Ce perovskite catalyst, preparation method and application of Ce perovskite catalyst in conversion of CO2
Patent Information
- Application Number
- CN202411126698.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
[0005]鉴于上述现有技术的不足之处,本发明的目的在于提供一种Ce系钙钛矿催化剂、制备方法及其在转化CO2中的应用,旨在解决现有技术中传统催化剂存在的稳定性差、难以分离、无法循环使用的问题
(1)本发明相比传统催化剂具有更多的金属氧空位,能有有效的与反应过程中产生的水结合,可提高反应物转化率,增强催化活性、反应选择性。
Smart Images

Figure CN119016058A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalyst technology, and in particular to a Ce-based perovskite catalyst, a preparation method and its application in converting CO 2 Application in. Background Art
[0002] As human use of natural gas and oil increases, CO 2 The increasing emissions and the resulting "greenhouse effect" have attracted widespread global attention. Since carbon dioxide is an abundant, non-toxic, non-flammable and cheap carbon source, the direct synthesis of chemicals and fuels from carbon dioxide has attracted great interest.
[0003] Currently, CO 2 Cycloaddition with epoxides has been the most studied due to its green process, and a variety of effective catalysts have been reported. However, the problem with this process is that epoxides are highly reactive, low boiling, flammable and explosive, requiring special synthesis process technology and storage and handling requirements. 2 Carboxylation is considered a green alternative, as the reaction produces only water and the diols can be produced from biomass, which is renewable. Therefore, the process route to carbonates using diols is very attractive.
[0004] The direct use of aliphatic diols and carbon dioxide to synthesize cyclic carbonates is very unfavorable in terms of thermodynamics and kinetics, and requires higher reaction temperature, pressure and additives to induce the equilibrium to shift to the formation of the target product. In industry, alcohols are often oxidized and carbonylated by phosgenation, but the toxicity of phosgene and the large amount of chlorinated waste generated during the reaction have limitations on safe transportation and green production; in this case, the formation of cyclic carbonates by coupling aliphatic diols and carbon dioxide is more advantageous, but the existing catalysts still have problems such as catalyst hydrolysis, poor stability, difficulty in separation, and inability to recycle due to their own structural properties. Therefore, the existing technology needs to be improved and enhanced. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a Ce-based perovskite catalyst, a preparation method and its application in the conversion of CO 2 The application of this technology is aimed at solving the problems of poor stability, difficulty in separation and inability to recycle of traditional catalysts in the existing technology.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions: In the first aspect, a Ce-based perovskite catalyst, chemical name: Ce x Mg (1-x) Zn yCu (1-y) O 3 where 0 < x < 1; 0 < y < 1. In the high-temperature variant structure, the B-site ions (Zn; Cu) form octahedral coordination with six oxygen ions, and the A-site ions (Ce; Mg) are located in the cavities formed by these octahedra.
[0007] Second aspect, a method for preparing a Ce-based perovskite catalyst as described above, comprising: Step 1: Mix cerium nitrate hexahydrate, magnesium nitrate hexahydrate, zinc nitrate hexahydrate, copper nitrate trihydrate, citric acid, and malic acid and add them to an ethylene glycol solution, mix and stir for 2 - 3 h until uniform to obtain a mixed solution; Step 2: Heat the mixed solution at 140 °C, dry it at 200 - 210 °C for 8 - 12 h to dry the water and excess ethylene glycol therein, and let it stand at room temperature for 1 - 2 h to obtain a dried mixed gel; Step 3: Put the dried sol-gel into a muffle furnace and calcine it at 700 °C for 4 h to obtain a Ce-based perovskite catalyst Ce x Mg (1-x) Zn y Cu (1-y) O 3 .
[0008] Further, in Step 1, the molar ratio of cerium nitrate hexahydrate, magnesium nitrate hexahydrate, zinc nitrate hexahydrate, and copper nitrate trihydrate is preferably x: 1 - x: y: 1 - y.
[0009] Further, in Step 1, the molar ratio of nitrate, citric acid, and malic acid is preferably 1: 0.5: 0.5.
[0010] Further, in Step 2, the excess ethylene glycol in the mixed solution is removed to obtain a mild gel.
[0011] Further, in Step 3, high-temperature calcination removes the organic ligands to obtain Ce x Mg (1-x) Zn y Cu (1-y) O 3 perovskite catalyst.
