Dentin hypersensitivity resistant mineralizing liquid as well as preparation method and application thereof
By using organic solvents such as glycerol and polyethylene glycol in dentin-sensitive mineralized liquid, combining phosphate and strontium ions to form stable ion clusters, the problem that mineralized materials are difficult to penetrate dentin is solved, and long-term effect is achieved Dentin tubular closure and nerve conduction passivation significantly improve the therapeutic effect of anti-dentin sensitivity.
Patent Information
- Application Number
- CN202411114013.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-14
AI Technical Summary
In the existing dentin-sensitive treatment methods, calcium phosphate minerals produced by mineralized materials are difficult to penetrate deep into the dentin, making it difficult to maintain the sealing effect for a long time, and the anti-dentin sensitivity effect is limited.
Provide an anti-dentin sensitive mineralization solution containing organic solvents (such as glycerol and polyethylene glycol), phosphorus and strontium sources. By mixing the solution, stable phosphate and strontium ion clusters can be effectively diffused to dentin tubes. Internally, combined with the idea of passivating nerve conduction, long-term dentin closure is achieved.
The mineralized liquid can maintain stability and form dense minerals in dentin tubules without the need for preservatives, significantly improve the sealing effect of dentin tubules, reduce dentin tubules, and provide antibacterial properties.
Smart Images

Figure CN119015133A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of oral care, and in particular to an anti-dentin sensitivity mineralizing liquid and a preparation method and application thereof. Background Art
[0002] Dentin hypersensitivity (DH) refers to the short-term, sharp pain or discomfort that occurs when exposed dentin is stimulated by mechanical, chemical, temperature, and osmotic pressure due to various reasons, and cannot be classified as other types of dental diseases. Dentin hypersensitivity is a common oral symptom that troubles a large number of people and affects the quality of life of patients to varying degrees. In the case of enamel corrosion, gingival recession, and tooth defects, dentin can be directly exposed to the oral environment; when stimulated by heat, cold, touch, osmosis, or chemicals, the movement of fluid in the dentinal tubules produces stimulation that is transmitted to the nerves, causing patients to experience sharp pain. Therefore, the treatment of dentin hypersensitivity is generally based on two strategies: (1) blunting the nerve conduction of external stimuli; (2) using dentinal tubule occlusion to block the exposed dentinal tubules. The materials used in the former are mainly soluble substances, but the anti-sensitivity effect they produce is difficult to sustain; the materials used in the latter are mainly mineralized materials, which produce substances similar to the inorganic components of teeth on the dentin after use - calcium phosphate directly seals the dentinal tubules. However, the calcium phosphate minerals produced by most mineralized materials only exist on the surface of the dentin and are difficult to penetrate into the dentin, making it difficult to maintain the sealing effect for a long time, and the anti-dentin sensitivity effect is limited. Summary of the invention
[0003] The purpose of the present invention is to provide an anti-dentin sensitivity mineralization liquid and its preparation method and application to solve the problems existing in the above-mentioned prior art. After coating the dentin surface, the anti-dentin sensitivity mineralization liquid provided by the present invention can effectively diffuse into the inside of the dentinal tubules, and finally achieve the purpose of anti-dentin sensitivity.
[0004] To achieve the above object, the present invention provides the following solutions:
[0005] The present invention provides an anti-dentin sensitivity mineralization solution, which comprises an organic solvent, a phosphorus source, a calcium source and a strontium source;
[0006] The concentration of phosphorus in the anti-dentin sensitivity mineralization solution is ≤125mmol / L, the concentration of calcium is ≤100mmol / L, and the concentration of strontium is ≤25mmol / L.
[0007] Preferably, the organic solvent comprises glycerol and polyethylene glycol;
[0008] The average molecular weight of the polyethylene glycol is 200-700Da;
[0009] The volume ratio of the glycerol to the polyethylene glycol is (1-9): (9-1).
