Microsphere catalyst containing MFI topology structure molecular sieve and preparation method and application thereof
By preparing microsphere catalysts containing MFI topological structures, the problem of difficult use of by-product fine powders during spray forming is solved, and the catalyst is uniform and has high strength, meeting the needs of cyclohexanone oxime gas-phase Beckman rearrangement reaction. , improves catalytic performance.
Patent Information
- Application Number
- CN202310594134.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
AI Technical Summary
The by-product fine powder produced by existing all-silicon-1 molecular sieve catalysts during spray forming are difficult to effectively utilize, resulting in increased production costs and insufficient catalytic performance.
Using the preparation method of microsphere catalyst containing MFI topological structure, the unqualified molecular sieve catalyst is mixed with molecular sieve, alkaline silica sol and water to be beaten, spray-drying, molding and calcining, and alkaline buffer solution with nitrogen-containing compounds. Contact to obtain a microsphere catalyst with uniform activity and high strength.
Effective recovery of by-product fine powders in spray molding is achieved. The obtained microsphere catalyst has a uniform particle size distribution and high bulk density, which meets the industrial requirements of cyclohexanone oxime gas-phase Beckman rearrangement reaction, and has significantly improved catalytic performance.
Smart Images

Figure CN119016089A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of cyclohexanone oxime gas-phase Beckmann rearrangement reaction, and in particular to a microsphere catalyst containing an MFI topological structure molecular sieve, and a preparation method and application thereof. Background Art
[0002] ε-caprolactam is the basic organic chemical raw material for the production of nylon 6 fiber and nylon 6 engineering plastics. At present, the industrial method for producing caprolactam is to use fuming sulfuric acid as a catalyst and solvent, and cyclohexanone oxime to undergo a liquid-phase Beckmann rearrangement reaction. This process has the disadvantages of equipment corrosion, environmental pollution, and unsatisfactory economic benefits, and produces a large amount of ammonium sulfate as a by-product.
[0003] The vapor-phase Beckmann rearrangement reaction of cyclohexanone oxime over a solid acid catalyst is a new process for achieving the ammonium sulfate-free conversion of ε-caprolactam. It has the advantages of no equipment corrosion, no environmental pollution, and the separation and purification of the product will also be greatly simplified. Therefore, the ammonium sulfate-free vapor-phase Beckmann rearrangement reaction process has received great attention from industry insiders.
[0004] All-silicon-1 molecular sieve has good catalytic performance in the vapor-phase Beckmann rearrangement reaction of cyclohexanone oxime. In the prior art, all-silicon-1 molecular sieve catalysts used in fluidized beds have been reported. Such all-silicon-1 molecular sieve catalysts are generally prepared by a spray molding method. However, when the molecular sieve catalyst is produced by a spray drying method, fine powder that does not meet the particle size distribution requirements will inevitably be produced, which is also a normal state. Since the production cost of the molecular sieve and catalyst used in the vapor-phase Beckmann rearrangement reaction of cyclohexanone oxime is relatively high, if the above-mentioned by-product unqualified molecular sieve catalyst cannot be effectively recovered, it will not only cause losses to production, but also greatly increase production costs. Summary of the invention
[0005] The purpose of the present invention is to overcome the problem in the prior art that by-product fine powder of the all-silicon-1 molecular sieve catalyst during the spray molding process is difficult to effectively utilize, and to provide a microsphere catalyst containing an MFI topological structure molecular sieve and a preparation method and application thereof. The preparation method uses the by-product fine powder during the spray molding process as a raw material to prepare the microsphere catalyst. The obtained microsphere catalyst has uniform activity and high strength, and the particle size distribution and bulk density can meet the industrial requirements of the catalyst for the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime, and has good catalytic performance.
[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a microsphere catalyst containing a molecular sieve with an MFI topological structure, comprising the following steps:
[0007] (1) mixing and slurrying unqualified molecular sieve catalyst, molecular sieve, alkaline silica sol and water to obtain a mixed slurry;
[0008] The viscosity of the mixed slurry is 30-120 mPa·s, and the particle size of the particles in the mixed slurry satisfies: D100≤30 μm, D90≤20 μm, D70≤10 μm;
[0009] (2) spray drying the mixed slurry and forming and calcining the mixed slurry;
[0010] (3) contacting the product obtained in step (2) with an alkaline buffer solution of a nitrogen-containing compound, and then drying;
[0011] Wherein, the molecular sieve in the unqualified molecular sieve catalyst and the molecular sieve are both molecular sieves with MFI topological structure, and the particle size of the unqualified molecular sieve catalyst is less than 50 μm or greater than 300 μm.