[0012] Third aspect, the application of the Ce-based perovskite catalyst in the conversion of CO 2 is mainly used for catalyzing the synthesis of cyclic carbonates from aliphatic diols and CO 2 .
[0013] Among them, the aliphatic diol is one of ethylene glycol, 1,2-propanediol, and 1,3-propanediol.
[0014] The technical solution adopted by the present invention has the following beneficial effects: (1) Compared with traditional catalysts, the present invention has more metal oxygen vacancies, which can effectively combine with the water generated during the reaction process, improve the conversion rate of reactants, and enhance catalytic activity and reaction selectivity.
[0015] (2) The catalyst system is based on metal oxides, which are solids at room temperature, not easily combustible, non-explosive, and non-oxidizing, and have good thermal stability and chemical stability. Description of the Drawings
[0016] Figure 1 It is the Fourier infrared spectrum of the catalyst prepared in Example 3; Figure 2 It is the X-ray diffractometer diagram of the catalyst prepared in Example 3; Figure 3 It is the scanning electron microscope diagram of the catalyst prepared in Example 3; Figure 4 It is the chemical structural formula of a Ce-based perovskite catalyst provided by the present invention. Specific Embodiments
[0017] To make the purpose, technical solution and effects of the present invention clearer and more definite, the following further elaborates on the present invention with reference to the accompanying drawings and by way of examples. It should be understood that the specific examples described herein are only used to explain the present invention and are not used to limit the present invention.
[0018] First aspect, a Ce-based perovskite catalyst, the structural general formula is: Ce x Mg (1-x) Zn y Cu (1-y) O 3 , where 0 < x < 1; 0 < y < 1. In the high-temperature variant structure, the B-site ions (Zn; Cu) form octahedral coordination with six oxygen ions, and the A-site ions (Ce; Mg) are located in the holes formed by these octahedra.
[0019] The chemical formula can be seen in Figure 4 , Figure 4 where A = Ce, Mg; B = Zn, Cu.
[0020] Second aspect, a preparation method of a Ce-based perovskite catalyst, including: Step 1: Mix cerium nitrate hexahydrate, magnesium nitrate hexahydrate, zinc nitrate hexahydrate, copper nitrate trihydrate, citric acid and malic acid and add them to an ethylene glycol solution, mix and stir for 2 - 3 h until uniform to obtain a mixed solution; the molar ratio of cerium nitrate hexahydrate, magnesium nitrate hexahydrate, zinc nitrate hexahydrate, copper nitrate trihydrate is preferably x: 1 - x: y: 1 - y; the molar ratio of nitrate, citric acid, malic acid is preferably 1: 0.5: 0.5.
[0021] Step 2: heating the mixed solution to 140°C, drying at 200-210°C for 8-12h, drying the water and excess ethylene glycol, removing the excess ethylene glycol in the mixed solution to obtain a moderate gel, and standing at room temperature for 1-2h to obtain a dried mixed gel; Step 3: Place the dried sol-gel in a muffle furnace and calcine at 700°C for 4 hours to remove the organic ligands and obtain the Ce-based perovskite catalyst Ce. x Mg (1-x) Zn y Cu (1-y) O 3 .
[0022] Application of Ce-based perovskite catalysts, mainly used for catalytic conversion of fatty glycols to CO 2 Synthesize cyclic carbonate; wherein the aliphatic diol is one of ethylene glycol, 1,2-propylene glycol and 1,3-propylene glycol.
[0023] The molar ratio of cerium nitrate hexahydrate, magnesium nitrate hexahydrate, zinc nitrate hexahydrate and copper nitrate trihydrate in step 1 is preferably x:1-x:y:1-y. By adjusting the metal ratio, metal oxygen vacancies are increased and the catalytic activity is improved.
[0024] The purpose of drying excess ethylene glycol in step 2 to obtain a moderate gel is to prevent the generation of a large amount of gas during the calcination process in step 3.
[0025] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments.
[0026] The present invention adopts Ce x Mg (1-x) Zn y Cu (1-y) O 3 Perovskite catalysts for catalytic conversion of ethylene glycol to CO 2 Cyclic carbonate is formed, and the prepared metal Ce x Mg (1-x) Zn y Cu (1-y) O 3 It has the characteristics of stable chemical structure, large specific surface area, abundant oxygen vacancies, and effective binding of water produced during the reaction to promote the forward reaction. In addition, the multi-metal in the perovskite structure has a synergistic catalytic effect and has both acid and base active sites, which can further improve the catalytic activity. To a certain extent, it overcomes the phenomenon of low catalyst activity and selectivity, and the catalyst is conducive to recovery and recycling.
