repeating units represented by the general formula (1) or (3), and then reacting the mixture with formaldehyde and an amine (R 1 R 2 NH) will be functional group (-CH 2 NR 1 R 2 ) is introduced into the above-obtained polymer. The aminophenol polymer can be used alone or in combination of two or more.

[0139] As other examples of corrosion-resistant protective films, films formed by coating a coating type anti-corrosion treatment containing at least one coating agent selected from rare earth oxide sol, anionic polymers, and cationic polymers can be cited. The coating agent can further contain phosphoric acid or phosphate, and a cross-linking agent for polymer cross-linking. In the rare earth oxide sol, particles of rare earth oxide (for example, particles with an average particle size of less than 100 nm) are dispersed in the liquid dispersion medium. As rare earth oxides, cerium oxide, yttrium oxide, neodymium oxide, lanthanum oxide, etc. can be cited. From the perspective of further improving adhesion, cerium oxide is preferably used. The rare earth oxides contained in the corrosion-resistant protective film can be used alone or in combination of two or more. As the liquid dispersion medium of the rare earth oxide sol, various solvents such as water, alcohol solvents, hydrocarbon solvents, ketone solvents, ester solvents, and ether solvents can be used, preferably water. As the cationic polymer, preferably, for example, polyethyleneimine, an ionic polymer complex formed by a polymer having polyethyleneimine and a carboxylic acid, a primary amine grafted acrylic resin having a primary amine grafted on an acryl main skeleton, polyallylamine or its derivatives, aminophenol, etc. are used. In addition, as the anionic polymer, preferably, poly(meth)acrylic acid or its salt, or a copolymer with (meth)acrylic acid or its salt as the main component is used. In addition, the crosslinking agent is preferably selected from at least one of a compound having any functional group selected from isocyanate, glycidyl, carboxyl, oxazoline, and a silane coupling agent. In addition, the above-mentioned phosphoric acid or phosphate is preferably condensed phosphoric acid or condensed phosphate.

[0140] An example of the corrosion-resistant protective film is a film formed by applying a coating in which fine particles of metal oxides such as aluminum oxide, titanium oxide, cerium oxide, tin oxide, or barium sulfate are dispersed in phosphoric acid to the surface of the barrier layer and then baking the coating at a temperature of 150° C. or higher.

[0141] If necessary, the corrosion-resistant protective film may be formed into a laminated structure in which at least one of a cationic polymer and an anionic polymer is further laminated. Examples of the cationic polymer and the anionic polymer include the above-mentioned polymers.

[0142] In addition, the composition analysis of the corrosion-resistant protective film can be performed using, for example, time-of-flight secondary ion mass spectrometry.

[0143] The amount of the corrosion resistant protective film formed on the surface of the barrier layer 3 during the chemical conversion treatment is not particularly limited. For example, in the case of a coating type chromic acid passivation treatment, the amount of the corrosion resistant protective film formed on the surface of the barrier layer 3 is preferably 0.1 m2. 2The surface contains, in terms of chromium, a chromic acid compound in a ratio of, for example, about 0.5 to 50 mg, preferably about 1.0 to 40 mg; in terms of phosphorus, a phosphorus compound in a ratio of, for example, about 0.5 to 50 mg, preferably about 1.0 to 40 mg; and an aminophenol polymer in a ratio of, for example, about 1.0 to 200 mg, preferably about 5.0 to 150 mg.

[0144] The thickness of the corrosion-resistant protective film can be preferably, but not particularly limited to, about 1 nm to 20 μm, more preferably about 1 nm to 100 nm, and further preferably about 1 nm to 50 nm, from the perspective of the cohesive force of the protective film and the adhesion to the barrier layer or the thermally fusible resin layer. It should be noted that the thickness of the corrosion-resistant protective film can be measured by transmission electron microscopy, or by a combination of transmission electron microscopy and energy dispersive X-ray spectroscopy or electron beam energy loss spectroscopy. By analyzing the composition of the corrosion-resistant protective film using time-of-flight secondary ion mass spectrometry, for example, secondary ions (such as Ce, P, and O) derived from Ce, P, and O can be detected. 2 PO 4 ﹢ 、CePO 4 ﹣ At least one of the above) or secondary ions such as those derived from Cr, P and O (e.g. CrPO 2 ﹢ CrPO 4 ﹣ At least one of the above (etc.) characteristic peaks.

[0145] The chemical conversion treatment is carried out by applying a solution containing a compound used for forming a corrosion-resistant protective film to the surface of the barrier layer by a rod coating method, a roller coating method, a gravure coating method, a dipping method, etc., and then heating the barrier layer to a temperature of about 70 to 200°C. In addition, before the barrier layer is subjected to the chemical conversion treatment, the barrier layer may be subjected to a degreasing treatment by an alkali dipping method, an electrolytic cleaning method, an acid cleaning method, an electrolytic acid cleaning method, etc. In this way, the degreasing treatment can be more efficiently performed on the surface of the barrier layer. In addition, by using an acid degreasing agent in which a fluorine-containing compound is dissolved in an inorganic acid in the degreasing treatment, not only is there a degreasing effect on the metal foil, but also a passive metal fluoride can be formed. In this case, only the degreasing treatment can be performed.

[0146] [Thermal Fusible Resin Layer 4]

[0147] In the packaging material for a power storage device of the present invention, the heat-fusible resin layer 4 is the innermost layer and is a layer (sealing layer) that seals the power storage device element by heat-fusion bonding the heat-fusible resin layers when assembling the power storage device.

[0148] The resin forming the heat-fusible resin layer 4 is not particularly limited as long as it can be heat-fused. It is preferably a resin having a polyolefin skeleton such as polyolefin, acid-modified polyolefin, or a resin having a polyester skeleton such as polyethylene terephthalate and polybutylene terephthalate. The fact that the resin constituting the heat-fusible resin layer 4 has a polyolefin skeleton can be analyzed by, for example, infrared spectroscopy, gas chromatography-mass spectrometry, and the like. In addition, when analyzing the resin constituting the heat-fusible resin layer 4 by infrared spectroscopy, it is preferable to detect a characteristic peak derived from maleic anhydride. For example, when measuring maleic anhydride-modified polyolefin by infrared spectroscopy, at a wave number of 1760 cm ﹣1 Nearby and wave number 1780cm ﹣1 In the case where the heat-fusible resin layer 4 is a layer formed by maleic anhydride-modified polyolefin, when measured by infrared spectroscopy, the peak from maleic anhydride can be detected. However, when the acid modification degree is low, the characteristic peak becomes smaller and may not be detected. In this case, analysis can be performed by nuclear magnetic resonance spectroscopy.

[0149] As polyolefins, specific examples include polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; ethylene / α-olefin copolymers; polypropylenes such as homopolypropylene, polypropylene block copolymers (e.g., block copolymers of propylene and ethylene), and polypropylene random copolymers (e.g., random copolymers of propylene and ethylene); propylene / α-olefin copolymers; ethylene-butene-propylene terpolymers, etc. Among them, polypropylene is preferred. In the case of copolymers, the polyolefin resin may be a block copolymer or a random copolymer. These polyolefin resins may be used alone or in combination of two or more.

[0150] In addition, the polyolefin may also be a cyclic polyolefin. Cyclic polyolefin is a copolymer of an olefin and a cyclic monomer. Olefins as structural monomers of the cyclic polyolefin include, for example, ethylene, propylene, 4-methyl-1-pentene, styrene, butadiene, isoprene, etc. In addition, cyclic monomers as structural monomers of the cyclic polyolefin include, for example, cyclic olefins such as norbornene, cyclic dienes such as cyclopentadiene, dicyclopentadiene, cyclohexadiene, and norbornadiene, etc. Among them, cyclic olefins are preferred, and norbornene is more preferred.