[0010] Preferably, the phosphorus source comprises phosphate and polyphosphate; the molar ratio of the phosphate to the polyphosphate is (1-50):1, calculated on the basis of phosphorus element;
[0011] The calcium source is calcium chloride and / or calcium nitrate;
[0012] The strontium source is strontium chloride and / or strontium nitrate.
[0013] Preferably, the phosphate is one or more of sodium hydrogen phosphate, sodium dihydrogen phosphate, sodium phosphate, potassium hydrogen phosphate, potassium dihydrogen phosphate, potassium phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate and ammonium phosphate; the polyphosphate is one or more of sodium polyphosphate, potassium polyphosphate and ammonium polyphosphate.
[0014] The present invention provides a method for preparing the above-mentioned anti-dentin sensitivity mineralizing solution, comprising the following steps:
[0015] Mixing 1 / 2 volume of an organic solvent and a phosphorus source to fully dissolve the organic solvent and obtain a phosphorus-containing solution; the concentration of phosphorus in the phosphorus-containing solution is ≤250 mmol / L;
[0016] Mix the remaining 1 / 2 volume of the organic solvent, the calcium source and the strontium source to fully dissolve them, thereby obtaining a solution containing calcium and strontium; the concentration of the calcium element in the solution containing calcium and strontium is ≤200mmol / L, and the concentration of the strontium element is ≤50mmol / L;
[0017] The phosphorus-containing solution is mixed with solutions containing calcium and strontium to obtain the anti-dentin sensitivity mineralization solution.
[0018] Preferably, the organic solvent comprises glycerol and polyethylene glycol;
[0019] The average molecular weight of the polyethylene glycol is 200-700Da;
[0020] The volume ratio of the glycerol to the polyethylene glycol is (1-9): (9-1).
[0021] Preferably, the phosphorus source comprises phosphate and polyphosphate; the molar ratio of the phosphate to the polyphosphate is (1-50):1, calculated on the basis of phosphorus element;
[0022] The calcium source is calcium chloride and / or calcium nitrate;
[0023] The strontium source is strontium chloride and / or strontium nitrate.
[0024] Preferably, the phosphate is one or more of sodium hydrogen phosphate, sodium dihydrogen phosphate, sodium phosphate, potassium hydrogen phosphate, potassium dihydrogen phosphate, potassium phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate and ammonium phosphate; the polyphosphate is one or more of sodium polyphosphate, potassium polyphosphate and ammonium polyphosphate.
[0025] The present invention provides the use of the above-mentioned anti-dentin sensitivity mineralization liquid in the preparation of anti-dentin sensitivity products and / or oral remineralization products.
[0026] The present invention provides an anti-dentin sensitivity product and / or an oral remineralization product, the active ingredients of which include the anti-dentin sensitivity mineralization liquid.
[0027] The present invention discloses the following technical effects:
[0028] The present invention proposes a biocompatible organic anti-dentin sensitivity mineralizing liquid. The present invention combines the idea of passivating nerve conduction on the basis of improving the effect of mineralizing materials in sealing dentinal tubules to achieve the therapeutic effect of improving anti-dentin sensitivity (anti-dentin sensitivity). The present invention uses two biocompatible organic solvents, glycerol and polyethylene glycol (average molecular weight between 200-700Da) as solvents, calcium ions and strontium ions as main cations, and phosphate and polyphosphate as main anions, to prepare an organic anti-dentin sensitivity mineralizing liquid, and the reagents used are highly biocompatible. In the anti-dentin sensitivity mineralizing liquid, the cations and anions are partially present in the form of free ions, and the rest are present in the form of ion clusters, and the size of the ion clusters is ≤5nm. The anti-dentin sensitivity mineralizing liquid can stably maintain the state of ions and ion clusters for more than 1 month in a sealed environment of ≤45°C without generating particles with an average size >5nm, and does not decay or deteriorate without adding an anticorrosive agent.