[0027] The present invention uses citric acid, malic acid and ethylene glycol to undergo an esterification reaction, thereby making the metal ions more dispersed, which is conducive to the formation of a perovskite structure; on the other hand, the open metal active sites in the perovskite can activate the C=O bond of carbon dioxide, which is conducive to the coupling of carbon dioxide; in addition, the oxygen vacancies in the catalyst structure can form a complex with the oxygen atoms of ethylene glycol, thereby activating ethylene glycol; therefore, the perovskite formed by multiple metal atoms synergistically catalyzes CO 2 Synthesize ethylene carbonate with ethylene glycol to prepare Ce x Mg (1-x) Zn y Cu (1-y) O 3 Perovskite catalysts for the catalysis of aliphatic diols and CO 2 Cyclic carbonate is generated. The catalyst has stable structural properties, can effectively combine with water produced during the reaction, promote the forward progress of the reaction, has high catalytic efficiency, good recycling performance, and has good industrial application prospects.
[0028] Example 1 (1) Preparation of Ce 0.5 Mg 0.5 Zn 0.8 Cu 0.2 O 3 Perovskite precursor solution 0.01 mol of cerium nitrate hexahydrate, 0.01 mol of magnesium nitrate hexahydrate, 0.016 mol of zinc nitrate hexahydrate, 0.004 mol of copper nitrate trihydrate, 0.02 mol of citric acid and 0.02 mol of malic acid were dissolved in 40 ml of ethylene glycol solution according to the molar ratio and stirred at 140° C. for 2 hours to obtain a perovskite precursor mixed solution.
[0029] (2) Preparation of Ce 0.5 Mg 0.5 Zn 0.8 Cu 0.2 O 3 Perovskite precursor gel The mixed solution of the perovskite precursor in a beaker was placed in an oven at 210° C. for 12 h to remove excess solvent. After naturally cooling to room temperature, the perovskite precursor gel was obtained.
[0030] (3) Preparation of Ce 0.5 Mg 0.5 Zn 0.8 Cu 0.2 O 3 Perovskite The perovskite precursor gel was placed in a crucible in a muffle furnace and calcined at 700 °C for 4 h. Ce was obtained after cooling to room temperature. 0.5 Mg 0.5 Zn 0.8 Cu0.2 O 3 Perovskite catalysts.
[0031] Example 2 (1) Preparation of Ce 0.5 Mg 0.5 Zn 0.2 Cu 0.8 O 3 Perovskite precursor solution 0.01 mol of cerium nitrate hexahydrate, 0.01 mol of magnesium nitrate hexahydrate, 0.004 mol of zinc nitrate hexahydrate, 0.016 mol of copper nitrate trihydrate, 0.02 mol of citric acid and 0.02 mol of malic acid were dissolved in 40 ml of ethylene glycol solution according to the molar ratio and stirred at 140° C. for 2 hours to obtain a perovskite precursor mixed solution.
[0032] (2) Preparation of Ce 0.5 Mg 0.5 Zn 0.2 Cu 0.8 O 3 Perovskite precursor gel The mixed solution of the perovskite precursor in a beaker was placed in an oven at 210° C. for 12 h to remove excess solvent. After naturally cooling to room temperature, the perovskite precursor gel was obtained.
[0033] (3) Preparation of Ce 0.5 Mg 0.5 Zn 0.2 Cu 0.8 O 3 Perovskite The perovskite precursor gel was placed in a muffle furnace using a crucible and calcined at 700 °C for 4 h. Ce was obtained after cooling to room temperature. 0.5 Mg 0.5 Zn 0.2 Cu 0.8 O 3 Perovskite catalysts.
[0034] Example 3 (1) Preparation of Ce 0.5 Mg 0.5 Zn 0.5 Cu 0.5 O 3 Perovskite precursor solution 0.01 mol of cerium nitrate hexahydrate, 0.01 mol of magnesium nitrate hexahydrate, 0.01 mol of zinc nitrate hexahydrate, 0.01 mol of copper nitrate trihydrate, 0.02 mol of citric acid and 0.02 mol of malic acid were dissolved in 40 ml of ethylene glycol solution according to the molar ratio and stirred at 140° C. for 2 hours to obtain a perovskite precursor mixed solution.