[0151] Acid-modified polyolefin refers to a polymer obtained by block polymerization or graft polymerization of polyolefin using an acid component. As the acid-modified polyolefin, the above-mentioned polyolefin, or a copolymer obtained by copolymerizing the above-mentioned polyolefin with a polar molecule such as acrylic acid or methacrylic acid, or a polymer such as a cross-linked polyolefin can be used. In addition, as the acid component used for acid modification, carboxylic acids or their anhydrides such as maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, and itaconic anhydride can be cited.

[0152] The acid-modified polyolefin may also be an acid-modified cyclic polyolefin. The acid-modified cyclic polyolefin refers to a polymer obtained by replacing a part of the monomers constituting the cyclic polyolefin with an acid component and copolymerizing, or by block polymerization or graft polymerization of the acid component and the cyclic polyolefin. The acid-modified cyclic polyolefin is the same as described above. In addition, the acid component used in the acid modification is the same as the acid component used in the modification of the above-mentioned polyolefin.

[0153] Preferred examples of the acid-modified polyolefin include polyolefin modified with carboxylic acid or its anhydride, polypropylene modified with carboxylic acid or its anhydride, maleic anhydride-modified polyolefin, and maleic anhydride-modified polypropylene.

[0154] The heat-adhesive resin layer 4 may be formed of a single resin or a blended polymer of two or more resins. Furthermore, the heat-adhesive resin layer 4 may be formed of only one layer or two or more layers of the same or different resins.

[0155] The heat-adhesive resin layer 4 may contain a lubricant or the like as needed. When the heat-adhesive resin layer 4 contains a lubricant, the moldability of the packaging material for a power storage device can be improved. The lubricant is not particularly limited, and a known lubricant can be used.

[0156] As the lubricant, preferably, but not particularly limited to, an amide-based lubricant can be mentioned. Specific examples of the lubricant include the compounds described as examples for the base material layer 1. The lubricant may be used alone or in combination of two or more.

[0157] When a lubricant is present on the surface of the heat-fusible resin layer 4, the amount of lubricant present is not particularly limited, but from the perspective of improving the moldability of the packaging material for a storage device, a preferred amount is 10 to 50 mg / m 2 About 15 to 40 mg / m 2 about.

[0158] The lubricant present on the surface of the heat-adhesive resin layer 4 may be a product obtained by exuding the lubricant contained in the resin constituting the heat-adhesive resin layer 4 or by coating the lubricant on the surface of the heat-adhesive resin layer 4 .

[0159] In addition, the thickness of the heat-fusible resin layer 4 is not particularly limited as long as the heat-fusible resin layers can be heat-fused to each other and play the function of sealing the storage device element. For example, it can be about 100 μm or less, preferably about 85 μm or less, and more preferably about 15 to 85 μm. It should be noted that, for example, when the thickness of the bonding layer 5 described later is 10 μm or more, the thickness of the heat-fusible resin layer 4 can be preferably about 85 μm or less, and more preferably about 15 to 45 μm. For example, when the thickness of the bonding layer 5 described later is less than 10 μm or the bonding layer 5 is not provided, the thickness of the heat-fusible resin layer 4 can be preferably about 20 μm or more, and more preferably about 35 to 85 μm.

[0160] [Joint layer 5]

[0161] In the packaging material for a power storage device of the present invention, the bonding layer 5 is a layer provided between the barrier layer 3 (or the corrosion-resistant protective film) and the heat-fusible resin layer 4 as necessary in order to firmly bond the two.

[0162] The bonding layer 5 is formed of a resin capable of bonding the barrier layer 3 to the heat-fusible resin layer 4. As the resin used for forming the bonding layer 5, for example, the same resin as the bonding agent illustrated in the bonding agent 2 can be used. In addition, from the perspective of firmly bonding the bonding layer 5 to the heat-fusible resin layer 4, the resin used in the formation of the bonding layer 5 preferably contains a polyolefin skeleton, and the polyolefins, acid-modified polyolefins, cyclic polyolefins, and acid-modified cyclic polyolefins illustrated in the above-mentioned heat-fusible resin layer 4 can be cited. On the other hand, from the perspective of firmly bonding the barrier layer 3 and the bonding layer 5, the bonding layer 5 preferably contains an acid-modified polyolefin. As the acid-modified component, dicarboxylic acids such as maleic acid, itaconic acid, succinic acid, and adipic acid or their anhydrides, acrylic acid, methacrylic acid, etc. can be cited. From the perspective of the ease of modification and versatility, maleic anhydride is most preferred. In addition, from the perspective of the heat resistance of the outer packaging material for the storage device, it is preferred that the olefin component is a polypropylene resin, and it is most preferred that the bonding layer 5 contains maleic anhydride-modified polypropylene.

[0163] The fact that the resin constituting the bonding layer 5 has a polyolefin skeleton can be analyzed by, for example, infrared spectroscopy, gas chromatography-mass spectrometry, etc., and the analysis method is not particularly limited. In addition, when, for example, maleic anhydride-modified polyolefin is analyzed by infrared spectroscopy, the fact that the resin constituting the bonding layer 5 includes an acid-modified polyolefin can be determined at a wave number of 1760 cm ﹣1 Nearby and wave number 1780cm ﹣1 The characteristic peak from maleic anhydride can be detected nearby. However, when the degree of acid modification is low, the characteristic peak becomes smaller and may not be detected. In this case, analysis can be performed by nuclear magnetic resonance spectroscopy.

[0164] In addition, from the perspective of durability such as heat resistance and corrosion resistance of the storage device packaging material and the ability to reduce thickness while ensuring molding performance, the adhesive layer 5 is more preferably a cured product of a resin composition containing an acid-modified polyolefin and a curing agent. As the acid-modified polyolefin, the above examples are preferably cited.

[0165] In addition, the bonding layer 5 is preferably a cured product containing an acid-modified polyolefin and a resin composition selected from a compound with an isocyanate group, a compound with an oxazoline group and a compound with an epoxy group, and is particularly preferably a cured product containing an acid-modified polyolefin and a resin composition selected from a compound with an isocyanate group and a compound with an epoxy group. In addition, the bonding layer 5 preferably contains at least one selected from polyurethane, polyester and epoxy resin, and is more preferably polyurethane and epoxy resin. As polyester, it is preferably a polyester resin generated by the reaction of an epoxy group with maleic anhydride, an amide polyester resin generated by the reaction of an oxazoline group with maleic anhydride. It should be noted that in the case of unreacted products of curing agents such as compounds with isocyanate groups, compounds with oxazoline groups, and epoxy resins remaining in the bonding layer 5, the presence of unreacted products can be confirmed by methods selected from, for example, infrared spectroscopy, Raman spectroscopy, and time-of-flight secondary ion mass spectrometry (TOF-SIMS).

[0166] In addition, from the perspective of further enhancing the adhesion between the barrier layer 3 and the bonding layer 5, the bonding layer 5 is preferably a cured product of a resin composition containing a curing agent having at least one selected from an oxygen atom, a heterocyclic ring, a C=N bond, and a C-O-C bond. As a curing agent having a heterocyclic ring, for example, a curing agent having an oxazoline group, a curing agent having an epoxy group, etc. can be cited. In addition, as a curing agent having a C=N bond, a curing agent having an oxazoline group, a curing agent having an isocyanate group, etc. can be cited. In addition, as a curing agent having a C-O-C bond, a curing agent having an oxazoline group, a curing agent having an epoxy group, etc. can be cited. The fact that the bonding layer 5 is a cured product of a resin composition containing these curing agents can be confirmed by methods such as gas chromatography-mass spectrometry (GCMS), infrared spectroscopy (IR), time-of-flight secondary ion mass spectrometry (TOF-SIMS), and X-ray photoelectron spectroscopy (XPS).

