Carbon dioxide separation membrane and preparation method thereof
The organic salts prepared by reacting organic acids and organic bases combine with polymers to form a high-performance carbon dioxide separation membrane, which solves the problems of insufficient performance of membrane materials, complexity of absorption methods and pollution in the prior art, and achieves high efficiency and stability carbon dioxide separation effect.
Patent Information
- Application Number
- CN202310590557.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-24
AI Technical Summary
Among the existing carbon dioxide capture technology, the membrane material performance of the membrane separation method is not high enough, resulting in limited large-scale applications. The absorption method has complexity and secondary pollution problems, making it difficult to effectively separate carbon dioxide.
The organic salt produced by the reaction of organic acid and organic base is used as the carbon dioxide support, and a high-performance carbon dioxide separation membrane is formed by combining the polymer, and high permeability rate and selectivity are achieved through the loading and release mechanism of the organic salt.
It achieves efficient carbon dioxide separation, improves the selectivity and permeability of the membrane, avoids secondary pollution, and has high stability in the preparation process and low cost.
Smart Images

Figure BDA0004245342930000031 
Figure BDA0004245342930000101 
Figure BDA0004245342930000111
Abstract
Description
Technical Field
[0001] The invention relates to membrane separation, in particular to a separation membrane for separating carbon dioxide. Background Art
[0002] In order to cope with the serious environmental problem of global warming, greenhouse gas emissions from power plants and energy-intensive industries (such as cement, steel and steel mills) should be reduced. Due to the important role of fossil energy in industrial development, relying solely on the development of clean energy is not enough to achieve zero carbon dioxide emissions within a given time. Carbon dioxide capture, utilization and storage technology (CCUS) is currently the "bottom line" technology for achieving low-carbon utilization of fossil energy. Carbon dioxide capture technology can be divided into three processes: post-combustion capture, pre-combustion capture and oxygen-enriched combustion capture. Among them, post-combustion carbon dioxide capture is considered to be a feasible solution suitable for existing plants.
[0003] The absorption method refers to the process in which the absorbent selectively absorbs the gas in the mixed components according to its own properties. It is also the most widely used method for separating carbon dioxide. However, the absorption method also has many disadvantages, such as the absorption process is relatively complicated, the absorption efficiency is not particularly stable, and the absorption liquid regeneration process is also prone to secondary pollution. In comparison, the membrane separation method captures carbon dioxide without phase change and secondary pollution. The gas membrane separation method has become one of the most watched carbon dioxide capture technologies due to its low cost, simple equipment, low operating cost, high efficiency and greenness.
[0004] The core of gas membrane separation technology is gas separation membrane, and the core of membrane lies in the selection of membrane material, which has a significant impact on the entire separation process. The selection of gas separation membrane material should take into account both its permeability and selectivity. Facilitated transfer membrane is a type of membrane that contains functional groups or structural units that can undergo reversible chemical reactions with target components to enhance the transfer of target components in the membrane. It can overcome the limitations of permeability and selectivity that are common in ordinary polymer membranes, and thus simultaneously achieve high permeability and high selectivity of separation membranes. Therefore, facilitated transfer membrane is considered to be a type of separation membrane with great development potential. However, gas membrane separation technology has not yet been widely used, mainly because the performance of membrane materials is not high enough and the performance of membrane materials prepared on a large scale is not stable enough. It can be seen that the development of high-performance carbon dioxide capture membrane materials and the preparation of membranes with stable performance are of great significance to achieving the dual carbon goals. Summary of the invention
[0005] In order to overcome at least one defect of the above-mentioned prior art, in the first aspect, an embodiment of the present invention provides a composition for forming a carbon dioxide separation membrane, comprising a polymer and an organic salt; the organic salt is prepared by reacting an organic acid with an organic base; the organic acid comprises a basic group and an acidic group, the basic group comprises an amino group and / or an imino group, and the acidic group comprises one or more of a carboxylic acid group, a phosphoric acid group, a sulfuric acid group, and a sulfonic acid group; the organic base comprises one or more of guanidine and its derivatives, and piperazine and its derivatives.
[0006] In a second aspect, an embodiment of the present invention provides a carbon dioxide separation membrane, comprising a polymer layer, wherein the raw material for preparing the polymer layer comprises the above-mentioned composition.
[0007] In a third aspect, an embodiment of the present invention provides a method for preparing the above-mentioned carbon dioxide separation membrane, comprising the following steps:
[0008] Providing a mixed solution, the mixed solution comprising the composition and a solvent; and
[0009] The mixed liquid is coated on the support layer, and the carbon dioxide separation membrane is obtained after drying.
