Catalyst for preparing octanol and preparation method thereof

Through the combination of rotary strengthening technology and filler bed, the problem of cumbersome catalyst preparation process and high energy consumption is solved, and efficient and environmentally friendly catalysts are prepared, achieving high conversion and yield of octanol.

CN119016050APending Publication Date: 2024-11-26CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310590059.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the preparation process of octanol catalysts is cumbersome or has high energy consumption, making it difficult to achieve a high conversion rate and green and environmentally friendly processing process.

Method used

Using rotary strengthening technology and rotary filler bed, liquid mist and droplets are formed under centrifugal force through wire mesh or cylindrical filler, sprayed onto the surface of the carrier, improving the diffusion and permeability rate of the impregnation liquid and uniform adsorption of active components, and preparing A catalyst with high dispersion of metal components and small average particle size.

Benefits of technology

It significantly shortens the impregnation time of the catalyst, improves the dispersion and performance of the catalyst, simplifies the process flow, is suitable for industrial production, and improves the conversion and yield of octanol.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016050A_ABST
    Figure CN119016050A_ABST
Patent Text Reader

Abstract

The invention provides a catalyst for preparing octanol and a preparation method thereof. The catalyst for preparing octanol comprises an active metal component and a carrier, the active metal component is one of Cu, Co and Ni; the carrier is one of Al2O3 (aluminum oxide), MgO (magnesium oxide), ZrO2 (zirconium oxide), TiO2 (titanium dioxide) and SiO2 (silicon dioxide The total weight of the catalyst is 100%, the active metal component accounts for 40-60 wt%, preferably 45-55 wt%, and the carrier accounts for 40-60 wt%, preferably 45-55 wt%; the catalyst is prepared in a rotary reinforced impregnation device. According to the preparation method disclosed by the invention, the dipping time of the metal active component can be greatly shortened, the metal active component can be more uniformly adsorbed on the surface of the carrier, the obtained catalyst is higher in dispersity and smaller in particle size, the breakage of the carrier is effectively avoided, the process is simple, and industrial production is easy to realize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysis, and more particularly to a catalyst for preparing octanol and a preparation method thereof. Background Art

[0002] Octenal is called 2-ethylhexenal. Since it is an α, β unsaturated aldehyde, it contains C=C double bond and C=O double bond in its molecule and can react with hydrogen. Since the bond energy of C=C bond is 615 kJ / mol and the bond energy of C=O bond is 715 kJ / mol, it is generally believed that C=C double bond is easier to hydrogenate than C=O double bond based on the data comparison of computational chemistry.

[0003] Due to the special properties of octenal itself, octenal will undergo primary hydrogenation and secondary hydrogenation processes during the reaction. During the primary hydrogenation process, octenal can selectively generate intermediate products octanal (2-ethyl-1-hexanal) and / or octenol (2-ethyl-2-hexen-1-ol). Both intermediate products can continue to react with hydrogen to eventually generate octanol.

[0004] Octanol, also known as 2-ethyl-1-hexanol (2-Ethylhexanol), is an important fine chemical raw material. It can be used to produce excellent and harmless plasticizers such as dioctyl adipate and dioctyl phthalate. It can also be widely used in the production of antioxidants, product adhesives, cosmetics, surfactants, etc. Another major use of octanol is the production of 2-ethylhexyl acrylate for coatings, adhesives, and inks. The use of 2-ethylhexyl nitrate as a diesel cetane improver additive, the use of 2-ethylhexyl phosphate as a lubricant additive, and other uses also highlight the commercial importance of octanol.

