Preparation method of porous bio-based atmospheric water enrichment material
By combining modified seafood mushrooms with hygroscopic salt, using their natural porous structure and oxygen-rich groups, the cost and non-degradable problems of the existing atmospheric water-enriched material preparation methods are solved, and efficient and green atmospheric water vapor is achieved. It is enriched and has strong renewable materials, which improves the sustainability of atmospheric water enrichment.
Patent Information
- Application Number
- CN202411138550.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The existing preparation methods for atmospheric water-enriched materials have problems such as high cost, complex process, non-degradable and hygroscopic salt dissolution, and there are few researches on improving the ability of hygroscopic salt enrichment in biomass porous materials.
Modified seafood mushrooms are used as porous biological matrix, combined with hygroscopic salts, and saturated solution is prepared by dissolving hygroscopic salts in anhydrous ethanol, and modified seafood mushrooms in the presence of NaOH and acid, introducing oxygen-rich groups to form hygroscopic salts. /Modified seafood mushroom material, using its natural porous structure to improve the enrichment ability of water vapor in the atmosphere.
It has achieved low-cost, efficient and green atmospheric water-enriched materials, which are highly recyclable and can be recycled by hygroscopic salts, which reduces environmental pollution and improves the sustainability of atmospheric water-enriched materials.
Smart Images

Figure CN119016032A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functional composite materials, in particular to a method for preparing a porous bio-based atmospheric water enrichment material. Background Art
[0002] Atmospheric water-enriched materials refer to materials that can absorb water in the atmosphere. They have high water absorption properties and can absorb water in a dry environment to form hydrogels or liquid water. The importance of atmospheric water-enriched materials lies in that they can help people collect and utilize water resources in the atmosphere, thereby solving the problem of water shortage. The application fields of atmospheric water-enriched materials are very wide, mainly including agriculture, environmental protection, medical care, construction, etc. In the agricultural field, atmospheric water-enriched materials can be used for soil water retention, plant growth and irrigation. In environmental protection, atmospheric water-enriched materials can be used to treat wastewater and purify the atmosphere. In medical care, atmospheric water-enriched materials can be used to prepare dressings and biomedical materials. In construction, atmospheric water-enriched materials can be used to prepare waterproof materials and thermal insulation materials, etc.
[0003] In addition to existing in the form of clouds and being collected through rainfall, the moisture in the atmosphere also exists mainly in the form of fog and water vapor in the air. Some different atmospheric water collection technologies have been developed from these two forms of existence. The main types are: fog capture technology developed for moisture in the atmosphere in the form of fog; dew collection technology based on cooling developed for moisture in the form of water vapor, and atmospheric water collection technology based on adsorption. The main problem with fog collection is that it requires 100% relative humidity (RH), which is limited by climate and geography. Dew collection technology requires cooling energy input to keep the condensation temperature below the vapor dew point. When the RH is below 40%, this will make active cooling very energy-consuming. At present, some scholars have studied passive radiation cooling materials for enriching water in the atmosphere, but there are few large-scale application studies. In contrast, atmospheric water enrichment materials that use adsorbents to capture moisture are more energy-efficient and are not restricted by hydrology, geographical location, etc. Among them, hygroscopic salts are a low-cost but efficient desiccant. Under moderate relative humidity conditions, deliquescent salts such as CaCl2, LiCl and LiBr can adsorb water molecules weighing 1-3 times their own weight. These hygroscopic salts have strong water absorption capacity and are very suitable for hygroscopic related applications, so they have received extensive attention in the field of water enrichment. However, a disadvantage that limits their use is that they will eventually dissolve in the collected water, resulting in reduced absorption kinetics, system corrosion, and difficulty in recovering the adsorbent. To solve this problem, the most popular strategy is to composite hygroscopic salts into designed matrices, where the loaded salts play a major role in capturing water molecules, while the matrix acts as a container to hold the salts that eventually liquefy. The water absorption performance of salt-based composites depends on the choice of salts, loading content, and matrix design. In recent years, a lot of research has been conducted to develop functional matrices with better water collection performance. The reported matrix materials can be divided into porous materials, hollow structure containers, fiber matrices, and polymer networks. However, most matrix materials supporting hygroscopic salts have disadvantages such as complex synthesis process, high energy consumption, and non-degradability, which have a negative impact on the cost-effectiveness and ecological benefits of atmospheric water enrichment materials. Therefore, how to design a low-cost, efficient, and green ecological substrate material is the key to promoting the sustainable development of atmospheric water enrichment materials based on adsorption.