[0010] A composition for forming a carbon dioxide separation membrane according to an embodiment of the present invention can be used to prepare a carbon dioxide gas separation membrane and can enable the gas separation membrane to have a higher carbon dioxide permeation rate. DETAILED DESCRIPTION
[0011] Typical embodiments that embody the features and advantages of the present invention will be described in detail in the following description. It should be understood that the present invention can have various changes in different embodiments without departing from the scope of the present invention, and the descriptions therein are essentially used as illustrations rather than to limit the present invention.
[0012] One embodiment of the present invention provides a composition for forming a carbon dioxide separation membrane, comprising a polymer and an organic salt; the organic salt is prepared by reacting an organic acid with an organic base; the organic acid comprises one or more basic groups and one or more acidic groups, the basic groups comprising amino groups (-NH2) and / or imino groups (-NH-), the acidic groups comprising one or more of carboxylic acid groups (-COOH), phosphoric acid groups (-PO(OH)2), sulfuric acid groups (-OSO2OH), and sulfonic acid groups (-SO2OH); the organic base comprises one or more of guanidine and its derivatives, piperazine and its derivatives.
[0013] A composition according to one embodiment of the present invention can be used to prepare a facilitated transfer membrane for carbon dioxide separation, wherein a polymer is a matrix and an organic salt is used as a carbon dioxide carrier; during operation, the carbon dioxide in the gas to be treated can act on the organic salt, and the organic salt can carry the carbon dioxide to move within the membrane and release the carbon dioxide, thereby transferring the carbon dioxide from the air inlet side of the membrane to the permeation side, thereby achieving separation of carbon dioxide from other components in the gas.
[0014] The organic salt of one embodiment of the present invention is stable in nature, not easily volatile, and has a high carbon dioxide loading capacity. When used as a carbon dioxide carrier in a carbon dioxide separation membrane, the prepared separation membrane can have higher carbon dioxide selectivity and permeability.
[0015] In one embodiment, the organic acid containing a carboxylic acid group includes amino acids, oligopeptides, tranexamic acid and their derivatives; further, amino acids are organic compounds containing a basic amino group and an acidic carboxyl group, including natural amino acids and unnatural amino acids, natural amino acids include glycine, alanine, valine, leucine, isoleucine, methionine (methionine), proline, tryptophan, serine, tyrosine, cysteine, phenylalanine, asparagine, glutamine, threonine, aspartic acid, glutamic acid, lysine, arginine, histidine, selenocysteine, pyrrolysine, etc., and unnatural amino acids are mainly derivatives of natural amino acids.
[0016] In one embodiment, the oligopeptide is prepared by dehydration condensation of 2 to 3 amino acids, including one or more of lysyl-proline, prolyl-isoleucine, prolyl-tryptophan, alanyl-glutamine, lysyl-phenylalanyl-lysine, lysyl-prolyl-valine, and lysyl-lysyl-lysine.
[0017] In one embodiment, the general formula of the organic acid containing a carboxylic acid group is as follows, wherein R1 represents hydrogen, a hydrocarbon group or a substituted hydrocarbon group containing 1 to 7 carbon atoms, and the substituent in the substituted hydrocarbon group can be an amino group, a carboxyl group, a phosphoric acid group, a hydroxyl group, or an acetyl group; R2 represents an alkylene group or a substituted alkylene group containing 1 to 7 carbon atoms, and the substituent in the substituted alkylene group can be an amino group, a carboxyl group, a phosphoric acid group, a hydroxyl group, or an acetyl group. Alternatively, R1 and R2 can be connected by a chemical bond and form a ring structure containing 2 to 7 carbon atoms together with the N atom.
[0018]
[0019] In one embodiment, the number of carbon atoms contained in R1 or R2 can be 1, 2, 3, 4, 5, 6 or 7.
[0020] In one embodiment, R1 can be an alkyl group or a substituted alkyl group containing 1 to 7 carbon atoms, such as methyl or ethyl; R2 can be an alkylene group or a substituted alkylene group containing 1 to 7 carbon atoms, such as methylene or ethylene.
[0021] In one embodiment, the organic acid containing a phosphoric acid group contains 1 to 10 carbon atoms, such as 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10; further, the organic acid containing a phosphoric acid group includes aminomethylphosphonic acid, 2-aminoethylphosphonic acid, 3-aminopropylphosphonic acid, and 4-aminobutanephosphonic acid.
[0022] In one embodiment, the organic acid containing a sulfuric acid group or a sulfonic acid group contains 1 to 10 carbon atoms, such as 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10; further, the organic acid containing a sulfuric acid group or a sulfonic acid group includes aminosulfonic acid, naphthylaminesulfonic acid, aminomethanesulfonic acid, 2-aminobenzenesulfonic acid, 3-aminobenzenesulfonic acid, 3-aminopropanesulfonic acid, 4-aminotoluene-3-sulfonic acid, 3-amino-4-hydroxybenzenesulfonic acid, 2,4-diaminobenzenesulfonic acid, 2,5-diaminobenzenesulfonic acid, 5-amino-2-naphthalenesulfonic acid, and hydroxylamine-O-sulfonic acid.