[0005] Chinese invention patent CN111068684A discloses a crude octanol liquid phase hydrogenation catalyst, which is a Ni-based catalyst, using catalytic cracking waste catalyst as raw material for pickling, crushing, sieving and other pretreatments, and then mixed with alumina glue, pore expander and binding agent to form a carrier, and then impregnated, dried, and roasted. This process is too cumbersome and is not conducive to operation. Chinese invention patent CN102407122A discloses a catalyst for preparing octanol by gas phase hydrogenation of octenal, which is a copper-zinc-aluminum catalyst, and is prepared by coprecipitation and cocurrent coprecipitation process and tableting, and the energy consumption of the reaction is too high, which is not conducive to energy saving and consumption reduction. When using microsphere catalyst, due to its own small particle size, high activity, the influence of external diffusion can be eliminated at the same time, and there is an advantage that the above-mentioned catalysts do not have.

[0006] In summary, it is particularly necessary to develop a catalyst with high conversion rate and green and environmentally friendly processing process. Summary of the invention

[0007] In order to solve the technical problems existing in the prior art, the present invention provides a catalyst for preparing octanol and a preparation method thereof.

[0008] The present invention utilizes the rotary strengthening technology, uses the rotary packed bed as the catalyst preparation equipment, and adopts the wire mesh or columnar packing. The impregnation liquid forms liquid mist and liquid droplets under the action of centrifugal force, and is sprayed on the surface of the carrier at a very high speed. The highly dispersed fine droplets, the extremely high initial velocity and the constantly updated phase interface can effectively improve the diffusion and penetration rate of the impregnation liquid in the pores of the carrier, promote the uniform adsorption of the active components on the surface of the carrier, greatly shorten the impregnation time, and finally, after drying and roasting, a catalyst with high dispersion of metal components and small average metal particle size is prepared, which can convert octenal into octanol.

[0009] One of the objects of the present invention is to provide a catalyst for preparing octanol.

[0010] The catalyst for preparing octanol comprises a carrier and an active metal component supported on the carrier; the active metal component is one of Cu, Co, and Ni, preferably Ni; the carrier is one of Al2O3, MgO, ZrO2, TiO2, and SiO2, preferably Al2O3;

[0011] Taking the total weight of the catalyst as 100%, the active metal component is 40-60wt%, and the carrier is 40-60wt%; preferably, the active metal component is 45-55wt%, and the carrier is 45-55wt%;

[0012] The catalyst is prepared by using a rotary enhanced impregnation device; the rotary enhanced impregnation device comprises a rotary enhanced packing bed, in which a carrier ring loaded with a carrier and a rotary packing are arranged, and the carrier ring is located outside the rotary packing; the carrier ring and the rotary packing can both rotate independently.

[0013] In a preferred embodiment of the present invention,

[0014] The precursor of the metal element in the active metal component is a soluble salt of the metal element, preferably at least one of the soluble salts of Cu, Co, and Ni, more preferably at least one of the nitrates, carbonates, and sulfates of Cu, Co, and Ni;

[0015] The specific surface area of ​​the carrier is 100 to 300 m 2 / g, pore volume is 0.5~1.5cm 3 / g, preferably, the specific surface area of ​​the carrier is 100 to 250m 2 / g, pore volume is 0.5~1.2cm 3 / g.

[0016] In a preferred embodiment of the present invention,

[0017] The rotary enhanced impregnation device also includes a liquid storage tank and a liquid pump. The rotary enhanced packing bed is a cylindrical structure and also includes a liquid distributor. The liquid distributor is located at the center of the rotary enhanced packing bed. Rotating packing and carrier rings are sequentially arranged on the periphery of the liquid distributor. The liquid pump is connected to the liquid storage tank to allow the impregnation liquid in the liquid storage tank to enter the liquid distributor through the impregnation liquid inlet. An impregnation liquid outlet is arranged at the lower end of the rotary enhanced packing bed.

[0018] In a preferred embodiment of the present invention,

[0019] The rotary intensified impregnation device further comprises a motor, preferably two motors, which are used to drive the carrier ring to rotate and the filler to rotate respectively;

[0020] The rotating packing is at least one of a wire mesh and a columnar packing, preferably at least one of a stainless steel wire mesh packing and a stainless steel columnar packing;

[0021] The carrier ring is a wire mesh carrier ring.