[0035] (2) Preparation of Ce0.5 Mg 0.5 Zn 0.5 Cu 0.5 O 3 Perovskite precursor gel The mixed solution of the perovskite precursor in a beaker was placed in an oven at 210° C. for 12 h to remove excess solvent. After naturally cooling to room temperature, the perovskite precursor gel was obtained.
[0036] (3) Preparation of Ce 0.5 Mg 0.5 Zn 0.5 Cu 0.5 O 3 Perovskite The perovskite precursor gel was placed in a crucible in a muffle furnace and calcined at 700 °C for 4 h. Ce was obtained after cooling to room temperature. 0.5 Mg 0.5 Zn 0.5 Cu 0.5 O 3 Perovskite catalysts.
[0037] Example 4 (1) Preparation of Ce 0.2 Mg 0.8 Zn 0.5 Cu 0.5 O 3 Perovskite precursor solution 0.04 mol of cerium nitrate hexahydrate, 0.016 mol of magnesium nitrate hexahydrate, 0.01 mol of zinc nitrate hexahydrate, 0.01 mol of copper nitrate trihydrate, 0.02 mol of citric acid and 0.02 mol of malic acid were dissolved in 40 ml of ethylene glycol solution according to the molar ratio and stirred at 140° C. for 2 hours to obtain a perovskite precursor mixed solution.
[0038] (2) Preparation of Ce 0.2 Mg 0.8 Zn 0.5 Cu 0.5 O 3 Perovskite precursor gel The mixed solution of the perovskite precursor in a beaker was placed in an oven at 210° C. for 12 h to remove excess solvent. After naturally cooling to room temperature, the perovskite precursor gel was obtained.
[0039] (3) Preparation of Ce 0.2 Mg 0.8 Zn 0.5 Cu 0.5 O 3 Perovskite The perovskite precursor gel was placed in a crucible in a muffle furnace and calcined at 700 °C for 4 h. Ce was obtained after cooling to room temperature. 0.2 Mg 0.8Zn 0.5 Cu 0.5 O 3 Perovskite catalysts.
[0040] Example 5 (1) Preparation of Ce 0.8 Mg 0.2 Zn 0.5 Cu 0.5 O 3 Perovskite precursor solution 0.01 mol of cerium nitrate hexahydrate, 0.01 mol of magnesium nitrate hexahydrate, 0.01 mol of zinc nitrate hexahydrate, 0.01 mol of copper nitrate trihydrate, 0.02 mol of citric acid and 0.02 mol of malic acid were dissolved in 40 ml of ethylene glycol solution according to the molar ratio and stirred at 140° C. for 2 hours to obtain a perovskite precursor mixed solution.
[0041] (2) Preparation of Ce 0.8 Mg 0.2 Zn 0.5 Cu 0.5 O 3 Perovskite precursor gel The mixed solution of the perovskite precursor in a beaker was placed in an oven at 210° C. for 12 h to remove excess solvent. After naturally cooling to room temperature, the perovskite precursor gel was obtained.
[0042] (3) Preparation of Ce 0.8 Mg 0.2 Zn 0.5 Cu 0.5 O 3 Perovskite The perovskite precursor gel was placed in a crucible in a muffle furnace and calcined at 700 °C for 4 h. Ce was obtained after cooling to room temperature. 0.8 Mg 0.2 Zn 0.5 Cu 0.5 O 3 Perovskite catalysts.
[0043] The perovskite catalyst prepared above was used to catalyze the reaction of ethylene glycol and CO 2 The reaction synthesizes ethylene carbonate.
[0044] The catalytic experimental conditions are: The catalysts prepared in Examples 1-5 were respectively used in a kettle reactor to catalyze CO 2Synthesize ethylene carbonate with ethylene glycol. The amount of catalyst is 5% of the total mass of the raw materials, ethylene glycol 50ml, di-cyanopyridine 20ml, the reactor temperature is 120℃, and the pressure is 3.5Mpa for 24h. After the reaction is completed, the vacuum distillation is carried out, and the residual heavy component is the perovskite catalyst. The distillate is used to determine the product purity by gas chromatography, and finally the conversion rate, selectivity and yield are calculated.