[0167] There are no particular restrictions on the compound having an isocyanate group, but from the perspective of effectively improving the adhesion between the barrier layer 3 and the bonding layer 5, a polyfunctional isocyanate compound can be preferably cited. There are no particular restrictions on the polyfunctional isocyanate compound, as long as it is a compound having two or more isocyanate groups. Specific examples of polyfunctional isocyanate-based curing agents include pentamethylene diisocyanate (PDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), polymers or urate bodies of these isocyanates, mixtures thereof, or copolymers with other polymers, etc. In addition, adducts, biuret bodies, isocyanurate bodies, etc. can also be cited.

[0168] The content of the compound having an isocyanate group in the bonding layer 5 is preferably in the range of 0.1 to 50 mass %, more preferably in the range of 0.5 to 40 mass %, in the resin composition constituting the bonding layer 5 . This can effectively improve the adhesion between the barrier layer 3 and the bonding layer 5 .

[0169] The compound with oxazoline group is not particularly limited, as long as it is the compound with oxazoline skeleton. As the specific example of the compound with oxazoline group, the compound with polystyrene main chain, the compound with acryloyl main chain etc. can be enumerated. In addition, as commercially available product, for example, EPOCROS series etc. made by Nippon Catalyst Co., Ltd. can be enumerated.

[0170] The proportion of the compound having an oxazoline group in the bonding layer 5 is preferably in the range of 0.1 to 50 mass %, more preferably in the range of 0.5 to 40 mass %, in the resin composition constituting the bonding layer 5. This can effectively improve the adhesion between the barrier layer 3 and the bonding layer 5.

[0171] As a compound having an epoxy group, for example, an epoxy resin can be cited. As the epoxy resin, there is no particular limitation, as long as it is a resin that can form a cross-linked structure through the epoxy group present in the molecule, and a known epoxy resin can be used. As the weight average molecular weight of the epoxy resin, preferably about 50 to 2000, more preferably about 100 to 1000, and further preferably about 200 to 800 can be cited. It should be noted that in the first embodiment of the present invention, the weight average molecular weight of the epoxy resin is a measured value measured by gel permeation chromatography (GPC) under the condition of using polystyrene as a standard sample.

[0172] Specific examples of epoxy resins include glycidyl ether derivatives of trimethylolpropane, bisphenol A diglycidyl ether, modified bisphenol A diglycidyl ether, bisphenol F type glycidyl ether, linear phenol glycidyl ether, glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, etc. The epoxy resins may be used alone or in combination of two or more.

[0173] The proportion of the epoxy resin in the bonding layer 5 is preferably in the range of 0.1 to 50 mass %, more preferably in the range of 0.5 to 40 mass %, in the resin composition constituting the bonding layer 5. This can effectively improve the adhesion between the barrier layer 3 and the bonding layer 5.

[0174] The polyurethane is not particularly limited, and known polyurethanes can be used. The bonding layer 5 can be, for example, a cured product of a two-component curing type polyurethane.

[0175] The proportion of polyurethane in the bonding layer 5 is preferably in the range of 0.1 to 50% by mass, more preferably in the range of 0.5 to 40% by mass, in the resin composition constituting the bonding layer 5. This can effectively improve the adhesion between the barrier layer 3 and the bonding layer 5 in an environment where there are components that easily induce corrosion of the barrier layer, such as electrolytes.

[0176] It should be noted that when the bonding layer 5 is a cured product of a resin composition containing at least one selected from a compound having an isocyanate group, a compound having an oxazoline group and an epoxy resin and the above-mentioned acid-modified polyolefin, the acid-modified polyolefin acts as a main agent, and the compound having an isocyanate group, the compound having an oxazoline group and the compound having an epoxy group respectively act as a curing agent.

[0177] The bonding layer 5 may further contain a modifier having a carbodiimide group.

[0178] The thickness of the bonding layer 5 is preferably about 50 μm or less, about 40 μm or less, about 30 μm or less, about 20 μm or less, or about 5 μm or less, and the thickness of the bonding layer 5 is preferably about 0.1 μm or more, or about 0.5 μm or more. In addition, as the range of the thickness of the bonding layer 5, preferably about 0.1 to 50 μm, about 0.1 to 40 μm, about 0.1 to 30 μm, about 0.1 to 20 μm, about 0.1 to 5 μm, about 0.5 to 50 μm, about 0.5 to 40 μm, about 0.5 to 30 μm, about 0.5 to 20 μm, or about 0.5 to 5 μm can be cited. More specifically, in the case of the bonding agent or the cured product of the acid-modified polyolefin and the curing agent illustrated in the bonding agent layer 2, it is preferably about 1 to 10 μm, and more preferably about 1 to 5 μm. In addition, when the resin exemplified as the heat-fusible resin layer 4 is used, it is preferably about 2 to 50 μm, and more preferably about 10 to 40 μm. It should be noted that, when the bonding layer 5 is a cured product of a resin composition containing a bonding agent, an acid-modified polyolefin, and a curing agent exemplified as the bonding agent layer 2, the bonding layer 5 can be formed by, for example, applying the resin composition and curing it by heating. In addition, when the resin exemplified as the heat-fusible resin layer 4 is used, it can be formed by, for example, extrusion molding of the heat-fusible resin layer 4 and the bonding layer 5.

[0179] [Surface covering layer 6]

[0180] In the outer packaging material for a storage device of the present invention, for the purpose of improving at least one of designability, electrolyte corrosion resistance, scratch resistance, and formability, a surface covering layer 6 may be provided on the substrate layer 1 (on the side of the substrate layer 1 opposite to the barrier layer 3) as needed. The surface covering layer 6 is a layer located on the outermost side of the outer packaging material for a storage device after the storage device is assembled using the outer packaging material for a storage device.

[0181] The surface covering layer 6 can include resins such as polyvinylidene chloride, polyester, polyamide, epoxy resin, acrylic resin, fluororesin, polyurethane, silicone resin, phenolic resin, and modified products of these resins. In addition, it can also be a copolymer of these resins, and it can also be a modified product of the copolymer. It can also be a mixture of these resins. The resin is preferably a curable resin. That is, the surface covering layer 6 is preferably formed by a cured product of a resin composition containing a curable resin.

[0182] When the resin forming the surface covering layer 6 is a curable resin, the resin may be either a one-component curing type or a two-component curing type, preferably a two-component curing type. Examples of the two-component curing type resin include two-component curing type polyurethane, two-component curing type polyester, and two-component curing type epoxy resin. Among them, two-component curing type polyurethane is preferred.