[0022] like Figure 1 As shown, the rotary enhanced impregnation device used in the present invention includes a motor 1, a motor 2, a rotary enhanced packing bed, a liquid storage tank, and a liquid pump. The rotary enhanced packing bed is a cylindrical structure, including a rotary packing and a carrier ring. The liquid distributor is located at the center of the rotary enhanced packing bed. Rotating packing and carrier rings are sequentially arranged on the periphery of the liquid distributor. The liquid pump allows the impregnation liquid in the liquid storage tank to enter the liquid distributor through the impregnation liquid inlet. An impregnation liquid outlet is arranged at the lower end of the rotary enhanced packing bed. The carrier ring is a wire mesh carrier ring. A certain amount of carrier particles are filled in the carrier ring according to actual needs. The rotary enhanced packing bed is provided with a liquid outlet at the lower end for discharging the liquid that has not been impregnated and returning it to the liquid storage tank. Among them, the carrier ring rotates at a low speed driven by motor 1, and the rotating filler rotates at a high speed driven by motor 2. The impregnation liquid is pumped into the impregnation device by a liquid pump, and is evenly sprayed into the inner side of the rotating filler through a liquid distributor. Under the action of centrifugal force, the mixed salt solution is sheared into tiny liquid elements by the rotating filler, and contacts with the alumina carrier in the carrier ring rotating at a low speed. The carrier is not filled in the carrier ring, and there will be a certain space to facilitate the rotation of the carrier. In this way, the solution can be impregnated at all angles of the carrier, so that the impregnation liquid can be evenly distributed on the carrier, and the catalyst precursor is obtained after a period of intensive impregnation.

[0023] A second object of the present invention is to provide a method for preparing a catalyst for preparing octanol, comprising the following steps:

[0024] (1) In the rotating enhanced impregnation device, the carrier is loaded into a rotatable carrier ring, and the soluble salt solution of the metal element is used as an impregnation liquid and sprayed into the inner side of the rotating filler. Under the action of centrifugal force, the impregnation liquid is sprayed on the rotating carrier to enhance the impregnation, and then a catalyst precursor is obtained, and then after drying and calcination, the catalyst is obtained;

[0025] Optionally, (2) repeat step (1).

[0026] During the rotary enhanced impregnation process, a soluble salt solution of metal elements is pumped into the rotary enhanced impregnation device and evenly sprayed into the inner side of the rotating filler through a liquid distributor. Under the action of centrifugal force, the salt solution is sheared into tiny liquid elements by the rotating filler, which come into contact with the carrier in the slow-rotating carrier ring, and the catalyst precursor is obtained by enhanced impregnation. The enhanced impregnation steps can be repeated, and the carrier can be subjected to multiple enhanced impregnations.

[0027] The preferred specific preparation steps are as follows:

[0028] (1) Impregnation step: After the carrier is treated, it is loaded into a wire mesh carrier ring. The impregnation liquid containing metal salts enters the rotary enhanced impregnation device through a pump and is evenly sprayed onto the inner edge of the rotating filler through a liquid distributor; under the action of high-speed centrifugal force, the impregnation liquid is sheared into tiny liquid microelements by the rotating filler and contacts the carrier in the carrier ring at an extremely high tangential initial velocity; the carrier ring rotates at a low speed to ensure that the carrier is fully in contact with the impregnation liquid microelements; the impregnated liquid returns to the liquid storage tank for liquid circulation, and after a certain impregnation time, a catalyst precursor is obtained; the impregnation operation can be repeated;

[0029] (2) Drying and calcining step: drying and calcining the catalyst precursor for decomposition;

[0030] (3) Steps (1) and (2) are optionally repeated according to the actual metal content requirement in the catalyst until the final catalyst is obtained.