[0029] The anti-dentin sensitivity mineralizing liquid prepared by the present invention, on the one hand, can ensure that it can effectively diffuse into the inside of the dentinal tubules after being coated on the surface of the dentin based on the ultra-small size of the ions and ion clusters in the anti-dentin sensitivity mineralizing liquid and the fluidity of the mineralizing liquid; on the other hand, when the anti-dentin sensitivity mineralizing liquid contacts saliva or body fluids, it will produce biocompatible minerals-polyphosphate-stabilized strontium-containing calcium phosphate, which can block the exposed dentinal tubules; and the introduced strontium ions can passivate the nerve conduction of external stimulation to alleviate the symptoms of tooth sensitivity; polyphosphate can also provide certain antibacterial properties. It can be seen that the anti-dentin sensitivity mineralizing liquid provided by the present invention can effectively prevent and treat dentin hypersensitivity.
[0030] The various components used in the present invention do not produce only a single effect, but after producing a synergistic effect with other components, the purpose of controlling the state, stability, mineralization performance, and use effect of the product is finally achieved. Since general materials will stimulate the oral cavity to produce a large amount of saliva instantly when applied to the tooth surface, the material may be quickly transformed into larger particles before penetrating into the dentinal tubules, thereby failing to penetrate into the dentinal tubules. The strontium ions and polyphosphates of the present invention can control the morphology and phase conversion rate of the anti-dentin sensitivity mineralizing liquid when it contacts saliva or body fluids together with polyethylene glycol, so as to reduce or avoid mineralization before it enters the dentinal tubules; in addition, the polyethylene glycol used in the present invention is not only a biocompatible solvent, but also can inhibit the aggregation of particles formed after contacting saliva or body fluids, and slow down the growth of their size. All of the above characteristics are conducive to the penetration of the material into the dentinal tubules.
[0031] The present invention also provides a method for preparing an anti-dentin sensitivity mineralizing liquid. The method is simple and convenient, does not require additional solutions, can reduce the types and amounts of raw materials, and greatly reduce production costs. Moreover, the raw materials used in the preparation of the anti-dentin sensitivity mineralizing liquid are water-soluble phosphates, water-soluble calcium salts, water-soluble strontium sources, and polyethylene glycol and glycerol solutions, without the involvement of other toxic substances. Therefore, the preparation process and the prepared product are non-toxic.
[0032] In summary, the present invention combines the two ideas of sealing dentinal tubules and blunting nerve conduction for the purpose of anti-tooth sensitivity, and cleverly combines the two in a liquid mineralized material based on an organic solvent; by stabilizing calcium, phosphate ions and ultra-small nanoparticles, the sealing effect of dentinal tubules is significantly improved; and the introduced ingredients have high stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 This is a scanning electron microscope image of a dentin cross section after the anti-dentin sensitivity mineralization solution prepared in Comparative Example 1 is applied to the dentin surface after acid etching;
[0035] Figure 2 This is a scanning electron microscope image of a dentin cross section after the anti-dentin sensitivity mineralization solution prepared in Comparative Example 2 is applied to the dentin surface after acid etching;
[0036] Figure 3This is a scanning electron microscope image of a dentin cross section after the anti-dentin sensitivity mineralizing solution prepared in Example 2 is applied to the dentin surface after acid etching; wherein A is a scanning electron microscope image of a dentin cross section at a scale of 10 μm, and B is a scanning electron microscope image of a dentin cross section at a scale of 2 μm;
[0037] Figure 4 The stability observation results of the anti-dentin sensitivity mineralization solutions prepared in Comparative Example 1 (A) and Example 2 (B);
[0038] Figure 5 This is an in-situ transmission electron microscopy image of the anti-dentin sensitivity mineralization solution prepared in Example 2. DETAILED DESCRIPTION
[0039] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0040] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0041] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0042] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0043] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0044] Example 1 Preparation of anti-dentin sensitivity mineralization solution
[0045] Mix 90 mL of glycerol with 10 mL of polyethylene glycol to obtain a mixed solvent, wherein the average molecular weight of the polyethylene glycol is 200 Da;
[0046] Utilize 1 / 2 of the mixed solvent to dissolve trisodium phosphate and sodium polyphosphate (molecular weight 1000Da), the amount of trisodium phosphate added is such that the concentration of phosphorus in the mixed solution is 240mmol / L, and the amount of sodium polyphosphate added is such that the concentration of phosphorus in the mixed solution is 10mol / L; the molar ratio of trisodium phosphate to sodium polyphosphate is 24:1 in terms of phosphorus;
[0047] The remaining 1 / 2 of the mixed solvent is used to dissolve calcium chloride and strontium chloride, so that the concentration of calcium element is 200 mmol / L and the concentration of strontium element is 50 mmol / L;
[0048] The two solutions are mixed to form an anti-dentin sensitivity mineralization solution, in which the concentration of phosphorus is 125 mol / L, the concentration of calcium is 100 mol / L, and the concentration of strontium is 25 mol / L.