[0183] As a two-component curing polyurethane, for example, a polyurethane including a main agent containing a polyol compound and an auxiliary agent containing an isocyanate compound can be cited. Preferably, a two-component curing polyurethane with a polyol such as polyester polyol, polyether polyol and acryl polyol as a main agent and an aromatic or aliphatic polyisocyanate as an auxiliary agent can be cited. In addition, as a polyurethane, for example, a polyurethane containing a polyurethane compound and an isocyanate compound obtained by reacting a polyol compound with an isocyanate compound in advance can be cited. As a polyurethane, for example, a polyurethane containing a polyurethane compound and a polyol compound obtained by reacting a polyol compound with an isocyanate compound in advance can be cited. As a polyurethane, for example, a polyurethane obtained by reacting a polyol compound with an isocyanate compound in advance and curing with moisture in the air can be cited. As a polyol compound, it is preferred to use a polyester polyol having a hydroxyl group in the side chain in addition to the hydroxyl group at the end of the repeating unit. As an auxiliary agent, aliphatic, alicyclic, aromatic, and aromatic aliphatic isocyanate compounds can be cited. As isocyanate compounds, for example, hexamethylene diisocyanate (HDI), xylene diisocyanate (XDI), isophorone diisocyanate (IPDI), hydrogenated XDI (H6XDI), hydrogenated MDI (H12MDI), toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), etc. can be cited. In addition, polyfunctional isocyanate modified bodies of one or more of these diisocyanates can also be cited. In addition, as polyisocyanate compounds, polymers (such as trimers) can also be used. Such polymers can include adducts, biuret bodies, urate bodies, etc. It should be noted that aliphatic isocyanate compounds refer to isocyanates with aliphatic groups but without aromatic rings, alicyclic isocyanate compounds refer to isocyanates with alicyclic hydrocarbon groups, and aromatic isocyanate compounds refer to isocyanates with aromatic rings. By forming the surface covering layer 6 from polyurethane, it is possible to impart excellent resistance to corrosion by an electrolyte to the outer packaging material for an electric storage device.

[0184] In the surface covering layer 6, at least one of the surface and the inside of the surface covering layer 6 can contain the above-mentioned lubricant, anti-blocking agent, matting agent, flame retardant, antioxidant, tackifier, antistatic agent and other additives as required according to the function of the surface covering layer 6 or its surface. As additives, for example, microparticles with an average particle size of about 0.5nm to 5μm can be cited. The average particle size of the additive is the median particle size measured by a laser diffraction / scattering particle size distribution measuring device.

[0185] The additive may be any of an inorganic substance and an organic substance. In addition, there is no particular limitation on the shape of the additive, and examples thereof include spherical, fibrous, plate-like, amorphous, and flaky shapes.

[0186] As the specific example of additive, talc, silica, graphite, kaolin, montmorillonite, mica, hydrotalcite, silica gel, zeolite, aluminum hydroxide, magnesium hydroxide, zinc oxide, magnesium oxide, aluminum oxide, neodymium oxide, antimony oxide, titanium oxide, cerium oxide, calcium sulfate, barium sulfate, calcium carbonate, calcium silicate, lithium carbonate, calcium benzoate, calcium oxalate, magnesium stearate, alumina, carbon black, carbon nanotube, high melting point nylon, acrylic resin, cross-linked acryl compound, cross-linked styrene, cross-linked polyethylene, benzoguanamine, gold, aluminum, copper, nickel, etc. can be enumerated. One kind of additive can be used alone, or two or more kinds can be used in combination. Among these additives, from the perspectives of dispersion stability, cost, etc., preferably silica, barium sulfate, titanium oxide can be enumerated. In addition, various surface treatments such as insulation treatment and high dispersibility treatment can also be implemented on the additive surface.

[0187] The method of forming the surface covering layer 6 is not particularly limited, and an example thereof includes a method of applying a resin that forms the surface covering layer 6. When an additive is added to the surface covering layer 6, the resin mixed with the additive may be applied.

[0188] The thickness of the surface covering layer 6 is not particularly limited as long as the above-mentioned function as the surface covering layer 6 can be exhibited, and is, for example, about 0.5 to 10 μm, preferably about 1 to 5 μm.

[0189] 3. Method for manufacturing outer packaging material for power storage device

[0190] There are no particular restrictions on the method for producing the outer packaging material for a storage device, as long as a laminated body formed by laminating the layers of the outer packaging material for a storage device of the present invention can be obtained, and the method comprises the steps of laminating at least a substrate layer 1, a barrier layer 3 and a heat-fusible resin layer 4 in sequence to obtain a laminated body. The substrate layer 1 is composed of two or more layers, the substrate layer 1 includes one or more layers of polyester film, the work hardening index of the substrate layer 1 in the longitudinal direction (MD direction) and the width direction (TD direction) are both 2.5 or more and 4.5 or less, and the difference between the work hardening index in the longitudinal direction and the width direction is 1.4 or less.

[0191] As an example of a method for manufacturing an outer packaging material for a storage device of the present invention, the following is described. First, a laminated body (hereinafter also referred to as "laminated body A") is formed in which a substrate layer 1, an adhesive layer 2, and a barrier layer 3 are laminated in sequence. The laminated body A can be formed specifically by applying an adhesive used in the formation of the adhesive layer 2 on the substrate layer 1 or on the barrier layer 3 whose surface has been chemically converted as required by a coating method such as a gravure coating method or a roll coating method, and drying it, and then laminating the barrier layer 3 or the substrate layer 1 and curing the adhesive layer 2 by a dry lamination method.

[0192] Next, a heat-fusible resin layer 4 is laminated on the barrier layer 3 of the laminate A. When the heat-fusible resin layer 4 is laminated directly on the barrier layer 3, it is sufficient as long as the heat-fusible resin layer 4 can be laminated on the barrier layer 3 of the laminate A by a method such as a heat lamination method, an extrusion lamination method, or the like. In addition, when a bonding layer 5 is provided between the barrier layer 3 and the heat-fusible resin layer 4, it is sufficient as long as, for example, (1) a method of laminating the bonding layer 5 and the heat-fusible resin layer 4 by extruding the bonding layer 5 on the barrier layer 3 of the laminate A (co-extrusion lamination method, tandem lamination method); (2) a method of separately forming a laminate in which the bonding layer 5 and the heat-fusible resin layer 4 are laminated, and laminating the laminate on the barrier layer 3 of the laminate A by a heat lamination method, or a method of forming a laminate in which the bonding layer 5 is laminated on the barrier layer 3 of the laminate A, and laminating the laminate by a heat lamination method. (1) a method of laminating a laminate with a heat-fusible resin layer 4; (2) a method of laminating a laminate with a heat-fusible resin layer 4; (3) a method of laminating a laminate with a heat-fusible resin layer 4 preformed as a sheet-like film by injecting a molten bonding layer 5 between the barrier layer 3 of the laminate A and the heat-fusible resin layer 4 preformed as a sheet-like film, and bonding the laminate A to the heat-fusible resin layer 4 with the aid of the bonding layer 5 (sandwich lamination method); (4) a method of coating a bonding agent solution for forming the bonding layer 5 on the barrier layer 3 of the laminate A and drying the bonding agent solution, or laminating the laminate by further baking, and laminating the heat-fusible resin layer 4 preformed as a sheet-like film on the bonding layer 5.

[0193] When the surface covering layer 6 is provided, the surface covering layer 6 is laminated on the surface of the substrate layer 1 on the opposite side to the barrier layer 3. The surface covering layer 6 can be formed, for example, by coating the above-mentioned resin for forming the surface covering layer 6 on the surface of the substrate layer 1. It should be noted that the order of the process of laminating the barrier layer 3 on the surface of the substrate layer 1 and the process of laminating the surface covering layer 6 on the surface of the substrate layer 1 is not particularly limited. For example, after the surface covering layer 6 is formed on the surface of the substrate layer 1, the barrier layer 3 can be formed on the surface of the substrate layer 1 on the opposite side to the surface covering layer 6.

[0194] As described above, a laminated body can be formed which has, in sequence, a surface covering layer 6 set as required / a base material layer 1 / an adhesive layer 2 set as required / a barrier layer 3 / a bonding layer 5 set as required / a hot-melt adhesive resin layer 4. However, in order to enhance the bonding property between the adhesive layer 2 set as required and the bonding layer 5, further heat treatment can be performed.