[0031] In a preferred embodiment of the present invention,

[0032] The mass concentration of the soluble salt solution of the metal element is 35-80%, and the solvent is water, preferably deionized water;

[0033] The soluble salt solution of the metal element is sprayed into the inner side of the rotating filler through a liquid distributor, and the liquid inlet flow rate of the liquid distributor is 1 to 50 ml / min, preferably 5 to 10 ml / min.

[0034] In a preferred embodiment of the present invention,

[0035] The rotating speed of the rotating filler is 1000-2000 rpm;

[0036] The rotation speed of the carrier ring is 10 to 20 rpm;

[0037] The rotating filler and the carrier ring can rotate in the same direction or in opposite directions, as long as the rotating filler rotates at a high speed and the carrier ring rotates at a low speed;

[0038] The time of the enhanced impregnation is 10 to 30 minutes;

[0039] The drying condition is drying at 100-120°C for 2-10 hours, preferably drying for 3-5 hours;

[0040] The calcination conditions are calcination at 300-600° C. for 2-10 hours, preferably calcination at 350-500° C. for 4-8 hours.

[0041] The third object of the present invention is to provide a catalyst for preparing octanol obtained by the above method.

[0042] The catalyst obtained by the preparation method provided by the present invention is subjected to reduction treatment to partially reduce the oxide to active metal, thereby obtaining a catalyst with high metal component dispersion and small average particle size, for example, the metal dispersion is 0.5-5% and the metal particle size is 10-100nm.

[0043] A fourth object of the present invention is to provide a method for preparing octanol, comprising:

[0044] Octenal and hydrogen are used as raw materials and reacted under liquid phase reaction conditions to generate octanol under the action of the catalyst.

[0045] In a preferred embodiment of the present invention,

[0046] The reaction temperature is 100-150°C;

[0047] The reaction pressure is 3-5 MPa;

[0048] Reaction space velocity is 1-3h -1 ;

[0049] The solvent is an alcohol solvent, preferably a monohydric alcohol having 2 to 8 carbon atoms, more preferably ethanol or octanol;

[0050] The mass ratio of the octenal to the solvent is 1:(2-6).

[0051] Compared with the prior art, the present invention has the following beneficial effects:

[0052] The rotating packed bed of the present invention is a chemical intensification device that can highly intensify microscopic mixing and mass transfer. In a hypergravity environment, the huge shear force generated by the rotation of the rotating packing can shear the fluid into very small liquid microelements, increase the contact area of ​​the physical phases, greatly improve the mixing and mass transfer effects between the phases, and increase the mass transfer coefficient by 10 to 1000 times compared with conventional reactors; therefore, the use of the rotating intensified impregnation method of the present invention can improve the dispersion of catalytic active components and improve catalytic performance.

[0053] The present invention utilizes the rotary strengthening technology, uses the rotary packed bed as the catalyst preparation equipment, and adopts the wire mesh or columnar packing. The impregnation liquid forms liquid mist and liquid droplets under the action of centrifugal force, and is sprayed on the surface of the carrier at a very high speed. The highly dispersed fine droplets, the extremely high initial velocity and the constantly updated phase interface can effectively improve the diffusion and penetration rate of the impregnation liquid in the pores of the carrier, promote the uniform adsorption of the active components on the surface of the carrier, greatly shorten the impregnation time, and finally, after drying and roasting, a catalyst with high dispersion of metal components and small average metal particle size is prepared.

[0054] The preparation method provided by the present invention greatly shortens the impregnation time of the metal active component, and the metal active component can be more evenly adsorbed on the surface of the carrier; at the same time, the carrier ring is equipped with a wire mesh, which can wrap the carrier to prevent the carrier from being damaged;

[0055] The catalyst prepared by the preparation method of the present invention has higher dispersion and smaller particle size;

[0056] The catalyst prepared by the present invention has a high content of metal active components and is suitable for use as a catalyst for preparing octanol.