[0004] Most plants (such as mushrooms) grown in nature have natural porous structures and good adsorption properties, and are easy to be processed into various shapes and sizes to meet different needs. These biomass porous materials are derived from low-cost natural biomass. Compared with fossil fuels, they do not produce harmful gases such as carbon dioxide and are more environmentally friendly. At the same time, biomass porous materials can be made from renewable biomass, which can be recycled to reduce dependence on natural resources. However, there are few reports on the application of biomass porous materials in atmospheric water enrichment materials and the research on the enrichment ability of hygroscopic salts to water vapor in the atmosphere. Therefore, how to design a biomass porous matrix material, and coordinate the advantages of matrix materials and hygroscopic salts to achieve the preparation of a new low-cost, green and efficient atmospheric water enrichment material is the key problem to be solved by the present invention. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a porous bio-based atmospheric water-enriching material, so as to solve the problems existing in the method for preparing an atmospheric water-enriching material in the prior art.
[0006] The present invention provides a method for preparing a porous bio-based atmospheric water enrichment material, comprising the following steps:
[0007] (1) Preparation of hygroscopic salt solution: dissolving hygroscopic salt in anhydrous ethanol solution to obtain a saturated hygroscopic salt solution at room temperature;
[0008] (2) Preparation of modified seafood mushroom: dry seafood mushroom is placed in a NaOH solution with a concentration of 1 to 5 wt% at a bath ratio of 1:100 to 1:50, boiled for 30 to 120 min, and then anhydrous ethanol and sodium chloroacetate are added to the solution, wherein the amount of anhydrous ethanol is 1:10 to 1:50 according to the bath ratio of seafood mushroom, and the molar mass of sodium chloroacetate and seafood mushroom is 1:1, the mixture is kept at 71° C. for 4 hours, filtered after the reaction is completed, and the filtrate is dried and washed with deionized water to obtain a fibrous pretreated seafood mushroom;
[0009] The pretreated seafood mushroom is dispersed in deionized water at a bath ratio of 1:20 to 1:100, nitric acid and phosphoric acid are added to the solution at a volume ratio of 1 to 5:1, the total acid concentration in the solution is 10 to 20%, and the reaction is carried out at room temperature for 3 to 5 hours, and sodium nitrite is continuously added to the solution, the concentration of sodium nitrite is 0.5 to 5%, and the reaction is carried out at room temperature for 12 to 48 hours, and the modified seafood mushroom with rich oxygen groups is obtained after filtering, washing with water, and drying.
[0010] (3) Preparation of hygroscopic salt / modified seafood mushroom material: The modified seafood mushroom is immersed in a hygroscopic salt solution according to the bath ratio for a certain period of time, taken out, and vacuum dried to obtain the hygroscopic salt / modified seafood mushroom material.
[0011] In the method for preparing a porous bio-based atmospheric water enrichment material as described above, preferably, the weight portion of the hygroscopic salt is 1 to 5 parts, and the weight portion of the modified seafood mushroom is 5 to 10 parts.
[0012] A method for preparing a porous bio-based atmospheric water-enriching material as described above, wherein, preferably, the hygroscopic salt is lithium chloride or potassium acetate or magnesium chloride or potassium carbonate or magnesium nitrate or ammonium nitrate or sodium chloride or potassium chloride or potassium nitrate or potassium sulfate.
[0013] A method for preparing a porous bio-based atmospheric water enrichment material as described above, wherein, preferably, the bath ratio in step (3) is 1:50-100, the immersion time is 5-10 hours, the vacuum drying temperature is 75°C, and the drying time is 2 hours.
[0014] A method for preparing a porous bio-based atmospheric water enrichment material as described above, wherein preferably, the seafood mushroom is a seafood mushroom with a growth period of 110 to 120 days.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] (1) Taking advantage of the natural porous structure of seafood mushrooms, the modified porous biomass material is combined with hygroscopic salts. The hygroscopic salts can adsorb moisture from the atmosphere to the surface of the material, and then the moisture is transferred to the interior of the seafood mushrooms and stored in the porous structure of oxygen-rich groups, thereby achieving efficient enrichment of water vapor in the atmosphere.