[0195] In the outer packaging material for a storage device, each layer constituting the laminate may be subjected to surface activation treatment such as corona treatment, sandblasting, oxidation treatment, ozone treatment, etc. as required to improve processing adaptability. For example, the surface of the substrate layer 1 opposite to the barrier layer 3 may be subjected to corona treatment to improve the adaptability of the surface of the substrate layer 1 to ink printing.

[0196] 4. Application of outer packaging materials for power storage devices

[0197] The outer packaging material for a storage device of the present invention is used in a packaging body for sealing and accommodating storage device elements such as a positive electrode, a negative electrode, and an electrolyte. That is, a storage device element having at least a positive electrode, a negative electrode, and an electrolyte can be accommodated in a packaging body formed by the outer packaging material for a storage device of the present invention to prepare a storage device.

[0198] Specifically, by using the outer packaging material for an electrical storage device of the present invention, in a state where the metal terminals respectively connected to the positive electrode and the negative electrode are protruding to the outside, the electrical storage device element having at least the positive electrode, the negative electrode and the electrolyte is covered in a manner that a flange portion (an area where the heat-fusible resin layers are in contact with each other) is formed at the periphery of the electrical storage device element, and the heat-fusible resin layers of the flange portion are heat-sealed to each other to achieve sealing, thereby obtaining an electrical storage device using the outer packaging material for an electrical storage device. It should be noted that, in the case where the electrical storage device element is accommodated in a packaging body formed by the outer packaging material for an electrical storage device of the present invention, the packaging body is formed in a manner that the heat-fusible resin portion of the outer packaging material for an electrical storage device of the present invention becomes the inner side (the surface in contact with the electrical storage device element). The heat-fusible resin layers of two outer packaging materials for an electrical storage device may be placed opposite to each other and overlapped, and the peripheral portions of the overlapped outer packaging materials for an electrical storage device may be heat-fused to form a packaging body, or as Figure 5 As shown in the example, a storage device is folded and closed with an outer packaging material, and the peripheral edge is heat-fused to form a package. Figure 5As shown in the example, the sides other than the folded sides are heat-fused to form a package body by sealing on three sides, or the package body can be folded in a manner to form a flange portion and sealed on four sides, or the outer packaging material for the storage device is wrapped around the storage device element, and the heat-fusible resin layers are heat-sealed to form a heat-fused portion, and a cover is provided to respectively close the openings at both ends, and the package is heat-fused with the outer packaging material for the storage device wrapped around the storage device element. The cover can be formed by, for example, a resin molded product, a metal molded product, an outer packaging material for the storage device, and the like. In addition, a recess for accommodating the storage device element can be formed in the outer packaging material for the storage device by deep drawing or stretch forming. As Figure 5 As shown in the example, one power storage device packaging material may be provided with the recessed portion, while the other power storage device packaging material may not be provided with the recessed portion, or the other power storage device packaging material may also be provided with the recessed portion.

[0199] The outer packaging material for the storage device of the present invention can be applied to storage devices such as batteries (including capacitors (condenser), capacitors (capacitor) etc.). In addition, the outer packaging material for the storage device of the present invention can also be used in any one of primary batteries and secondary batteries, preferably in secondary batteries. There is no particular restriction on the type of secondary battery to which the outer packaging material for the storage device of the present invention is applied, and examples thereof include lithium ion batteries, lithium ion polymer batteries, all-solid batteries, semi-solid batteries, quasi-solid batteries, polymer batteries, all-resin batteries, lead storage batteries, nickel-hydrogen storage batteries, nickel-cadmium storage batteries, nickel-iron storage batteries, nickel-zinc storage batteries, silver oxide-zinc storage batteries, metal-air batteries, multivalent cation batteries, capacitors, capacitors etc. Among these secondary batteries, lithium ion batteries and lithium ion polymer batteries can be cited as preferred applicable objects of the outer packaging material for the storage device of the present invention.

[0200] Example

[0201] Hereinafter, the present invention will be described in detail with reference to Examples and Comparative Examples, but the present invention is not limited to the Examples.

[0202] <Production and Evaluation of Polyester Film>

[0203] The polyester film was produced and evaluated according to the following methods.

[0204] (1) Composition of polyester

[0205] The polyester resin and film were dissolved in hexafluoroisopropanol (HFIP) and 1 H-NMR and 13 C-NMR was used to quantify the contents of monomer residues and by-product diethylene glycol.

[0206] (2) Film thickness and layer thickness

[0207] When measuring the overall thickness of the film, the film was cut into 200 mm × 300 mm using a micrometer, and the thickness of each sample at 5 random locations was measured and the average value was taken. In addition, the sample was embedded with epoxy resin, the film cross section was cut with a microtome, and the film cross section was observed with a transmission electron microscope (TEMH7100 manufactured by Hitachi, Ltd.) at a magnification of 5000 times to obtain the thickness of each layer of the film and the outer packaging material.

[0208] (3) Length and width directions of polyester film

[0209] In the present invention, the TD direction in the production of the polyester film is defined as the width direction, and the direction perpendicular to the width direction (MD direction (feed direction)) is defined as the longitudinal direction.

[0210] (4) Intrinsic viscosity

[0211] The solution viscosity was measured in o-chlorophenol at 25°C using an Ostwald viscometer, and the intrinsic viscosity of the polyester film was calculated based on the solution viscosity. The unit of the intrinsic viscosity is [dl / g]. It should be noted that the number n is 3, and the average value is taken.

[0212] (5) Planar orientation coefficient fn of polyester film

[0213] The layer for measuring the surface orientation coefficient (hereinafter referred to as the measuring layer) is brought into close contact with the glass surface, and then the sodium D line is used as the light source. An Abbe refractometer is used to measure the refractive indices (Nx, Ny, Nz) in the a direction, b direction and thickness direction, and the surface orientation coefficient fn of the measuring layer is calculated by the following formula.

[0214] Plane orientation coefficient fn = (Nx + Ny) / 2 - Nz

[0215] (6) Tensile elongation at break of polyester film

[0216] The film was cut into rectangular samples with a length of 150 mm and a width of 15 mm in the length and width directions. Under the conditions of 25°C and 63% Rh, a tensile tester (film strength and elongation automatic measuring device "TENSILON AMF / RTA-100" manufactured by Nippon Kaisha Instruments Co., Ltd.) was used to perform tensile tests on the length and width directions of the film at a crosshead speed of 50 mm / min, a width of 15 mm, and a chuck spacing of 30 mm. The elongation at break was taken as the tensile elongation at break. The measurement was performed 5 times, and the average value was adopted.

[0217] (7) Crystallinity of polyester film

[0218] According to JIS K7122 (1999), using a differential scanning calorimeter robot DSC-RDC220 manufactured by Seiko Instruments, and using "DISKSESSION" SSC / 5200 for data analysis, 5 mg of a film sample was placed on an aluminum tray and heated from room temperature to 300°C at a rate of 20°C / min, and maintained at 300°C for 5 minutes. At this time, the measured endothermic peak heat ΔHm, cold crystallization heat ΔHc, and melting heat ΔHm0 (140.1 J / g) of completely crystalline PET were calculated by the following formula.

[0219] Crystallinity (%) = (ΔHm - ΔHc) / ΔHm0 × 100

[0220] (8) Rigid amorphous component content of polyester film

[0221] The amount of the rigid amorphous component is calculated using the following formula based on the measured amount of the mobile amorphous component and the crystallinity.

[0222] The amount of rigid amorphous component (%) = 100 - (the amount of mobile amorphous component + crystallinity).