[0057] The preparation method provided by the invention effectively avoids the breakage of the carrier, has a simple process, is easy to realize industrial production, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 It is a schematic diagram of the rotary enhanced impregnation equipment;

[0059] In the figure: 1-1 is motor 1, 1-2 is motor 2, 1-3 is a rotating reinforced packing bed, 1-4 is a liquid storage tank, 1-5 is a liquid pump, 1-6 is a liquid distributor, 1-7 is a rotating packing, 1-8 is a wire mesh carrier ring, 1-9 is an alumina carrier, 1-10 is an impregnation liquid inlet, and 1-11 is an impregnation liquid outlet;

[0060] Figure 2 It is a side view schematic diagram of the internal structure of the rotary enhanced impregnation equipment;

[0061] In the figure: 1-12 is the wire mesh carrier ring gear, 1-3 is the rotating reinforced filler bed, 1-8 is the wire mesh carrier ring, 1-9 is the alumina carrier, 1-7 is the rotating filler, 1-6 is the liquid distributor, and 1-11 is the impregnation liquid outlet. DETAILED DESCRIPTION

[0062] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.

[0063] The test instruments and test conditions used in the examples are as follows:

[0064] The specific surface area (BET) and pore volume of the catalyst were measured by N2 adsorption-desorption method.

[0065] The dispersion and average particle size of the active components in the catalyst were measured by hydrogen chemisorption.

[0066] The sources of raw materials used in the examples are as follows:

[0067] All reagents used were commercially available and of analytical grade.

[0068] The rotary impregnation device used in the embodiment is as follows Figure 1 As shown in, it includes: a motor 1 (1-1), a motor 2 (1-2), a rotating reinforced packing bed 1-3, a liquid storage tank 1-4, a liquid pump 1-5, and the rotating reinforced packing bed 1-3 is a cylindrical structure, including a liquid distributor 1-6, a rotating packing 1-7 and a wire mesh carrier ring 1-8. The liquid distributor 1-6 is located at the center of the rotating reinforced packing bed 1-3. One end of the liquid distributor 1-6 is closed, and the other end is provided with a pipeline opening 1-10 connected to the liquid pump 1-5 through a pipeline. Rotating packing 1-7 and a wire mesh carrier ring 1-8 are sequentially arranged on the periphery of the liquid distributor 1-6. The lower end of the rotating reinforced packing bed 1-3 is provided with a liquid outlet 1-11 for discharging the unimpregnated liquid and returning it to the liquid storage tank 1-4. Among them, the wire mesh carrier ring 1-8 is filled with alumina carrier 1-9, and the rotating filler 1-7 adopts stainless steel wire mesh filler. The motor 1 drives the carrier ring 1-8 to rotate at a low speed, and the motor 2 drives the rotating filler 1-7 to rotate at a high speed. The impregnation liquid is pumped into the impregnation device by the liquid pump 1-5, and is evenly sprayed into the inner side of the rotating filler 1-7 through the liquid distributor 1-6. Under the action of centrifugal force, the impregnation liquid is sheared into tiny liquid elements by the rotating filler 1-7, and contacts with the alumina carrier 1-9 in the slow-rotating carrier ring 1-8. After a period of intensive impregnation, a catalyst precursor is obtained.

[0069] Figure 2 for Figure 2 It is a side view of the internal structure of the rotary intensified impregnation equipment, where 1-12 is the wire mesh carrier ring gear, and the other parts are the same as Figure 1 The names are the same as those in the annotations.

[0070] Example 1

[0071] Using the rotary enhanced impregnation method, 50g of the shaped Al2O3 carrier (BET specific surface area of ​​159m 2 / g, pore volume is 0.79cm 3 / g) is loaded into a wire mesh carrier ring, an impregnation solution containing nickel nitrate (mass concentration is 78%) is placed in a liquid tank, the rotating packed bed is started, the speed of the packed bed is 1500rpm, the speed of the carrier ring is 10rpm, the impregnation solution is pumped into the rotating bed through a horizontal flow pump, the liquid inlet flow rate of the liquid distributor is 5ml / min, after 20min of intensive impregnation, the catalyst precursor is taken out, and then dried at 120°C for 3h and calcined at 400°C for 4h, finally a catalyst with a Ni content of 45wt% and an Al2O3 carrier content of 55wt% is obtained.