[0049] Example 2 Preparation of anti-dentin sensitivity mineralization solution
[0050] Mix 50 mL of glycerol and 50 mL of polyethylene glycol to obtain a mixed solvent, wherein the average molecular weight of the polyethylene glycol is 500 Da;
[0051] Utilize 1 / 2 of the mixed solvent to dissolve trisodium phosphate and sodium polyphosphate (molecular weight 5000Da), the amount of trisodium phosphate added is such that the concentration of phosphorus in the mixed solution is 100mmol / L, and the amount of sodium polyphosphate added is such that the concentration of phosphorus in the mixed solution is 50mol / L; the molar ratio of trisodium phosphate to sodium polyphosphate is 2:1 in terms of phosphorus;
[0052] The remaining 1 / 2 of the mixed solvent is used to dissolve calcium chloride and strontium chloride, so that the concentration of calcium element is 120mmol / L and the concentration of strontium element is 20mmol / L;
[0053] The two solutions are mixed to form an anti-dentin sensitivity mineralization solution, in which the concentration of phosphorus is 75 mmol / L, the concentration of calcium is 60 mmol / L, and the concentration of strontium is 10 mmol / L.
[0054] Example 3 Preparation of anti-dentin sensitivity mineralization solution
[0055] Mix 10 mL of glycerol and 90 mL of polyethylene glycol to obtain a mixed solvent, wherein the average molecular weight of the polyethylene glycol is 700 Da;
[0056] Utilize 1 / 2 of the mixed solvent to dissolve trisodium phosphate and sodium polyphosphate (molecular weight 10000Da), the amount of trisodium phosphate added is such that the concentration of phosphorus in the mixed solution is 40mmol / L, and the amount of sodium polyphosphate added is such that the concentration of phosphorus in the mixed solution is 10mol / L; the molar ratio of trisodium phosphate to sodium polyphosphate is 4:1 in terms of phosphorus;
[0057] The remaining 1 / 2 of the mixed solvent is used to dissolve calcium chloride and strontium chloride, so that the concentration of calcium element is 140mmol / L and the concentration of strontium element is 10mmol / L;
[0058] The two solutions are mixed to form an anti-dentin sensitivity mineralization solution, in which the concentration of phosphorus is 25 mmol / L, the concentration of calcium is 70 mmol / L, and the concentration of strontium is 5 mmol / L.