[0223] The theoretical value of the specific heat difference of completely amorphous polyethylene terephthalate is 0.4052 J / (g°C).

[0224] Furthermore, in the present invention, the theoretical value of the specific heat difference of a completely amorphous material of polyethylene terephthalate is referred to.

[0225] It should be noted that the amount of active amorphous components was measured in the following manner. Using a temperature transmitter DSC manufactured by TA Instruments, 5 mg of the sample was measured in a nitrogen environment at a heating rate of 2°C / min, a temperature transmission range of ±1°C, and a temperature transmission cycle of 60 seconds in the range of 0°C to 150°C. The specific heat difference at the measured glass transition temperature was obtained. It was calculated using the following formula.

[0226] Active amorphous component amount (%) = (specific heat difference) / (theoretical value of specific heat difference of completely amorphous polyester) × 100

[0227] Theoretical value of specific heat difference of completely amorphous polyethylene terephthalate = 0.4052 J / (g℃)

[0228] Furthermore, in the present invention, the product containing 70 mol % or more of polyethylene terephthalate units refers to the theoretical value of the specific heat difference of completely amorphous polyethylene terephthalate.

[0229] (9) Glass transition temperature Tg and melting point (melting endothermic peak temperature Tm) of polyester film

[0230] According to JIS K 7122 (1999), using a differential scanning calorimeter (EXSTARDSC6220 manufactured by Seiko Instruments), 3 mg of the resin was heated from 30°C to 300°C at 20°C / min in a nitrogen atmosphere. Then, the temperature was maintained at 300°C for 5 minutes, and then the temperature was lowered to 30°C at 40°C / min. After further maintaining the temperature at 30°C for 5 minutes, the temperature was increased from 30°C to 300°C at 20°C / min. The glass transition temperature obtained during the heating process was calculated by the following formula (i).

[0231] Glass transition temperature = (extrapolated glass transition start temperature + extrapolated glass transition end temperature) / 2(i)

[0232] Among them, the extrapolated glass transition start temperature is the temperature of the intersection of the straight line extending from the low temperature side baseline to the high temperature side and the tangent line drawn from the point where the slope of the curve of the glass transition step change part becomes the maximum value. The extrapolated glass transition end temperature is the temperature of the intersection of the straight line extending from the high temperature side baseline to the low temperature side and the tangent line drawn from the point where the slope of the curve of the glass transition step change part becomes the maximum value. In addition, the peak top of the endothermic peak accompanied by crystal melting of the resin is taken as the melting point (melting endothermic peak temperature Tm).

[0233] (10) Work hardening index of polyester film

[0234] The film was cut into rectangular samples with a length of 150 mm and a width of 15 mm in the length and width directions. Under the conditions of 25°C and 63% Rh, a tensile tester (film strength and elongation automatic measuring device "TENSILON AMF / RTA-100" manufactured by Nippon Kaisha Instruments Co., Ltd.) was used to perform tensile tests on the length and width directions of the film at a crosshead speed of 50 mm / min, a width of 15 mm, and a chuck spacing of 30 mm. The initial length was set to L. 0 (mm), the length at 5% elongation is L 1 (mm), the nominal stress at 5% elongation is set as P 1 (MPa), the length at which the elongation is 60% is L 2 (mm), the nominal stress at 60% elongation is set as P 2 (MPa), the true strain value at an elongation of 5% is obtained by formula (1), the true strain value at an elongation of 60% is obtained by formula (2), the true stress value at an elongation of 5% is obtained by formula (3), and the true stress value at an elongation of 60% is obtained by formula (4). Based on the values ​​obtained from (1) to (4), the slope of the equation established when the X-axis is the true strain and the Y-axis is the true stress is the work hardening index. The average value of 5 measurements in the length direction and the width direction was used.

[0235] True strain at 5% elongation = L n (L 1 / L 0 ) (1)

[0236] True strain at 60% elongation = L n (L 2 / L 1 ) (2)

[0237] True stress at 5% elongation = L n (P 1 (1+L n (L 1 / L 0 ))) (3)

[0238] True stress at 60% elongation = L n (P 2 (1+L n (L 2 / L 1 ))) (4)

[0239] ※L n : Natural logarithm

[0240] (11) Thermal shrinkage of polyester film in the length and width directions at 150°C

[0241] The film was cut into square samples with a length of 120 mm and a width of 120 mm. Lines were drawn perpendicularly at 100 mm in the length and width directions of the sample, and the sample was placed in a hot air oven heated to 150°C for 30 minutes for heat treatment. The distance between the lines after heat treatment was measured, and the heat shrinkage was calculated based on the change in the distance between the lines before and after heating to obtain the heat shrinkage. Five samples were measured in the length and width directions, and the average value was used for evaluation.

[0242] (12) Dynamic friction coefficient of polyester film

[0243] The sliding tester manufactured by Toyo Seiki Co., Ltd. was used to measure the stable area of ​​the resistance value after the initial rise after the two sides of the film were rubbed together according to JIS-K7125 (1999) as the dynamic friction coefficient μd. Three groups (6 sheets) of samples were cut from the roll in the length direction of the rectangle with a width of 80 mm and a length of 200 mm. The measurement was performed three times and the average value was calculated.

[0244] (Manufacture of polyester film)

[0245] Resins constituting polyester films used for film formation The raw materials, auxiliary materials and master batches of each example and each comparative example were mixed according to the types and proportions shown in Table 1. In addition, the raw materials, auxiliary materials and master batches of particles used in each example and comparative example were prepared as follows.

[0246] Polyester A

[0247] Polyethylene terephthalate resin containing 100 mol% of terephthalic acid component as a dicarboxylic acid component and 100 mol% of ethylene glycol component as a diol component (intrinsic viscosity: 0.72 dl / g)

[0248] Granule Masterbatch A

[0249] Polyester A is a polyethylene terephthalate pellet masterbatch containing agglomerated silica particles having an average particle size of 1.2 μm at a particle concentration of 2% by mass.

[0250] (Coating agent A)

[0251] Acrylic resin composed of a copolymer of methyl methacrylate / ethyl acrylate / acrylic acid / N-methacrylamide = 63 / 35 / 1 / 1% by mass: 3.00% by mass

[0252] Melamine crosslinking agent: 0.75 mass%

[0253] Colloidal silica particles (average particle size 80 nm): 0.15 mass%

[0254] Hexanol: 0.26 mass%

[0255] Butyl cellosolve: 0.18 mass%

[0256] Water: 95.66% by mass

[0257] Using an extruder, the polyester species and pellet masterbatch recorded in Table 1 were dried in a vacuum dryer at 180°C for 4 hours. After fully removing the moisture, the main raw material, the auxiliary raw material and the pellet masterbatch were put into the extruder as described in Table 1 and melted at a temperature of 280°C. Then, the molten resin extruded from the extruder was cooled and solidified on a casting drum cooled to 25°C with the resin extruded from the die mouth to obtain an unstretched sheet. At this time, the distance between the T-die die lip and the cooling drum was set to 35mm, and a linear electrode with a diameter of 0.1mm was used to apply static electricity at a voltage of 14kV to make it close to the cooling drum. In addition, the speed of the unstretched sheet passing through the cooling drum was set to 25m / min, and the contact length between the unstretched sheet and the cooling drum was set to 2.5m.