[0072] Example 2

[0073] Using the rotary enhanced impregnation method, 50g of the shaped SiO2 carrier (BET specific surface area of ​​112m 2 / g, pore volume is 0.58cm 3 / g) is loaded into a wire mesh carrier ring, an impregnation solution containing copper nitrate (mass concentration of 40%) is placed in a liquid tank, the rotating packed bed is started, the speed of the packed bed is 2000rpm, the speed of the carrier ring is 15rpm, the impregnation solution is pumped into the rotating bed through a horizontal flow pump, the liquid inlet flow rate of the liquid distributor is 10ml / min, after 30min of intensive impregnation, the catalyst precursor is taken out, and then dried at 110°C for 5h and calcined at 350°C for 7h, finally, a catalyst with a Cu content of 50wt% and a SiO2 carrier content of 50wt% is obtained.

[0074] Example 3

[0075] Using the rotary enhanced impregnation method, 50g of the shaped TiO2 carrier (BET specific surface area of ​​225m 2 / g, pore volume is 1.04cm 3 / g) is loaded into a wire mesh carrier ring, an impregnation solution containing cobalt nitrate (mass concentration of 55%) is placed in a liquid tank, the rotating packed bed is started, the speed of the packed bed is 1000rpm, the speed of the carrier ring is 10rpm, the impregnation solution is pumped into the rotating bed through a horizontal flow pump, the liquid inlet flow rate of the liquid distributor is 8ml / min, after 15min of intensive impregnation, the catalyst precursor is taken out, and then dried at 100°C for 5h and calcined at 500°C for 8h, finally a catalyst with a Co content of 55wt% and a TiO2 carrier content of 45wt% is obtained.

[0076] Example 4

[0077] 10 ml of the catalyst obtained in Example 1 was loaded into a stainless steel fixed bed reactor, and high-purity N2 was introduced at a flow rate of 300 mL / min. The temperature was raised to 120°C, and the high-purity N2 was switched to H2 at a flow rate of 200 mL / min. The temperature was raised to 400-450°C and maintained for 4 h to reduce the catalyst, and then the temperature was slowly lowered to room temperature. The reactor was opened to unload the catalyst, and 1 g of the reduced catalyst was placed in a reactor. In the presence of 20 g of the reaction raw materials (the mass ratio of octenal to octanol was 1:3), the reaction temperature was 120°C, the reaction pressure was 4 MPa, and the reaction space velocity was 2 h -1 The reaction is carried out to prepare octanol.

[0078] Example 5

[0079] The difference from Example 4 is that the catalyst is replaced by the catalyst obtained in Example 2;

[0080] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 4 to prepare octanol.

[0081] Example 6

[0082] In addition to the above differences, the differences from Example 4 are: the catalyst is replaced by the catalyst obtained in Example 3;

[0083] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 4 to prepare octanol.

[0084] Example 7

[0085] The difference from Example 4 is that the mass ratio of octenal to octanol is 1:2, the reaction temperature is 100°C, the reaction pressure is 5 MPa, and the reaction space velocity is 1 h -1 ;

[0086] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 4 to prepare octanol.

[0087] Example 8

[0088] The difference from Example 7 is that the catalyst is replaced by the catalyst obtained in Example 2;

[0089] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 7 to prepare octanol.

[0090] Example 9

[0091] The difference from Example 7 is that the catalyst is replaced by the catalyst obtained in Example 3;

[0092] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 7 to prepare octanol.

[0093] Example 10

[0094] The difference from Example 4 is that the mass ratio of octenal to octanol is 1:6, the reaction temperature is 150°C, the reaction pressure is 3 MPa, and the reaction space velocity is 3 h -1 ;

[0095] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 4 to prepare octanol.