[0023] In one embodiment, guanidine and its derivatives include one or more of guanidine hydrochloride, guanidine sulfate, guanidine phosphate, guanidine carbonate, guanidine propionate, sulfaguanidine, guanidine acetic acid, dimethyl biguanide, N-phenylethyl biguanide, phenyl biguanide, agmatine sulfate, guanidine sulfonate, acetylguanidine, biguanide hydrochloride, methylguanidine hydrochloride, ethylguanidine hydrochloride, and 1-(tert-butoxycarbonyl)guanidine.
[0024] In one embodiment, piperazine and its derivatives include one or more of piperazine, piperazinone, 2-methylpiperazine, N-ethylpiperazine, 1-formaldehydepiperazine, N-aminoethylpiperazine, 2,3-diaminopiperazine, 1-(2-pyridyl)piperazine, 1-(4-pyridyl)piperazine, homopiperazine, piperazine-2-carboxylic acid, and piperazine-1-sulfonamide.
[0025] In one embodiment, the organic acid is selected from one or more of lysine, lysyl-proline, lysyl-lysyl-lysine, tranexamic acid, naphthylaminesulfonic acid, proline, aminomethylphosphonic acid, and 2,4-diaminobenzenesulfonic acid; the organic base is selected from one or more of sulfaguanidine, piperazine, N-aminoethylpiperazine, 2,3-diaminopiperazine, 1-(2-pyrimidinyl)piperazine, 1-(2-pyridinyl)piperazine, and dimethylbiguanide.
[0026] The present invention does not particularly limit the type of polymer, and the polymer may be a polymer suitable for film formation. To further improve the performance of the separation membrane, the polymer preferably has the ability to load carbon dioxide, for example, the polymer may be one or more of polyvinyl alcohol, polyvinylamine, polyallylamine, polyacrylamide, polyethyleneimine, cellulose, chitosan, and polyamide-amine.
[0027] In one embodiment, the number average molecular weight of the polymer can be 1 to 6 million, further 300,000 to 1 million, for example 50,000, 100,000, 200,000, 250,000, 350,000, 400,000, 450,000, 500,000, 600,000, 700,000, 800,000, 900,000, 2 million, 3 million, 4 million, or 5 million.
[0028] In one embodiment, the ratio of the amount of organic salt to the polymer is (0.01-0.6) mol:(1-20) g, for example, 0.1 mol:(1-2) g, 0.2 mol:(1-2) g, 0.3 mol:(1-2) g, 0.4 mol:(1-2) g, 0.5 mol:(1-2) g, (0.01-0.6) mol:3 g, (0.01-0.6) mol:5 g, (0.01-0.6) mol:8 g, (0.01-0.6) mol:10 g, (0.01-0.6) mol:12 g, (0.01-0.6) mol:15 g, (0.01-0.6) mol:18 g.
[0029] One embodiment of the present invention provides a carbon dioxide separation membrane, including a polymer layer, wherein the polymer layer has a structure that allows gas to pass through, and the raw material for preparing the polymer layer includes the above-mentioned composition.
[0030] In one embodiment, the carbon dioxide separation membrane includes a support layer, the polymer layer is disposed on the support layer, the support layer is used to provide good mechanical strength for the carbon dioxide separation membrane, and the support layer has a porous structure to allow gas to pass through. Further, the material of the support layer includes one or more of ceramics, metal oxides, polyolefin resins, polysulfone resins, polyvinylidene fluoride, and polydimethylsiloxane.
[0031] One embodiment of the present invention provides a method for preparing the above-mentioned carbon dioxide separation membrane, comprising the following steps:
[0032] S1: providing a mixed solution (or coating solution), the mixed solution comprising the above-mentioned organic salt, polymer and solvent; and
[0033] S2: coating the mixed liquid on the support layer, and preparing the carbon dioxide separation membrane after drying.
[0034] In one embodiment, the solvent of step S1 includes water.
[0035] In one embodiment, the preparation process of the carbon dioxide carrier organic salt comprises:
[0036] Prepare an organic acid aqueous solution;
[0037] preparing an organic base aqueous solution; and
[0038] The organic acid aqueous solution and the organic base aqueous solution are mixed for neutralization reaction to obtain an organic salt.
[0039] In one embodiment, the reaction temperature of the organic acid aqueous solution and the organic base aqueous solution can be 20-60°C, for example, 22°C, 25°C, 28°C, 30°C, 32°C, 35°C, 40°C, 45°C, 50°C, 55°C; the reaction time can be 0.5-4h, for example, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h.
[0040] In one embodiment, in the preparation of the organic salt, the molar ratio of the organic acid to the organic base used may be 1:(0.9-1.1), further 1: 1. For example, an equal volume of an organic acid aqueous solution and an organic base aqueous solution of equal molar concentration may be used for the reaction.