[0258] Subsequently, the unstretched sheet was preheated with a roller group heated to the film preheating temperature recorded in Table 2, and then stretched in the length direction (longitudinal direction) to the ratios shown in Table 2 using a heating roller controlled at the film stretching temperature recorded in Table 2, and cooled with a roller group at a temperature of 25°C to obtain a uniaxially stretched film. The uniaxially stretched film was subjected to corona discharge treatment in air, and ultrasonic dispersion and mixing were performed on the treated surface with coating agent A, and the surface bonded to the casting part was evenly coated with a #4 metal coating rod to perform surface treatment as an anchoring agent layer. Next, while holding both ends of the uniaxially stretched film with tweezers, it was guided to the preheating zone in the tenter machine that was controlled at the film preheating temperature recorded in Table 2, and continued to be continuously stretched in the heating zone that was kept at the film stretching temperature recorded in Table 2, and the direction perpendicular to the length direction (width direction) was stretched to the ratios shown in Table 2. Then, the film was heat treated for 20 seconds at the heat treatment temperature shown in Table 2 in the heat treatment zone of the tenter, and then relaxed at the relaxation temperature shown in Table 2 and at the relaxation rate shown in Table 2. Then, the film was cooled uniformly and slowly to obtain polyester films having the thickness shown in Table 2. The properties of the polyester film are shown in Table 3.

[0259] (13) Overall breaking strength and tensile elongation of the substrate layer

[0260] The substrate layer (laminated body of PET / adhesive layer / ONy) was cut into a rectangle of 150 mm long and 15 mm wide in the length and width directions and used as a sample. Under the conditions of 25°C and 63% Rh, a tensile tester (film strength and elongation automatic measuring device "TENSILON AMF / RTA-100" manufactured by Nippon Kaisha Instruments Co., Ltd.) was used to perform tensile tests on the length and width directions of the film at a crosshead speed of 50 mm / min, a width of 15 mm, and a chuck spacing of 30 mm. The load at the time of breaking was taken as the breaking strength, and the elongation at this time was taken as the tensile breaking elongation. The measurement was performed 5 times, and the average value was adopted. The results are shown in Table 5.

[0261] (14) Work hardening index of the entire base material layer

[0262] The substrate layer (a laminate of PET / adhesive layer / ONy) was cut into a rectangular shape of 150 mm long and 15 mm wide in the length and width directions and used as a sample. Under the conditions of 25°C and 63% Rh, a tensile tester ("TENSILON AMF / RTA-100", an automatic film strength and elongation measuring device manufactured by Nippon Kaisha Keiseki Co., Ltd.) was used to perform a tensile test on the length and width directions of the film at a crosshead speed of 50 mm / min, a width of 15 mm, and a chuck spacing of 30 mm. The initial length was set to L. 0 (mm), the length at 5% elongation is L 1(mm), the nominal stress at 5% elongation is set as P 1 (MPa), the length at which the elongation is 60% is L 2 (mm), the nominal stress at 60% elongation is set as P 2 (MPa), the true strain value at an elongation of 5% is obtained by formula (1), the true strain value at an elongation of 60% is obtained by formula (2), the true stress value at an elongation of 5% is obtained by formula (3), and the true stress value at an elongation of 60% is obtained by formula (4). Based on the values ​​obtained from (1) to (4), the slope of the established equation when the X-axis is the true strain and the Y-axis is the true stress is the work hardening index. The average value of 5 measurements in the length direction and the width direction was used. The results are shown in Table 5.

[0263] True strain at 5% elongation = L n (L 1 / L 0 ) (1)

[0264] True strain at 60% elongation = L n (L 2 / L 1 ) (2)

[0265] True stress at 5% elongation = L n (P 1 (1+L n (L 1 / L 0 )))(3)

[0266] True stress at 60% elongation = L n (P 2 (1+L n (L 2 / L 1 )))(4)

[0267] ※L n : Natural logarithm

[0268] <Manufacturing of packaging materials for power storage devices>

[0269] (Examples 1 to 4 and Comparative Examples 1 to 2)

[0270] As the first substrate layer 11, a resin film obtained by the above method (polyethylene terephthalate film, thickness as described in Table 2) was prepared. In addition, as the second substrate layer 12, a stretched nylon film (thickness and other properties as described in Table 4) was prepared. Next, the first substrate layer 11 and the second substrate layer 12 were laminated using a two-component curing polyurethane adhesive (polyol compound and aromatic isocyanate compound, thickness after curing was 3 μm), and a substrate layer 1 including a laminated film formed by laminating the first substrate layer 11 and the second substrate layer 12 via an adhesive layer was obtained. Next, the obtained substrate layer 1 and an aluminum foil (JIS H4160: 1994A8079H-O, thickness 60 μm) with a corrosion-resistant protective film formed on both surfaces as a barrier layer 3 were prepared. Next, the barrier layer and the ONy film side of the substrate layer were laminated by dry lamination using a two-component curing polyurethane adhesive (polyol compound and aromatic isocyanate compound), and then an aging treatment was performed to prepare a laminate of substrate layer (first substrate layer / adhesive layer / second substrate layer) / adhesive layer (thickness after curing is 3 μm) / barrier layer (thickness 60 μm).

[0271] Next, maleic anhydride-modified polypropylene (PPa, thickness 40 μm) as a bonding layer and polypropylene (PP, thickness 40 μm) as a heat-fusible resin layer were co-extruded on the barrier layer of the laminated body obtained above, thereby laminating the bonding layer / heat-fusible resin layer on the barrier layer. Next, the laminated body obtained was subjected to aging treatment and heated to obtain an outer packaging material for a storage battery device having a base material layer (PET / adhesive layer / ONy) / adhesive layer (thickness 3 μm) / barrier layer (thickness 60 μm) / adhesive layer (thickness 40 μm) / heat-fusible resin layer (thickness 40 μm) laminated in this order.

[0272] (Example 5 and Comparative Example 3)

[0273] As the first substrate layer 11, a resin film obtained by the above method (polyethylene terephthalate film, thickness as described in Table 2) was prepared. In addition, as the second substrate layer 12, a stretched nylon film (thickness and other properties as described in Table 4) was prepared. Next, the first substrate layer 11 and the second substrate layer 12 were laminated using a two-component curing polyurethane adhesive (polyol compound and aromatic isocyanate compound, thickness after curing is 3 μm), and a substrate layer 1 including a laminated film formed by laminating the first substrate layer 11 and the second substrate layer 12 through an adhesive layer was obtained. Next, the obtained substrate layer 1 and an aluminum foil (JIS H4160: 1994A8021H-O, thickness 40 μm) with a corrosion-resistant protective film formed on both surfaces as a barrier layer 3 were prepared. Next, the barrier layer and the ONy film side of the substrate layer were laminated by dry lamination using a two-component curing polyurethane adhesive (polyol compound and aromatic isocyanate compound), and then an aging treatment was performed to prepare a laminate of substrate layer (first substrate layer / adhesive layer / second substrate layer) / adhesive layer (thickness after curing is 3 μm) / barrier layer (thickness 40 μm).

[0274] Next, maleic anhydride-modified polypropylene (PPa, thickness 40 μm) as a bonding layer and polypropylene (PP, thickness 40 μm) as a heat-fusible resin layer were co-extruded on the barrier layer of the laminated body obtained above, thereby laminating the bonding layer / heat-fusible resin layer on the barrier layer. Next, the laminated body obtained was subjected to aging treatment and heated to obtain an outer packaging material for a storage battery device having a base material layer (PET / adhesive layer / ONy) / adhesive layer (thickness 3 μm) / barrier layer (thickness 40 μm) / adhesive layer (thickness 40 μm) / heat-fusible resin layer (thickness 40 μm) laminated in this order.

[0275] In each of the Examples and Comparative Examples, erucamide was applied as a lubricant on the outer surface of the base material layer of the packaging material for a power storage device.