[0059] Example 4 Preparation of anti-dentin sensitivity mineralization solution
[0060] Mix 90 mL of glycerol and 10 mL of polyethylene glycol to obtain a mixed solvent, wherein the average molecular weight of the polyethylene glycol is 200 Da;
[0061] Utilize 1 / 2 of the mixed solvent to dissolve trisodium phosphate and sodium polyphosphate (molecular weight 50000Da), the amount of trisodium phosphate added is such that the concentration of phosphorus in the mixed solution is 120mmol / L, and the amount of sodium polyphosphate added is such that the concentration of phosphorus in the mixed solution is 100mol / L; the molar ratio of trisodium phosphate to sodium polyphosphate is 1.2:1 in terms of phosphorus;
[0062] The remaining 1 / 2 of the mixed solvent is used to dissolve calcium chloride and strontium chloride, so that the concentration of calcium element is 40mmol / L and the concentration of strontium element is 10mmol / L;
[0063] The two solutions are mixed to form an anti-dentin sensitivity mineralization solution, in which the concentration of phosphorus is 110 mmol / L, the concentration of calcium is 20 mmol / L, and the concentration of strontium is 5 mmol / L.
[0064] Example 5 Preparation of anti-dentin sensitivity mineralization solution
[0065] Mix 50 mL of glycerol and 50 mL of polyethylene glycol to obtain a mixed solvent, wherein the average molecular weight of the polyethylene glycol is 500 Da;
[0066] Utilize 1 / 2 of the mixed solvent to dissolve trisodium phosphate and sodium polyphosphate (molecular weight 100000Da), the amount of trisodium phosphate added is such that the concentration of phosphorus in the mixed solution is 140mmol / L, and the amount of sodium polyphosphate added is such that the concentration of phosphorus in the mixed solution is 10mol / L; the molar ratio of trisodium phosphate to sodium polyphosphate is 14:1 in terms of phosphorus;
[0067] The remaining 1 / 2 of the mixed solvent is used to dissolve calcium chloride and strontium chloride, so that the concentration of calcium element is 14 mmol / L and the concentration of strontium element is 5 mmol / L;
[0068] The two solutions are mixed to form an anti-dentin sensitivity mineralization solution, in which the concentration of phosphorus is 75 mmol / L, the concentration of calcium is 7 mmol / L, and the concentration of strontium is 2.5 mmol / L.
[0069] Example 6 Preparation of anti-dentin sensitivity mineralization solution
[0070] Mix 10 mL of glycerol and 90 mL of polyethylene glycol to obtain a mixed solvent, wherein the average molecular weight of the polyethylene glycol is 700 Da;
[0071] Utilize 1 / 2 of the mixed solvent to dissolve trisodium phosphate and sodium polyphosphate (molecular weight 500000Da), the amount of trisodium phosphate added is such that the concentration of phosphorus in the mixed solution is 30mmol / L, and the amount of sodium polyphosphate added is such that the concentration of phosphorus in the mixed solution is 20mol / L; the molar ratio of trisodium phosphate to sodium polyphosphate is 1.5:1 in terms of phosphorus;
[0072] The remaining 1 / 2 of the mixed solvent is used to dissolve calcium chloride and strontium chloride, so that the concentration of calcium element is 200 mmol / L and the concentration of strontium element is 40 mmol / L;
[0073] The two solutions are mixed to form an anti-dentin sensitivity mineralization solution, in which the concentration of phosphorus is 25 mmol / L, the concentration of calcium is 100 mmol / L, and the concentration of strontium is 20 mmol / L.
[0074] Comparative Example 1
[0075] Prepare 100 mL of glycerol solvent;
[0076] Dissolve trisodium phosphate in 1 / 2 glycerol solvent to a concentration of 150 mmol / L, and add sodium polyphosphate in an amount such that the concentration of phosphorus in the mixed solution is 50 mol / L;
[0077] Use the remaining 1 / 2 of the mixed solvent to dissolve calcium chloride to a concentration of 140 mmol / L;
[0078] The two solutions are mixed to form an anti-dentin sensitivity mineralization solution, in which the concentration of phosphorus is 75 mmol / L and the concentration of calcium is 70 mmol / L.