[0041] In one embodiment, the carbon dioxide carrier and the high molecular polymer can be dissolved in water (e.g., deionized water) to form a mixed solution. Further, in the mixed solution, the mass percentage concentration of the polymer can be 0.1-2.0%, such as 0.2%, 0.25%, 0.3%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%; the concentration of the organic salt can be 0.01-0.6 mol / L, such as 0.02 mol / L, 0.05 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L.
[0042] In one embodiment, in step S2, the coating thickness of the mixed liquid on the support layer can be 50 to 500 μm, for example, 60 μm, 80 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm; the coating speed can be 2 to 10 cm / s, for example, 3 cm / s, 4 cm / s, 5 cm / s, 6 cm / s, 7 cm / s, 8 cm / s, 9 cm / s.
[0043] In one embodiment, the drying time of step S2 can be 5 to 48 hours, for example, 8 hours, 10 hours, 12 hours, 15 hours, 18 hours, 20 hours, 22 hours, 24 hours, 25 hours, 28 hours, 30 hours, 32 hours, 35 hours, 36 hours, 40 hours, 45 hours; the drying treatment can be carried out under constant temperature and humidity conditions, for example, in a constant temperature and humidity chamber; the drying treatment temperature can be 30 to 80°C, for example, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C; the relative humidity of the drying treatment can be 20 to 60%, for example, 30%, 35%, 40%, 45%, 50%, 55%.
[0044] The carbon dioxide carrier organic salt according to one embodiment of the present invention has the advantages of high loading capacity and stable properties compared with existing carbon dioxide carriers. When used to prepare a gas separation membrane, a facilitated transport membrane with high permeation rate and high selectivity can be prepared.
[0045] A carbon dioxide separation membrane according to an embodiment of the present invention can be used to process a gas containing carbon dioxide, in particular a gas containing carbon dioxide and nitrogen.
[0046] The carbon dioxide separation membrane of one embodiment of the present invention has a carbon dioxide permeation rate of 800 to 4000 GPU, further 1000 to 4000 GPU, such as 1100 GPU, 1200 GPU, 1300 GPU, 1400 GPU, 1500 GPU, 1600 GPU, 1700 GPU, 1800 GPU, 2000 GPU, 2200 GPU, 2500 GPU, 2600 GPU, 2800 GPU, 3000 GPU, 3200 GPU, 3500 GPU, 3800 GPU for a carbon dioxide / nitrogen mixture; the separation factor of carbon dioxide / nitrogen can be 15 to 120, further 40 to 120, such as 20, 30, 35, 42, 45, 46, 48, 50, 52, 55, 58, 60, 70, 80, 90, 100, 110. The above parameters are measured at a pressure of 0.1 to 2.0 bar and room temperature.
[0047] The following is a further description of a carbon dioxide separation membrane according to an embodiment of the present invention in conjunction with a specific example. Unless otherwise specified, the raw materials used are all commercially available. In a few cases, the organic acid or organic base solution may be a suspension, and the organic salt solution obtained after the organic acid and the organic base are mixed and reacted is a clear solution.
[0048] Example 1
[0049] (1) Using lysine as an organic acid, a 0.4 mol / L lysine aqueous solution was prepared;
[0050] (2) using sulfaguanidine as an organic base, dissolving an appropriate amount in boiling water to prepare a 0.4 mol / L sulfaguanidine aqueous solution;
[0051] (3) taking equal volumes of the above lysine aqueous solution and sulfaguanidine aqueous solution, mixing and heating to 60° C., and stirring for 2 h to prepare a carbon dioxide carrier aqueous solution;
[0052] (4) preparing a polymer solution comprising 0.1% (mass percentage, the same below) polyvinyl alcohol, 0.1% polyvinylamine, and 0.05% polyacrylamide;
[0053] (5) taking 1 mL of the above carbon dioxide carrier aqueous solution and 9 mL of the above polymer solution and mixing them thoroughly to obtain a coating solution;
[0054] (6) A composite membrane of polyethersulfone and polydimethylsiloxane was used as a porous support layer, and a film was formed by scraping on its surface with a coating thickness of 100 μm and a coating speed of 5 cm / s; the resulting structure was then transferred to a constant temperature and humidity chamber at a temperature of 40°C and a relative humidity of 30% and dried for 24 hours to obtain a gas separation membrane containing a carbon dioxide carrier.
[0055] Example 2
[0056] This embodiment uses substantially the same raw materials and processes as those of embodiment 1 to prepare a gas separation membrane, the only difference being that lysyl-proline is used as the organic acid and piperazine is used as the organic base.
[0057] Example 3
[0058] This embodiment uses substantially the same raw materials and process as those of embodiment 2 to prepare a gas separation membrane, the only difference being that lysyl-lysyl-lysine is used as the organic acid.