[0276] <Evaluation of Formability>

[0277] The outer packaging material for the power storage device was cut into a rectangular shape with a length (MD (Machine Direction)) of 90 mm and a width (TD (Transverse Direction)) of 150 mm to prepare a test sample. The test sample was cold-formed (single-stage pultrusion) using a rectangular forming die having a diameter of 31.6 mm (MD direction) × 54.5 mm (TD direction) (a female die, the surface of which has a maximum height roughness (Rz nominal value) of 3.2 μm, R of chamfers of 2.0 mm, and R of ridges of 1.0 mm as specified in Table 2 of the comparative surface roughness standard sheet of JIS B 0659-1: 2002 Annex 1 (reference)) and a matching forming die (a male die, the surface of which has a maximum height roughness (Rz nominal value) of 1.6 μm, R of chamfers of 2.0 mm, and R of ridges of 1.0 mm as specified in Table 2 of the comparative surface roughness standard sheet of JIS B 0659-1: 2002 Annex 1 (reference)), under a pressing pressure (surface pressure) of 0.25 MPa, and the forming depth was changed from a forming depth of 0.5 mm in units of 0.5 mm, and each of 10 test samples was subjected to cold forming (single-stage pultrusion). At this time, the test sample is placed on the die so that the heat-fusible resin layer side is located on the convex side for molding. In addition, the gap between the convex and the concave is set to 0.3mm. Molding is carried out at 25°C. In a dark room, a flashlight is used to illuminate the test sample after cold forming, and whether the aluminum alloy foil has pinholes or cracks is confirmed by whether it is light-transmitting. The deepest molding depth in which no pinholes or cracks appear in the 10 test samples of the aluminum alloy foil is set to Amm, and the number of test samples in which pinholes, etc. appear in the shallowest molding depth in which pinholes, etc. appear in the aluminum alloy foil is set to B. The value calculated according to the following formula is rounded to two decimal places as the limit molding depth of the outer packaging material for the storage device. The judgment was made according to the following four-level depth standards. The results are shown in Table 5.

[0278] Limit forming depth = Amm + (0.5mm / 10 pieces) × (10 pieces - B pieces)

[0279] (Moldability Evaluation Criteria)

[0280] S: The maximum forming depth is 9.0 mm or more

[0281] A: The ultimate forming depth is 8.5 mm or more and less than 9.0 mm

[0282] B: The ultimate forming depth is 8.0 mm or more and less than 8.5 mm

[0283] C: The ultimate forming depth is 7.5 mm or more and less than 8.0 mm

[0284] D: The ultimate forming depth is less than 7.5mm

[0285] [Table 1]

[0286]

[0287] [Table 2]

[0288]

[0289] [Table 3]

[0290]

[0291] In Table 3, “-” means not measured.

[0292] [Table 4]

[0293]

[0294] [Table 5]

[0295]

[0296] As described above, the present invention provides the following aspects of the invention.

[0297] Item 1: An outer packaging material for an electric storage device, comprising a laminate having at least a base layer, a barrier layer and a heat-fusible resin layer in this order,

[0298] The above-mentioned substrate layer is composed of more than two layers, and the above-mentioned substrate layer includes more than one layer of polyester film. The work hardening index of the above-mentioned substrate layer in the length direction and the width direction is greater than 2.5 and less than 4.5, and the difference between the work hardening index in the length direction and the width direction is less than 1.4.

[0299] Item 2: The outer packaging material for an electric storage device according to Item 1, wherein the intrinsic viscosity of the polyester film is 0.66 dl / g or more and 1.00 dl / g or less.

[0300] Item 3: The outer packaging material for a storage battery device according to Item 1 or Item 2, wherein the amount of a rigid amorphous component in the resin film is 5% to 60%.

[0301] Item 4: The packaging material for an electric storage device according to any one of Items 1 to 3, wherein the polyester film has a thickness of 5 μm or more and 40 μm or less.

[0302] Item 5: The packaging material for an electric storage device according to any one of Items 1 to 4, wherein the polyester film has a melting point of 235° C. or higher.

[0303] Item 6: The packaging material for a power storage device according to any one of Items 1 to 5, wherein the polyester film has a crystallinity of 15% or more and 40% or less.

[0304] Item 7: The packaging material for a power storage device according to any one of Items 1 to 6, wherein the tensile elongation at break in at least one of the longitudinal direction and the width direction of the base layer is 80% or more.

[0305] Item 8: An electricity storage device, wherein an electricity storage device element including at least a positive electrode, a negative electrode, and an electrolyte is housed in a packaging body formed of the electricity storage device packaging material according to any one of Items 1 to 7.

[0306] Item 9: A method for producing an outer packaging material for a storage device, comprising the step of laminating at least a base layer, a barrier layer and a heat-fusible resin layer in this order to obtain a laminate.

[0307] The above-mentioned substrate layer is composed of more than two layers, and the above-mentioned substrate layer includes more than one layer of polyester film. The work hardening index of the above-mentioned substrate layer in the length direction and the width direction is greater than 2.5 and less than 4.5, and the difference between the work hardening index in the length direction and the width direction is less than 1.4.

[0308] Explanation of symbols

[0309] 1. Base material layer

[0310] 2. Adhesive layer

[0311] 3. Barrier layer

[0312] 4. Thermally fusible resin layer

[0313] 5. Bonding layer

[0314] 6. Surface covering layer

[0315] 10. Outer packaging materials for power storage devices

Claims

1. An outer packaging material for an electric storage device, It is characterized in that The invention is composed of a laminated body which at least comprises a base material layer, a barrier layer and a heat-fusible resin layer in this order, The substrate layer is composed of two or more layers. The substrate layer comprises one or more polyester films, The work hardening index of the substrate layer in the length direction and the width direction are both greater than 2.5 and less than 4.5, and the difference between the work hardening index in the length direction and the work hardening index in the width direction is less than 1.

4.

2. The outer packaging material for an electric storage device according to claim 1, It is characterized in that The polyester film has an intrinsic viscosity of 0.66 dl / g or more and 1.00 dl / g or less.

3. The outer packaging material for an electric storage device according to claim 1 or 2, It is characterized in that The rigid amorphous component content of the resin film is greater than 5% and less than 60%.

4. The outer packaging material for an electric storage device according to claim 1 or 2, It is characterized in that The polyester film has a thickness of 5 μm or more and 40 μm or less.

5. The outer packaging material for an electric storage device according to claim 1 or 2, It is characterized in that The melting point of the polyester film is 235° C. or higher.

6. The outer packaging material for an electric storage device according to claim 1 or 2, It is characterized in that The polyester film has a crystallinity of 15% or more and 40% or less.

7. The outer packaging material for an electric storage device according to claim 1 or 2, It is characterized in that The tensile elongation at break of the substrate layer in at least one of the longitudinal direction and the width direction is greater than 80%.

8. An electric storage device, It is characterized in that An electric storage device element including at least a positive electrode, a negative electrode and an electrolyte is housed in a packaging body formed of the outer packaging material for an electric storage device according to claim 1 or 2.

9. A method for manufacturing an outer packaging material for an electric storage device, It is characterized in that The method comprises the steps of laminating at least a substrate layer, a barrier layer and a heat-fusible resin layer in this order to obtain a laminate. The substrate layer is composed of two or more layers, and the substrate layer includes one or more polyester films. The work hardening index of the substrate layer in the length direction and the width direction are both greater than 2.5 and less than 4.5, and the difference between the work hardening index in the length direction and the work hardening index in the width direction is less than 1.4.

Citation Information

Patent Citations

  • Layered package material, outer package material for battery, and the battery

    JP2008287971A