[0096] Embodiment 11

[0097] The difference from Example 10 is that the catalyst is replaced by the catalyst obtained in Example 2;

[0098] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 10 to prepare octanol.

[0099] Example 12

[0100] The difference from Example 10 is that the catalyst is replaced by the catalyst obtained in Example 3;

[0101] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 10 to prepare octanol.

[0102] Comparative Example 1

[0103] Using the traditional impregnation method, 50 g of the shaped Al2O3 carrier (BET specific surface area of ​​159 m 2 / g, pore volume is 0.79cm 3 / g), and impregnated with nickel nitrate solution by equal volume impregnation method. After 20 minutes of impregnation, the catalyst precursor was taken out, and then dried at 120°C for 3 hours and calcined at 400°C for 4 hours to finally obtain a catalyst with a Ni content of 45wt%.

[0104] Comparative Example 2

[0105] The difference from Example 4 is that the catalyst is replaced by the catalyst obtained in Comparative Example 1;

[0106] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 4 to prepare octanol.

[0107] Comparative Example 3

[0108] The difference from Example 7 is that the catalyst is replaced by the catalyst obtained in Comparative Example 1;

[0109] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 7 to prepare octanol.

[0110] Comparative Example 4

[0111] The difference from Example 10 is that the catalyst is replaced by the catalyst obtained in Comparative Example 1;

[0112] Except for the above differences, other raw materials, amounts and processes are the same as those in Example 10 to prepare octanol.

[0113] According to the above evaluation method, the catalysts prepared in Examples 1 to 3 and Comparative Example 1 were evaluated for reaction, and Table 1 shows the detailed evaluation results.

[0114] Table 1 BET characterization results and reaction evaluation results of catalysts

[0115]

[0116] Compared with Comparative Example 1, the nickel dispersion of the prepared catalyst in Example 1 increases from 0.94% to 2.58%, and the nickel particle size increases from 87.5nm to 35.8nm, which proves that the rotary enhanced impregnation method of the present invention can improve the dispersion of the catalytically active components while reducing their particle size, thereby obtaining a catalyst with higher metal dispersion and smaller metal particle size, which is more conducive to the reaction and has better catalytic performance.

[0117] Compared with Comparative Example 2, the conversion rate of octenal in Example 4 increases from 84% to 95%, and the yield of octanol increases from 80% to 90%;

[0118] Compared with Comparative Example 3, the conversion rate of octenal in Example 7 increased from 81% to 90%, and the yield of octanol increased from 80% to 85%.

[0119] Compared with Comparative Example 4, the conversion rate of octenal in Example 10 increased from 85% to 96%, and the yield of octanol increased from 87% to 92%.

[0120] Compared with the corresponding comparative examples, the octenal conversion rate of the above embodiments is increased by about 10%, and the octanol yield is increased by about 5-10%. Under the condition of high base conversion rate, a significant improvement is still achieved.

[0121] In Examples 4 to 12, octanol was prepared using the catalysts prepared in Examples 1 to 3, respectively. The octenal conversion rate was 84 to 96%, and the octanol yield was 81 to 92%, which confirmed that the catalyst prepared in the present invention had a high conversion rate for preparing octanol and good catalytic performance.

Claims

1. A catalyst for preparing octanol, comprising a carrier and an active metal component supported on the carrier; the active metal component is one of Cu, Co, and Ni; the carrier is Al 2 O 3 、MgO、ZrO 2 、TiO 2 、SiO 2 One of; Taking the total weight of the catalyst as 100%, the active metal component is 40-60wt%, and the carrier is 40-60wt%; preferably, the active metal component is 45-55wt%, and the carrier is 45-55wt%; The catalyst is prepared by using a rotary enhanced impregnation device; the rotary enhanced impregnation device comprises a rotary enhanced packing bed, in which a carrier ring loaded with a carrier and a rotary packing are arranged, and the carrier ring is located outside the rotary packing; the carrier ring and the rotary packing can both rotate independently.