[0045] The traditional catalyst CeO 2 , triethylamine and zinc bromide, 1,8-diazabicycloundec-7-ene (DBU), were used to catalyze the reaction of aliphatic diols (ethylene glycol) and CO 2 The catalytic process conditions and process for synthesizing ethylene carbonate were the same as those described above. The effects of different catalyst types on the catalytic performance were investigated, and the catalytic results are shown in Table 1.
[0046] Table 1 Effect of different catalysts on catalytic performance catalyst Conversion rate / % Selectivity / % Yield / % <![CDATA[CeO 2 ]]> 2.35 83.56 1.96 Triethylamine, zinc bromide 6.45 56.78 3.66 DBU, triethylamine 5.38 69.16 3.72 Example 1 14.45 91.39 13.21 Example 2 13.25 90.69 12.02 Example 3 18.18 92.19 16.76 Example 4 14.57 90.65 13.21 Example 5 16.78 91.54 15.36 From the data in Table 1, it can be seen that the catalytic effect of perovskite catalysts in synthesizing ethylene carbonate is better than that of CeO 2 , DBU, triethylamine and zinc bromide, especially Example 3 (Ce 0.5 Mg 0.5 Zn 0.5 Cu 0.5 O 3 ) has the best catalytic effect, with an ethylene glycol conversion rate of 18.18% and an ethylene carbonate selectivity of 92.19%.
[0047] Example 6 Ce 0.5 Mg 0.5 Zn 0.5 Cu 0.5 O 3 Taking perovskite catalyst as an example, it catalyzes the reaction of different fatty diols (ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol) and CO 2 Performance evaluation of synthesized cyclic carbonates. The catalytic results are shown in Table 2.
[0048] Table 2 Evaluation of catalytic performance of different fatty diols Fatty diols Conversion rate / % Selectivity / % Yield / % Ethylene glycol 18.18 92.19 16.76 1,2-propylene glycol 17.89 90.15 16.13 1,3-Propanediol 15.65 70.76 11.07 1,4-Butanediol 10.76 50.75 5.46 From the data in Table 2, it can be seen that the yield of the five-membered ring carbonate synthesized from ethylene glycol and 1,2-propylene glycol is higher, and the yield of the six-membered ring carbonate and the seven-membered ring carbonate synthesized from 1,3-propylene glycol and 1,4-butanediol is lower. This is because the structure of the five-membered ring is the most stable and easy to form, while the stability of the six-membered ring and the seven-membered ring is poor.
[0049] Example 7 Ce 0.5 Mg0.5 Zn 0.5 Cu 0.5 O 3 Taking the perovskite catalyst as an example, the catalyst extracted after the reaction was re-calcined and the cyclic catalytic performance was studied. The catalytic reaction conditions were the same as above, and the cyclic catalytic evaluation results were shown in Table 3.
[0050] Table 3Ce 0.8 Mg 0.2 Zn 0.5 Cu 0.5 O 3 Evaluation of cyclic catalytic performance of catalysts Cycle times Conversion rate / % Selectivity / % Yield / % 1 18.18 92.19 16.76 2 16.15 91.54 14.78 3 14.75 90.43 13.34 4 12.57 87.98 11.06 5 10.38 85.59 8.88 From the data in Table 3, it can be seen that with the increase in the number of catalyst cycles, the conversion rate and yield of the product both decrease. This is because within a certain number of times, as the number of times the catalyst is used increases, the oxygen vacancies of the catalyst decrease, resulting in fewer activation center sites, leading to a decrease in catalytic activity. After five cycles, the ethylene glycol conversion rate reached 10.38%, and the selectivity of ethylene carbonate was 85.59%.
[0051] The chemical structure of the catalyst prepared in Example 3 was characterized by Fourier transform infrared spectroscopy (FT-IR). Figure 1 The chemical structure of the catalyst prepared in Example 3 was tested by X-ray diffractometer (XRD). Figure 2 The chemical structure of the catalyst prepared in Example 3 was characterized by scanning electron microscopy (SEM). Figure 3 .
[0052] Figure 1 The chemical structure of the catalyst prepared in Example 3 was tested by Fourier transform infrared spectroscopy (FT-IR). It can be seen from the analysis that the ideal ABO 3 The perovskite structure belongs to the oxygen group. The stretching vibration peaks of the AO bond and the BO bond mainly appear in the infrared spectrum. The stretching vibration of AO is around 2300cm-1, and the stretching vibration of BO is around 650cm-1. In summary, it is verified that the structure of this series of catalysts is correct.