[0079] Comparative Example 2
[0080] Mix 50 mL of glycerol and 50 mL of polyethylene glycol to obtain a mixed solvent, wherein the average molecular weight of the polyethylene glycol is 500 Da;
[0081] Dissolve trisodium phosphate and sodium polyphosphate (molecular weight 5000Da) in 1 / 2 of a mixed solvent, wherein the amount of trisodium phosphate added is such that the concentration of phosphorus in the mixed solution is 150 mmol / L, and no polyphosphate is added;
[0082] The remaining 1 / 2 of the mixed solvent is used to dissolve calcium chloride and strontium chloride, so that the concentration of calcium element is 120mmol / L and the concentration of strontium element is 20mmol / L;
[0083] The two solutions are mixed to form an anti-dentin sensitivity mineralization solution, in which the concentration of phosphorus is 75 mmol / L, the concentration of calcium is 60 mmol / L, and the concentration of strontium is 10 mmol / L.
[0084] Experimental Example 1
[0085] The anti-dentin sensitivity mineralization solution prepared in Example 2 and Comparative Example 1-2 was subjected to a dentin tubule blocking experiment, and the specific steps were as follows:
[0086] Dentin slices 1 mm above the pulp chamber of the tooth crown were cut, soaked in 10% ethylenediaminetetraacetic acid solution for 5 min, ultrasonicated for 10 min, and washed with deionized water to obtain dentin samples with exposed tubules.
[0087] The anti-dentin sensitivity mineralization liquid prepared in Example 2 and Comparative Example 1-2 was applied to the surface of the dentine after acid etching, and then the dentine sample to be repaired was immersed in simulated saliva and placed in a constant temperature oven at 37°C for 24 hours before being taken out; rinsed under running water for 1 minute and then dried, and then observed under an electron microscope. The results are as follows Figure 1-Figure 3 As shown, after the samples treated with the anti-dentin sensitivity mineralization liquid prepared in Comparative Examples 1 and 2 were treated, although the surface was covered with a layer of mineralized material, no material penetrated into the dentin tubules ( Figure 1 and Figure 2 ); however, the dentin treated with the prepared anti-dentin sensitivity mineralizing solution produced dense mineralization on the surface and inside, thus achieving a good dentinal tubule sealing effect ( Figure 3). At the same time, the blocking rate was calculated according to whether the material entered the dentinal tubules. The results showed that the blocking rate of Example 2 was 90% after treatment, and the blocking rates of Comparative Examples 1 and 2 were less than 10%.
[0088] Experimental Example 2
[0089] The stability of the anti-dentin sensitivity mineralization solution prepared in Example 2 and Comparative Example 1 was observed. Specifically, the anti-dentin sensitivity mineralization solution prepared in Example 2 and Comparative Example 1 was mixed with water at a volume ratio of 1:10, and allowed to stand to observe the clarity, stability, and whether there was precipitation. Figure 4 As shown, the anti-dentin sensitivity mineralization solution prepared in Comparative Example 1 becomes turbid after being mixed with water. After standing for 10 minutes, obvious precipitation occurs. It can be seen that the anti-dentin sensitivity mineralization solution prepared in Comparative Example 1 is not stable ( Figure 4 A), the anti-dentin sensitivity mineralization solution prepared in Example 2 will also become turbid after mixing with water. After standing for 10 minutes, there is no obvious precipitation. It can be seen that the anti-dentin sensitivity mineralization solution prepared in Example 2 has a high stability ( Figure 4 B).
[0090] Experimental Example 3
[0091] The anti-dentin sensitivity mineralization solution prepared in Example 2 was observed by in-situ liquid transmission electron microscopy. Figure 5 As shown, the size of the ion clusters is ≤5 nm.
[0092] Experimental Example 4
[0093] The storage time and product quality of the anti-dentin sensitivity mineralizing liquid prepared in Example 2 were investigated. The results showed that the anti-dentin sensitivity mineralizing liquid prepared in Example 2 could stably maintain the ion and ion cluster state for more than 1 month in a sealed environment of ≤45°C without producing particles with an average size of >5nm, and would not corrode or deteriorate without the addition of anti-corrosion agents.