2. The catalyst according to claim 1, Features: The precursor of the metal element in the active metal component is a soluble salt of the metal element, preferably at least one of the soluble salts of Cu, Co, and Ni, more preferably at least one of the nitrates, carbonates, and sulfates of Cu, Co, and Ni; and / or, The specific surface area of ​​the carrier is 100 to 300 m 2 / g, pore volume is 0.5~1.5cm 3 / g, preferably, the specific surface area of ​​the carrier is 100 to 250m 2 / g, pore volume is 0.5~1.2cm 3 / g.

3. The catalyst according to claim 1, Features: The rotary enhanced impregnation device also includes a liquid storage tank and a liquid pump. The rotary enhanced packing bed is a cylindrical structure and also includes a liquid distributor. The liquid distributor is located at the center of the rotary enhanced packing bed. Rotating packing and carrier rings are sequentially arranged on the periphery of the liquid distributor. The liquid pump is connected to the liquid storage tank to allow the impregnation liquid in the liquid storage tank to enter the liquid distributor through the impregnation liquid inlet. An impregnation liquid outlet is arranged at the lower end of the rotary enhanced packing bed.

4. The catalyst according to claim 1, Features: The rotary intensified impregnation device further comprises a motor, preferably two motors, which are used to drive the carrier ring to rotate and the filler to rotate respectively; and / or, The rotating packing is at least one of a wire mesh and a columnar packing, preferably at least one of a stainless steel wire mesh packing and a stainless steel columnar packing; and / or, The carrier ring is a wire mesh carrier ring.

5. A method for preparing a catalyst for preparing octanol as claimed in any one of claims 1 to 4, The following steps are involved: (1) In the rotating enhanced impregnation device, the carrier is loaded into a rotatable carrier ring, and the soluble salt solution of the metal element is used as an impregnation liquid and sprayed into the inner side of the rotating filler. Under the action of centrifugal force, the impregnation liquid is sprayed on the rotating carrier to enhance the impregnation, and then a catalyst precursor is obtained, and then after drying and calcination, the catalyst is obtained; Optionally, (2) repeat step (1).

6. The method for preparing the catalyst according to claim 5, Features: The mass concentration of the soluble salt solution of the metal element is 35-80%, and the solvent is water, preferably deionized water; and / or, The soluble salt solution of the metal element is sprayed into the inner side of the rotating filler through a liquid distributor, and the liquid inlet flow rate of the liquid distributor is 1 to 50 ml / min, preferably 5 to 10 ml / min.

7. The method for preparing the catalyst according to claim 5, Features: The rotating speed of the rotating filler is 1000-2000 rpm; and / or, The rotation speed of the carrier ring is 10-20 rpm; and / or, The time of the enhanced impregnation is 10 to 30 minutes; and / or, The drying condition is drying at 100-120° C. for 2-10 hours, preferably drying for 3-5 hours; and / or, The calcination conditions are calcination at 300-600° C. for 2-10 hours, preferably calcination at 350-500° C. for 4-8 hours.

8. A catalyst obtained by the preparation method according to any one of claims 5 to 7.

9. A method for preparing octanol using the catalyst according to any one of claims 1 to 4 or 8, wherein the method include: Octenal and hydrogen are used as raw materials, and a reaction is carried out in a solvent under the action of the catalyst to prepare the octanol.

10. The method for preparing octanol as claimed in claim 9, Features: The reaction temperature is 100-150°C; and / or, The reaction pressure is 3-5 MPa; and / or, Reaction space velocity is 1~3h -1 and / or, The solvent is an alcohol solvent, preferably a monohydric alcohol having 2 to 8 carbon atoms, more preferably ethanol or octanol; and / or, The mass ratio of the octenal to the solvent is 1:(2-6).

Citation Information

Patent Citations

  • Preparation method of octylene aldehyde gas phase hydrogenation catalyst for octanol production

    CN102407122A

  • Crude octanol liquid phase hydrogenation catalyst and preparation method thereof

    CN111068684A