[0059] Example 4
[0060] This embodiment uses substantially the same raw materials and processes as those of Embodiment 1 to prepare a gas separation membrane, with the only difference being that tranexamic acid is used as the organic acid, N-aminoethylpiperazine is used as the organic base, and the concentrations of the organic acid aqueous solution and the organic base aqueous solution are both 1 mol / L.
[0061] Example 5
[0062] This embodiment uses substantially the same raw materials and processes as those of Embodiment 1 to prepare a gas separation membrane, with the only difference being that the organic acid is naphthylaminesulfonic acid, the organic base is 2,3-diaminopiperazine, and the concentrations of the organic acid aqueous solution and the organic base aqueous solution are both 1 mol / L.
[0063] Example 6
[0064] This embodiment uses substantially the same raw materials and processes as those of Embodiment 1 to prepare a gas separation membrane, the only difference being that proline is used as the organic acid and 1-(2-pyridyl)piperazine is used as the organic base.
[0065] Example 7
[0066] This embodiment uses substantially the same raw materials and processes as those of embodiment 1 to prepare a gas separation membrane, the only difference being that the organic acid used is aminomethylphosphonic acid, and the organic base used is 1-(2-pyrimidinyl)piperazine.
[0067] Example 8
[0068] This embodiment uses substantially the same raw materials and processes as those of embodiment 1 to prepare a gas separation membrane, with the only difference being that 2,4-diaminobenzenesulfonic acid is used as the organic acid, dimethylbiguanide is used as the organic base, and the concentrations of the organic acid aqueous solution and the organic base aqueous solution are both 1 mol / L.
[0069] Example 9
[0070] This example uses substantially the same raw materials and process as Example 2 to prepare a gas separation membrane, with the only difference being that in step (5), 6 mL of the carbon dioxide carrier aqueous solution and 4 mL of the polymer solution are mixed.
[0071] Example 10
[0072] This example uses substantially the same raw materials and process as Example 2 to prepare a gas separation membrane, with the only difference being that the coating thickness in step (6) is 200 μm and the speed is 4 cm / s.
[0073] Embodiment 11
[0074] This example uses substantially the same raw materials and process as Example 1 to prepare a gas separation membrane, with the only difference being that in step (5), 0.1 mL of the carbon dioxide carrier aqueous solution is mixed with 9.9 mL of the polymer solution.
[0075] Example 12
[0076] This embodiment uses the same raw materials and process as embodiment 2 to prepare the gas separation membrane, with the only difference being that: in step (5), 4 mL of carbon dioxide carrier aqueous solution and 6 mL of polymer solution are mixed; and in step (6), the coating thickness is 200 μm and the speed is 4 cm / s.
[0077] Embodiment 13
[0078] (1) Using lysine as an organic acid, a 1 mol / L lysine aqueous solution was prepared;
[0079] (2) using 2,3-diaminopiperazine as an organic base, preparing a 1 mol / L 2,3-diaminopiperazine aqueous solution;
[0080] (3) taking equal volumes of the above lysine aqueous solution and 2,3-diaminopiperazine aqueous solution, mixing and heating to 40° C., and stirring for 4 h to prepare a carbon dioxide carrier aqueous solution;
[0081] (4) preparing a polymer solution comprising 0.1% (mass percentage, the same below) polyvinyl alcohol, 1% polyvinylamine, 0.01% polyacrylamide, and 0.1% polyethyleneimine;
[0082] (5) taking 1 mL of the above carbon dioxide carrier aqueous solution and 9 mL of the above polymer solution and mixing them thoroughly to obtain a coating solution;
[0083] (6) A polyvinylidene fluoride membrane is used as a porous support layer, and a film is formed by scraping on its surface with a thickness of 200 μm and a speed of 10 cm / s; the resulting structure is then transferred to a constant temperature and humidity chamber at a temperature of 40°C and a relative humidity of 30% and dried for 24 hours to obtain a gas separation membrane containing a carbon dioxide carrier.
[0084] Comparative Example 1
[0085] This comparative example uses substantially the same raw materials and processes as Example 1 to prepare a gas separation membrane, with the only difference being that steps (1), (2), (3), and (5) are omitted, i.e., no organic salt is added as a carrier to the prepared gas separation membrane.
[0086] Comparative Example 2
[0087] This comparative example uses substantially the same raw materials and process as Example 6 to prepare a gas separation membrane, with the only difference being that the alkali used is inorganic alkali sodium hydroxide.
[0088] Under the conditions of 25°C and 2 bar inlet pressure, a mixed gas of CO2 / N2 (15 / 85 vol) was used as the test gas, and the permeation rates of the gas separation membranes of the above embodiments and comparative examples for carbon dioxide and nitrogen humidified to a relative humidity of 90% were tested respectively, and the CO2 / N2 separation factor (i.e., the ratio of the CO2 permeation rate to the N2 permeation rate) was calculated. The specific results are shown in Table 1.