[0017] (2) The raw materials of the porous bio-based atmospheric water enrichment material of the present invention are derived from natural seafood mushrooms, hygroscopic salts, etc., with low preparation cost, simple synthesis process, green environmental protection, and biodegradability. It is a low-cost, green, and efficient atmospheric water enrichment material.
[0018] (3) The porous bio-based atmospheric water-enriching material of the present invention has good reproducibility and reusability, and can be used multiple times to reduce the consumption of natural resources. Hygroscopic salts can also be regenerated and recycled to reduce environmental pollution. The porous bio-based atmospheric water-enriching material can improve the sustainability of atmospheric water enrichment, realize the recycling of resources, protect the environment, and promote sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is the infrared spectrum of the modified seafood mushroom of the present invention;
[0020] Figure 2 This is a scanning electron microscope image of a partially enlarged cross section of the modified seafood mushroom of the present invention;
[0021] Figure 3 This is a scanning electron microscope image of a partially enlarged longitudinal section of the modified seafood mushroom of the present invention;
[0022] Figure 4 is a partially enlarged scanning electron microscope image of the cross section of the hygroscopic salt / modified seafood mushroom in Example 1 of the present invention;
[0023] Figure 5 is a scanning electron microscope image of a partially enlarged longitudinal section of the hygroscopic salt / modified seafood mushroom in Example 1 of the present invention;
[0024] Figure 6 This is a graph showing the water enrichment performance of hygroscopic salt / modified seafood mushroom in Example 1 of the present invention. DETAILED DESCRIPTION
[0025] The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, but should not be construed as limiting the present invention.
[0026] The present invention provides a method for preparing a porous bio-based atmospheric water enrichment material, comprising the following steps:
[0027] (1) Preparation of hygroscopic salt solution: dissolve the hygroscopic salt in anhydrous ethanol solution to obtain a saturated hygroscopic salt solution at room temperature. The weight proportion of the hygroscopic salt is 1 to 5 parts. In the embodiments provided in the present application, the hygroscopic salt is lithium chloride or potassium acetate or magnesium chloride or potassium carbonate or magnesium nitrate or ammonium nitrate or sodium chloride or potassium chloride or potassium nitrate or potassium sulfate.
[0028] (2) Preparation of modified seafood mushroom: The weight proportion of the modified seafood mushroom is 5 to 10 parts, and the dried seafood mushroom is placed in a NaOH solution with a concentration of 1 to 5 wt% at a bath ratio of 1:100 to 1:50, and boiled for 30 to 120 minutes. Then, anhydrous ethanol and sodium chloroacetate are added to the solution, wherein the amount of anhydrous ethanol is 1:10 to 1:50 according to the bath ratio of seafood mushroom, and the molar mass of sodium chloroacetate and seafood mushroom is 1:1. The mixture is kept at 71°C for 4 hours, and filtered after the reaction is completed. The pretreated seafood mushroom is dried and washed with deionized water to obtain fibrous pretreated seafood mushrooms; the pretreated seafood mushrooms are dispersed in deionized water at a bath ratio of 1:20 to 1:100, nitric acid and phosphoric acid are added to the solution at a volume ratio of 1 to 5:1, the total acid concentration in the solution is 10 to 20%, and the reaction is carried out at room temperature for 3 to 5 hours, and sodium nitrite is continuously added to the solution, the concentration of sodium nitrite is 0.5 to 5%, and the reaction is carried out at room temperature for 12 to 48 hours; after filtering, washing with water, and drying, modified seafood mushrooms rich in oxygen groups are obtained. In the embodiment provided in the present application, the seafood mushroom is a seafood mushroom with a growth period of 110 to 120 days.
[0029] (3) Preparation of hygroscopic salt / modified seafood mushroom material: The modified seafood mushroom is immersed in the hygroscopic salt solution according to the bath ratio, immersed for a certain period of time, taken out, and vacuum dried to obtain the hygroscopic salt / modified seafood mushroom material. In the embodiments provided in the present application, the bath ratio is 1:50-100, the immersion time is 5-10 hours, the vacuum drying temperature is 75°C, and the drying time is 2 hours.