[0053] Figure 2 The chemical structure of the catalyst prepared in Example 3 was tested by X-ray diffractometer (XRD). From the analysis of the figure, it can be seen that the characteristic diffraction peaks 2θ (28̊, 32̊, 48̊, 58̊) of perovskite appeared, forming a regular crystal structure.
[0054] The peak grain sizes were calculated and recorded using the Scherrer formula, and the average grain size (D) was calculated.
[0055] D = Kγ / (Bcosθ) (1) In formula (1): K is the Scherrer constant (if B is the half-width height of the diffraction peak, then B is the integrated height width of the diffraction peak, then K=1.00); γ is the X-ray wavelength, which is 0.154056nm; B is the half-width of the diffraction peak of the measured sample, in rad, and θ is the diffraction angle, in (̊). The catalyst Ce prepared by calculation 0.5 Mg 0.5 Zn 0.5 Cu 0.5 O 3 The particle size is 20.72nm. This is basically consistent with the results of FT-IR analysis, which indirectly shows that this series of catalysts has formed a regular perovskite structure, and the structure of this series of catalysts is correct.
[0056] Figure 3 The chemical structure of the catalyst prepared in Example 3 was characterized by using a scanning electron microscope (SEM). From the scanning electron microscope photos at different magnifications, it can be seen that after high-temperature calcination, Example 3 has the porous and layered structure that perovskite should have, which is the characteristic morphology of perovskite particle aggregation. It can also be seen that the grains are uniform, the crystals are loose and porous, and the pores are large, which is conducive to surface adsorption and the entry of lattice oxygen, thereby improving the catalytic performance. In summary, this series proves that the structure of the polymer is correct.
[0057] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the schemes disclosed herein. The present invention is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not disclosed in this disclosure. The description and examples are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the claims.
Claims
1. A Ce-based perovskite catalyst, characterized in that: The structural general formula is: Ce x Mg (1-x) Zn y Cu (1-y) O3, where 0 < x < 1; 0 < y < 1. In the high-temperature variant structure, the B-site ions Zn and Cu form octahedral coordination with six oxygen ions, and the A-site ions Ce and Mg are located in the cavities formed by these octahedra.
2. A method for preparing a Ce-based perovskite catalyst as claimed in claim 1, characterized in that: include: Step 1: adding cerium nitrate hexahydrate, magnesium nitrate hexahydrate, zinc nitrate hexahydrate, copper nitrate trihydrate, citric acid and malic acid to the ethylene glycol solution, mixing and stirring for 2-3 hours until the mixture is uniform, to obtain a mixed solution; Step 2: heating the mixed solution to 140°C, drying at 200-210°C for 8-12h to dry the water and excess ethylene glycol, and standing at room temperature for 1-2h to obtain a dried mixed gel; Step 3: Place the dried sol-gel in a muffle furnace and calcine at 700°C for 4 hours to obtain the Ce-based perovskite catalyst Ce x Mg (1-x) Zn y Cu (1-y) O3.
3. The method for preparing a Ce-based perovskite catalyst according to claim 2, characterized in that: In step 1, the molar ratio of cerium nitrate hexahydrate, magnesium nitrate hexahydrate, zinc nitrate hexahydrate and copper nitrate trihydrate is preferably x:1-x:y:1-y.
4. The method for preparing a Ce-based perovskite catalyst according to claim 2, characterized in that: In step 1, the molar ratio of nitrate, citric acid and malic acid is preferably 1:0.5:0.
5.
5. The method for preparing a Ce-based perovskite catalyst according to claim 2, characterized in that: In step 2, excess ethylene glycol in the mixed solution is removed to obtain a moderate gel.
6. The method for preparing a Ce-based perovskite catalyst according to claim 2, characterized in that: In step 3, high temperature calcination is performed to remove the organic ligands and obtain Ce x Mg (1-x) Zn y Cu (1-y) O3 perovskite catalyst.
7. Use of the Ce-based perovskite catalyst as claimed in claim 1 in converting CO2, characterized in that: Used to catalyze the synthesis of cyclic carbonates from aliphatic diols and CO2.