[0089] The specific test process is as follows: the gas separation membrane is cut into a suitable size and fixed in the membrane pool; the feed gas (CO2 / N2 mixed gas) is connected to the membrane pool, and the output pressure of the feed gas is controlled by a pressure reducing valve. Before the feed gas contacts the membrane to be tested in the membrane pool, it must first pass through a humidification tank and a dehumidification tank to make the mixed gas at saturated humidity or other humidity conditions; after part of the gas in the feed gas passes through the membrane, it is transmitted to the gas chromatograph by a purge gas (He) to analyze the gas composition on the permeation side of the membrane.
[0090] Table 1
[0091]
[0092]
[0093] According to Example 1, Comparative Example 1 and Table 1, the CO2 permeation rate and separation factor of the gas separation membrane of Example 1 are much higher than those of Comparative Example 1, indicating that the use of organic salt carriers can greatly improve the carbon dioxide permeation rate and selectivity of the gas separation membrane.
[0094] According to Examples 1 to 3, Examples 6 to 7, Comparative Example 2 and Table 1, under the same other conditions, the CO2 permeation rate and separation factor of the gas separation membranes of Examples 1 to 3 and 6 to 7 using organic salt carriers are much higher than those of the gas separation membrane of Comparative Example 2 using inorganic salt carriers, indicating that the performance of the organic salt carrier of the embodiments of the present invention is better than that of the inorganic salt carrier.
[0095] According to Examples 1 and 11, the gas separation membrane of Example 1 contains more carbon dioxide carrier organic salts than Example 11. From Table 1, it can be seen that the CO2 permeation rate and separation factor of the gas separation membrane of Example 1 are greater than the CO2 permeation rate and separation factor of the gas separation membrane of Example 11. This result shows that appropriately increasing the content of carbon dioxide carrier in the gas separation membrane can increase the CO2 permeation rate and separation factor. In addition, according to Examples 2 and 9 and Table 1, compared with Example 2, the content of carbon dioxide carrier in the gas separation membrane in Example 9 is greatly increased. Although it can increase the CO2 permeation rate, the separation factor decreases. This shows that too high an organic salt carrier content will reduce the selectivity of the membrane. Based on the above results, the ratio of the amount of organic salt to the polymer is preferably (0.02-0.12) mol: (1-2.25) g.
[0096] According to Examples 1 and 2 and Table 1, compared with Example 1, the CO2 permeation rate of the gas separation membrane of Example 2 is higher, indicating that the organic salt prepared by the reaction of lysine-proline and piperazine has a higher carbon dioxide loading capacity than the organic salt prepared by the reaction of lysine and sulfaguanidine.
[0097] According to Examples 2, 3 and Table 1, compared with Example 3, the gas separation membrane of Example 2 has a higher CO2 permeation rate and a similar separation factor, indicating that the performance of the organic salt carrier prepared by the reaction of lysyl-proline and piperazine is generally better than that of the organic salt prepared by the reaction of lysyl-lysyl-lysine and piperazine.
[0098] According to Examples 1, 3 to 8 and Table 1, compared with Examples 3 to 8, the gas separation membrane of Example 1 has a higher CO2 permeation rate and separation factor, indicating that the performance of the organic salt carrier prepared by the reaction of lysine and sulfaguanidine is generally better than that of the organic salt prepared by the reaction of lysyl-lysyl-lysine, piperazine, etc.
[0099] According to Examples 2, 4, 5, 6, 7, 8 and Table 1, the gas separation membrane of Example 2 has a higher CO2 permeation rate than Examples 4, 5, 6, 7, 8, indicating that the organic salt prepared by the reaction of lysyl-proline and piperazine has a higher carbon dioxide loading capacity than other organic salts such as tranexamic acid and N-aminoethylpiperazine.
[0100] According to Examples 3, 6, 7 and Table 1, compared with Examples 3 and 7, the gas separation membrane of Example 6 has a higher CO2 permeation rate and separation factor, indicating that the performance of the organic salt carrier prepared by the reaction of proline and 1-(2-pyridyl)piperazine is generally better than the organic salt prepared by the reaction of lysyl-lysyl-lysine and piperazine and the organic salt prepared by the reaction of aminomethylphosphonic acid and 1-(2-pyrimidinyl)piperazine.
[0101] According to Examples 4, 5, 6, 8 and Table 1, the concentration of the organic salt in Example 6 is less than that in Examples 4, 5, and 8, but the gas separation membrane in Example 6 has a higher CO2 permeation rate and separation factor than those in Examples 4, 5, and 8, indicating that the performance of the organic salt carrier in Example 6 is better than that of the organic salt carrier in Examples 4, 5, and 8 as a whole. Further, compared with Example 8, the gas separation membranes in Examples 4 and 5 have a higher CO2 permeation rate and separation factor, indicating that the performance of the organic salt carrier in Examples 4 and 5 is better than that of the organic salt carrier in Example 8 as a whole.