[0030] Reference Figure 1 As shown in the figure, curve G is the infrared spectrum of the modified seafood mushroom, and curve T is the infrared spectrum of the natural seafood mushroom. It can be seen from the infrared spectrum that the natural seafood mushroom contains the peak structure of the cellulose macromolecular chain, indicating that the composition of the natural seafood mushroom includes cellulose components. The cellulose macromolecules of the natural seafood mushroom are at 1645cm -1 The characteristic vibration peak of water adsorption near the 1735cm -1 A weak carbonyl vibration peak appears, which may be because the natural seafood mushroom cellulose macromolecules have certain carboxyl groups, which further confirms that the natural seafood mushroom itself has a good ability to absorb water. Figure 1 It was found that the modified seafood mushroom was at 1735cm -1 An obvious stretching vibration absorption band of carboxyl C=O appears at the position, and the peak intensity is relatively obvious, indicating that oxygen-rich carboxyl groups appear in the cellulose macromolecular chain of the modified seafood mushroom, and the number is relatively large. At the same time, the overall peak shape of the modified seafood mushroom has not changed significantly, which shows that the modified seafood mushroom maintains the carbon skeleton of cellulose and its structure is not destroyed, which is beneficial to ensure the stability and mechanical properties of the porous structure of the modified seafood mushroom. The present invention introduces a large number of carboxyl groups into the porous structure of the seafood mushroom through oxidative modification, thereby improving its hydrophilic properties and the water storage capacity of the seafood mushroom. In addition, by comparing the infrared spectra of natural seafood mushroom and modified seafood mushroom, it can be seen that the modified seafood mushroom has a strong carbonyl group at 1645cm -1 The absorption peak intensity at is also significantly higher than that of natural seafood mushrooms, indicating that the amount of adsorbed water in the cellulose macromolecules of the modified seafood mushrooms has increased, which further confirms the strong water binding ability of the modified seafood mushrooms.
[0031] Reference Figure 2 As shown, the modified seafood mushroom has a natural three-dimensional porous structure formed by cross-linking of cellulose macromolecular chains, which provides a good structural advantage for storing atmospheric water absorbed by hygroscopic salts.
[0032] Reference Figure 3 As shown, the modified seafood mushroom has a certain orientation structure inside, indicating that the seafood mushroom cellulose macromolecules form a connected pore structure inside it, which also provides a channel for the atmospheric water adsorbed by hygroscopic salt to be transmitted inside the seafood mushroom, reducing the mass transfer barrier, which will be beneficial to the hygroscopic salt / modified seafood mushroom material to achieve efficient atmospheric water enrichment.
[0033] Several embodiments are listed below to further illustrate the contents of the present invention. Those skilled in the art will appreciate that more preparation methods can be designed based on the following embodiments, all of which fall within the protection scope of the present invention.
[0034] Example 1
[0035] Weigh a certain mass of lithium chloride and dissolve it in an anhydrous ethanol solution to obtain a saturated hygroscopic salt solution at room temperature. Immerse the modified seafood mushroom in the hygroscopic salt solution according to a bath ratio of 1:80 for 8 hours, take it out, and vacuum dry it at 75°C for 2 hours to obtain a hygroscopic salt / modified seafood mushroom material. The modified seafood mushroom used in this embodiment was prepared according to the method provided in this application.
[0036] Reference Figure 4 As shown in the figure, the hygroscopic salt is firmly and evenly loaded on the surface of the cellulose macromolecules of the modified seafood mushroom. The porous material has a large specific surface area and porosity, which can increase the contact area and adsorption amount of the hygroscopic salt, thereby improving the efficiency of atmospheric enrichment of water. At the same time, the biomass porous material is used in combination with the hygroscopic salt. The porous material can store the water adsorbed by the hygroscopic salt, further enhancing the hygroscopic performance of the hygroscopic salt and improving the collection efficiency of atmospheric enrichment of water.
[0037] Reference Figure 5 As shown, the hygroscopic salt is firmly and evenly loaded inside the modified seafood mushroom, and the porous structure of the modified seafood mushroom serves as a matrix to provide support for the hygroscopic salt, preventing it from deliquescence and loss after moisture absorption.
[0038] Reference Figure 6 As shown, in an atmosphere with an air humidity (RH) of 30%, the amount of water enriched by the hygroscopic salt / modified seafood mushroom increases with the increase of adsorption time, and the maximum value can reach 0.5g / g, and equilibrium is reached after 50min of adsorption. The water enrichment capacity of the porous bio-based atmospheric water-enriching material is significantly higher than the value reported in the literature (Fuel Process. Technol. 2002, 79 (3), 225-231., Adv. Mater. 2020, 32 (39), 2002936.), which further confirms its efficient atmospheric water enrichment capacity.