[0094] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A mineralizing solution for resisting dentin sensitivity, It is characterized in that The anti-dentin sensitivity mineralization solution comprises an organic solvent, a phosphorus source, a calcium source and a strontium source; The concentration of phosphorus in the anti-dentin sensitivity mineralization solution is ≤125mmol / L, the concentration of calcium is ≤100mmol / L, and the concentration of strontium is ≤25mmol / L.
2. The anti-dentin sensitivity mineralizing solution according to claim 1, It is characterized in that The organic solvent includes glycerol and polyethylene glycol; The average molecular weight of the polyethylene glycol is 200-700Da; The volume ratio of the glycerol to the polyethylene glycol is (1-9): (9-1).
3. The anti-dentin sensitivity mineralizing solution according to claim 1, It is characterized in that The phosphorus source includes phosphate and polyphosphate; the molar ratio of the phosphate to the polyphosphate is (1-50):1 based on phosphorus element; The calcium source is calcium chloride and / or calcium nitrate; The strontium source is strontium chloride and / or strontium nitrate.
4. The anti-dentin sensitivity mineralizing solution according to claim 3, It is characterized in that The phosphate is one or more of sodium hydrogen phosphate, sodium dihydrogen phosphate, sodium phosphate, potassium hydrogen phosphate, potassium dihydrogen phosphate, potassium phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate and ammonium phosphate; the polyphosphate is one or more of sodium polyphosphate, potassium polyphosphate and ammonium polyphosphate.
5. The method for preparing the anti-dentin sensitivity mineralizing solution according to claim 1, It is characterized in that The following steps are involved: Mixing 1 / 2 volume of an organic solvent and a phosphorus source to fully dissolve the organic solvent and obtain a phosphorus-containing solution; the concentration of phosphorus in the phosphorus-containing solution is ≤250 mmol / L; Mix the remaining 1 / 2 volume of the organic solvent, the calcium source and the strontium source to fully dissolve them, thereby obtaining a solution containing calcium and strontium; the concentration of the calcium element in the solution containing calcium and strontium is ≤200mmol / L, and the concentration of the strontium element is ≤50mmol / L; The phosphorus-containing solution is mixed with solutions containing calcium and strontium to obtain the anti-dentin sensitivity mineralization solution.
6. The preparation method according to claim 5, It is characterized in that The organic solvent includes glycerol and polyethylene glycol; The average molecular weight of the polyethylene glycol is 200-700Da; The volume ratio of the glycerol to the polyethylene glycol is (1-9): (9-1).
7. The preparation method according to claim 5, It is characterized in that The phosphorus source includes phosphate and polyphosphate; the molar ratio of the phosphate to the polyphosphate is (1-50):1 based on phosphorus element; The calcium source is calcium chloride and / or calcium nitrate; The strontium source is strontium chloride and / or strontium nitrate.
8. The preparation method according to claim 5, It is characterized in that The phosphate is one or more of sodium hydrogen phosphate, sodium dihydrogen phosphate, sodium phosphate, potassium hydrogen phosphate, potassium dihydrogen phosphate, potassium phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate and ammonium phosphate; the polyphosphate is one or more of sodium polyphosphate, potassium polyphosphate and ammonium polyphosphate.
9. Use of the anti-dentin sensitivity mineralization solution according to any one of claims 1 to 4 in the preparation of an anti-dentin sensitivity product and / or an oral remineralization product.
10. An anti-dentin sensitivity product and / or an oral remineralization product, It is characterized in that The effective ingredients include the anti-dentin sensitivity mineralization solution according to any one of claims 1-4.
Citation Information
Patent Citations
Tooth sensitivity resisting composition containing strontium salt
CN109966314A
Oral care composition capable of enhancing effect, application of oral care composition and oral care product containing oral care composition
CN115778838A
Method for constructing biomimetic mineralization enamel of biomimetic mineralization leading edge by instantly mixing calcium ion source and phosphorus ion source