[0102] Combined with the above results, in order to improve the comprehensive performance of the separation membrane, the carbon dioxide carrier is preferably an organic salt obtained by the reaction of lysine and sulfaguanidine (Example 1), an organic salt obtained by the reaction of lysyl-proline and piperazine (Example 2), an organic salt obtained by the reaction of proline and 1-(2-pyridyl)piperazine (Example 6), an organic salt obtained by the reaction of tranexamic acid and N-aminoethylpiperazine (Example 4), an organic salt obtained by the reaction of naphthylaminesulfonic acid and 2,3-diaminopiperazine (Example 5); further preferably, an organic salt obtained by the reaction of lysine and sulfaguanidine (Example 1), an organic salt obtained by the reaction of lysyl-proline and piperazine (Example 2), an organic salt obtained by the reaction of proline and 1-(2-pyridyl)piperazine (Example 6); further preferably, an organic salt obtained by the reaction of lysine and sulfaguanidine (Example 1), an organic salt obtained by the reaction of lysyl-proline and piperazine (Example 2).
[0103] According to the above results, the organic acid for preparing the organic salt is preferably lysine, lysyl-proline, proline, tranexamic acid, naphthamine sulfonic acid; more preferably lysine, lysyl-proline, proline; more preferably lysine, lysyl-proline. The organic base for preparing the organic salt is preferably sulfaguanidine, piperazine, 1-(2-pyridyl)piperazine, N-aminoethylpiperazine, 2,3-diaminopiperazine, more preferably sulfaguanidine, piperazine, 1-(2-pyridyl)piperazine; more preferably sulfaguanidine and piperazine.
[0104] Compared with Example 2, Example 10 can improve the permeability selectivity of the membrane by optimizing the scraping thickness and scraping speed. Therefore, the coating thickness of the mixed solution on the support layer is preferably 180-220 μm, more preferably 190-210 μm, and more preferably 200 μm; the coating speed is preferably 4-5 cm / s.
[0105] Example 12: Optimizing the carrier content, coating thickness and coating speed can further improve the permeation selectivity of the membrane. Example 13: Changing the support layer type and membrane preparation conditions can also prepare separation membranes with suitable performance for different support layers.
[0106] Unless otherwise defined, the terms used in the present invention have the meanings commonly understood by those skilled in the art.
[0107] The embodiments described in the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Those skilled in the art may make various other substitutions, changes and improvements within the scope of the present invention. Therefore, the present invention is not limited to the above embodiments, but is only limited by the claims.
Claims
1. A composition for forming a carbon dioxide separation membrane, comprising a polymer and an organic salt; the organic salt is prepared by reacting an organic acid with an organic base; the organic acid comprises a basic group and an acidic group, the basic group comprises an amino group and / or an imino group, the acidic group comprises one or more of a carboxylic acid group, a phosphoric acid group, a sulfuric acid group, and a sulfonic acid group; the organic base comprises one or more of guanidine and its derivatives, piperazine and its derivatives.
2. The composition according to claim 1, wherein The organic acid containing a carboxylic acid group is selected from one or more of amino acids, oligopeptides, and tranexamic acid; the organic acid containing a phosphate group contains 1 to 10 carbon atoms; the organic acid containing a sulfate group or a sulfonic acid group contains 1 to 10 carbon atoms; The amino acids include one or more of glycine, alanine, valine, leucine, isoleucine, methionine, proline, tryptophan, serine, tyrosine, cysteine, phenylalanine, asparagine, glutamine, threonine, aspartic acid, glutamic acid, lysine, arginine, histidine, selenocysteine, and pyrrolysine; and / or, The guanidine and its derivatives include one or more of guanidine hydrochloride, guanidine sulfate, guanidine phosphate, guanidine carbonate, guanidine propionate, sulfaguanidine, guanidine acetic acid, dimethyl biguanidine, N-phenylethyl biguanidine, phenyl biguanidine, agmatine sulfate, guanidine sulfamate, acetylguanidine, biguanide hydrochloride, methylguanidine hydrochloride, ethylguanidine hydrochloride, and 1-(tert-butyloxycarbonyl)guanidine; and / or, The piperazine and its derivatives include one or more of piperazine, piperazinone, 2-methylpiperazine, N-ethylpiperazine, 1-formaldehydepiperazine, N-aminoethylpiperazine, 2,3-diaminopiperazine, 1-(2-pyridyl)piperazine, 1-(4-pyridyl)piperazine, homopiperazine, piperazine-2-carboxylic acid, and piperazine-1-sulfonamide.