[0039] Example 2
[0040] Weigh a certain mass of lithium bromide and dissolve it in an anhydrous ethanol solution to obtain a saturated hygroscopic salt solution at room temperature. Immerse the modified seafood mushroom in the hygroscopic salt solution according to a bath ratio of 1:80 for 8 hours, take it out, and vacuum dry it at 75°C for 2 hours to obtain a hygroscopic salt / modified seafood mushroom material. The modified seafood mushroom used in this embodiment is prepared according to the method provided in this application.
[0041] Example 3
[0042] Weigh a certain mass of calcium chloride and dissolve it in an anhydrous ethanol solution to obtain a saturated hygroscopic salt solution at room temperature. Immerse the modified seafood mushroom in the hygroscopic salt solution according to a bath ratio of 1:80 for 8 hours, take it out, and vacuum dry it at 75°C for 2 hours to obtain a hygroscopic salt / modified seafood mushroom material. The modified seafood mushroom used in this embodiment was prepared according to the method provided in this application.
[0043] The above describes in detail the structure, features and effects of the present invention based on the embodiments shown in the drawings. The above is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown in the drawings. Any changes made according to the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the description and drawings, should be within the protection scope of the present invention.
Claims
1. A method for preparing a porous bio-based atmospheric water enrichment material, characterized in that: The following steps are involved: (1) Preparation of hygroscopic salt solution: dissolving hygroscopic salt in anhydrous ethanol solution to obtain a saturated hygroscopic salt solution at room temperature; (2) Preparation of modified seafood mushroom: dry seafood mushroom is placed in a NaOH solution with a concentration of 1 to 5 wt% at a bath ratio of 1:100 to 1:50, boiled for 30 to 120 min, and then anhydrous ethanol and sodium chloroacetate are added to the solution, wherein the amount of anhydrous ethanol is 1:10 to 1:50 according to the bath ratio of seafood mushroom, and the molar mass of sodium chloroacetate and seafood mushroom is 1:1, the mixture is kept at 71° C. for 4 hours, filtered after the reaction is completed, and the filtrate is dried and washed with deionized water to obtain a fibrous pretreated seafood mushroom; The pretreated seafood mushroom is dispersed in deionized water at a bath ratio of 1:20 to 1:100, nitric acid and phosphoric acid are added to the solution at a volume ratio of 1 to 5:1, the total acid concentration in the solution is 10 to 20%, and the reaction is carried out at room temperature for 3 to 5 hours, and sodium nitrite is continuously added to the solution, the concentration of sodium nitrite is 0.5 to 5%, and the reaction is carried out at room temperature for 12 to 48 hours, and the modified seafood mushroom with rich oxygen groups is obtained after filtering, washing with water, and drying. (3) Preparation of hygroscopic salt / modified seafood mushroom material: The modified seafood mushroom is immersed in a hygroscopic salt solution according to the bath ratio for a certain period of time, taken out, and vacuum dried to obtain the hygroscopic salt / modified seafood mushroom material.
2. The method for preparing the porous bio-based atmospheric water enrichment material according to claim 1, characterized in that: The weight proportion of the hygroscopic salt is 1 to 5 parts, and the weight proportion of the modified seafood mushroom is 5 to 10 parts.
3. The method for preparing the porous bio-based atmospheric water enrichment material according to claim 1, characterized in that: The hygroscopic salt is lithium chloride or potassium acetate or magnesium chloride or potassium carbonate or magnesium nitrate or ammonium nitrate or sodium chloride or potassium chloride or potassium nitrate or potassium sulfate.
4. The method for preparing the porous bio-based atmospheric water enrichment material according to claim 1, characterized in that: The bath ratio in step (3) is 1:50-100, the immersion time is 5-10 hours, the vacuum drying temperature is 75° C., and the drying time is 2 hours.
5. The method for preparing the porous bio-based atmospheric water enrichment material according to claim 1, characterized in that: The seafood mushroom is a seafood mushroom with a growth period of 110 to 120 days.
Citation Information
Patent Citations
Biomass-based air water collection material as well as preparation method and application thereof
CN118185056A
Porous photo-thermal composite material based on atmospheric water vapor adsorption as well as preparation method and application of porous photo-thermal composite material
CN118344653A
Method of producing water out of air
RU2101423C1