3. The composition according to claim 2, wherein The oligopeptide is prepared by dehydration condensation of 2 to 3 amino acids, including one or more of lysyl-proline, prolyl-isoleucine, prolyl-tryptophan, alanyl-glutamine, lysyl-phenylalanyl-lysine, lysyl-prolyl-valine, lysyl-lysyl-lysine; and / or, The organic acid comprising a carboxylic acid group has the following general formula: Wherein, R1 represents hydrogen, a hydrocarbon group or a substituted hydrocarbon group containing 1 to 7 carbon atoms, wherein the substituent in the substituted hydrocarbon group is selected from an amino group, a carboxyl group, a phosphoric acid group, a hydroxyl group, and an acetyl group; R2 represents an alkylene group or a substituted alkylene group containing 1 to 7 carbon atoms, wherein the substituent in the substituted alkylene group is selected from an amino group, a carboxyl group, a phosphoric acid group, a hydroxyl group, and an acetyl group; or, R1 and R2 are connected by a chemical bond and together with the N atom form a ring structure containing 2 to 7 carbon atoms; and / or, The organic acid containing a phosphate group is selected from one or more of aminomethylphosphonic acid, 2-aminoethylphosphonic acid, 3-aminopropylphosphonic acid, and 4-aminobutanephosphonic acid; the organic acid containing a sulfate group or a sulfonic acid group is selected from one or more of aminosulfonic acid, naphthylaminesulfonic acid, aminomethanesulfonic acid, 2-aminobenzenesulfonic acid, 3-aminobenzenesulfonic acid, 3-aminopropanesulfonic acid, 4-aminotoluene-3-sulfonic acid, 3-amino-4-hydroxybenzenesulfonic acid, 2,4-diaminobenzenesulfonic acid, 2,5-diaminobenzenesulfonic acid, 5-amino-2-naphthalenesulfonic acid, and hydroxylamine-O-sulfonic acid.
4. The composition according to claim 1, wherein The organic acid is selected from one or more of lysine, lysyl-proline, lysyl-lysyl-lysine, tranexamic acid, naphthylaminesulfonic acid, proline, aminomethylphosphonic acid, and 2,4-diaminobenzenesulfonic acid; the organic base is selected from one or more of sulfaguanidine, piperazine, N-aminoethylpiperazine, 2,3-diaminopiperazine, 1-(2-pyridyl)piperazine, 1-(2-pyrimidyl)piperazine, and dimethylbiguanide; and / or, The polymer includes one or more of polyvinyl alcohol, polyvinylamine, polyallylamine, polyacrylamide, polyethyleneimine, cellulose, chitosan, and polyamide-amine; and / or, The number average molecular weight of the polymer is 1 to 6 million; and / or, The content ratio of the organic salt to the polymer is (0.01-0.6) mol: (1-20) g.
5. The composition according to claim 1, wherein The organic salt is selected from one or more of the following organic salts: an organic salt obtained by the reaction of lysine and sulfaguanidine, an organic salt obtained by the reaction of lysyl-proline and piperazine, an organic salt obtained by the reaction of proline and 1-(2-pyridyl)piperazine, an organic salt obtained by the reaction of tranexamic acid and N-aminoethylpiperazine, and an organic salt obtained by the reaction of naphthylaminesulfonic acid and 2,3-diaminopiperazine. 6 . A carbon dioxide separation membrane, comprising a polymer layer, wherein a raw material for preparing the polymer layer comprises the composition according to any one of claims 1 to 5.
7. The carbon dioxide separation membrane according to claim 6 comprises a support layer, and the polymer layer is arranged on the support layer; the material of the support layer comprises one or more of ceramics, metal oxides, polyolefins, polysulfones, polyvinylidene fluoride, and polydimethylsiloxane.
8. The method for preparing the carbon dioxide separation membrane according to claim 7, comprising the following steps: Providing a mixed solution, the mixed solution comprising the composition and a solvent; and The mixed liquid is coated on the support layer, and the carbon dioxide separation membrane is obtained after drying.
9. The method according to claim 8, wherein: In the mixed solution, the mass percentage concentration of the polymer is 0.1-2.0%, and the concentration of the organic salt is 0.01-0.6 mol / L; and / or, The coating thickness of the mixed solution is 50 to 500 μm, further 180 to 220 μm; the coating speed is 2 to 10 cm / s, further 4 to 5 cm / s.
10. The method according to claim 8, wherein: The drying process is performed at a temperature of 30 to 80° C. and a relative humidity of 20 to 60%.
Citation Information
Patent Citations
BE539081A
Carbon dioxide separating membrane having both primary amine and carbonate and preparation method thereof
CN104857867A
Acid gas separation membrane, acid gas separation device, method for producing acid gas separation membrane, and acid gas separation method
CN114340771A
Ionic liquid composition for carbon dioxide separation membrane, carbon dioxide separation membrane holding said composition, and carbon dioxide concentration device provided with said carbon dioxide separation membrane
CN115151334A
Process for separating CO2 from other gases
US4659343A