[0012] The mixed slurry also includes an auxiliary agent, which is an alcohol compound and / or an epoxy compound; preferably, based on the mass of the mixed slurry, the amount of the auxiliary agent is 1-10wt%.
[0013] The second aspect of the present invention provides a microsphere catalyst containing a molecular sieve with an MFI topological structure obtained by the above preparation method.
[0014] The third aspect of the present invention provides the use of the microsphere catalyst containing the MFI topological structure molecular sieve in the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime.
[0015] The method for preparing a microsphere catalyst containing a molecular sieve with an MFI topological structure provided by the present invention realizes the effective recovery of by-product fine powder or coarse powder that does not meet the particle size distribution requirements during spray molding, and the obtained microsphere catalyst has uniform activity and high strength, and the particle size distribution and bulk density can meet the industrial requirements of a catalyst for the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime, and has good catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 is an electron microscope image of the microsphere catalyst prepared in Example 1;
[0017] Figure 2 This is the particle size distribution curve of the microsphere catalyst prepared in Example 1. DETAILED DESCRIPTION
[0018] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0019] The first aspect of the present invention provides a method for preparing a microsphere catalyst containing a molecular sieve with an MFI topological structure, comprising the following steps:
[0020] (1) mixing and slurrying unqualified molecular sieve catalyst, molecular sieve, alkaline silica sol and water to obtain a mixed slurry;
[0021] The viscosity of the mixed slurry is 30-120 mPa·s, and the particle size of the particles in the mixed slurry satisfies: D100≤30 μm, D90≤20 μm, D70≤10 μm;
[0022] (2) spray drying the mixed slurry and forming and calcining the mixed slurry;
[0023] (3) contacting the product obtained in step (2) with an alkaline buffer solution of a nitrogen-containing compound, and then drying;
[0024] Wherein, the molecular sieve in the unqualified molecular sieve catalyst and the molecular sieve are both molecular sieves with MFI topological structure, and the particle size of the unqualified molecular sieve catalyst is less than 50 μm or greater than 300 μm.
[0025] In the present invention, the "unqualified molecular sieve catalyst" refers to a microsphere catalyst whose particle size distribution does not meet the requirements of qualified products, which may come from the lower cyclone material in the spray molding process, the agglomerated material of the sprayer, or the catalyst finished product whose particle size distribution does not meet the requirements of qualified products after screening.
[0026] In a specific embodiment of the present invention, the preparation method further comprises: crushing the unqualified molecular sieve catalyst. The crushing can be carried out by conventional operation methods in the art, such as air flow crushing, and then passing through a 100-200 mesh sieve. In the above preferred case, it is conducive to improving the pulping effect.
[0027] In the present invention, the molecular sieve in step (1) can be a molecular sieve raw powder or provided by a slurry containing a molecular sieve, and the present invention can be realized. The "slurry containing a molecular sieve" refers to a mixed solution containing a target molecular sieve obtained by washing, filtering and concentrating the product of the molecular sieve mother liquid crystal, and the concentration can be carried out by a membrane filtration method, which is a conventional operation in the art.
[0028] In a specific embodiment of the present invention, the molecular sieve is provided by a slurry containing the molecular sieve, and the solid content of the slurry containing the molecular sieve is 15-40 wt%, preferably 20-35 wt%.
[0029] In another specific embodiment of the present invention, the molecular sieve is provided by molecular sieve raw powder, and the molecular sieve raw powder is prepared by drying the product of molecular sieve mother liquid crystal at 100-130°C, crushing it, and passing it through a 100-200 mesh sieve. The above preferred embodiment is conducive to increasing the solid content of the mixed slurry.
[0030] According to the present invention, the molecular sieve in the unqualified molecular sieve catalyst may be the same as or different from the molecular sieve, and both are molecular sieves with MFI topological structure. Preferably, the molecular sieve in the unqualified molecular sieve catalyst has the same composition as the molecular sieve, so that the microsphere catalyst prepared has uniform components, which is conducive to improving the performance of the microsphere catalyst.
[0031] The present invention has a wide range of selection for the molecular sieve with MFI topological structure, and the molecular sieve with MFI topological structure disclosed in the prior art that can be used for cyclohexanone oxime gas phase Beckmann rearrangement reaction can be applied to the present invention. For example, the molecular sieve slurry can be the molecular sieve with MFI topological structure disclosed in patent applications CN102050464A, CN112142062A, CN112239212A, CN111847472A, CN107337213A, and CN109775714A. The unqualified molecular sieve catalyst can be the molecular sieve catalyst obtained in the spray molding process of the above molecular sieve or the particle size distribution in the finished product does not meet the requirements of qualified products.
[0032] In a specific embodiment, the unqualified molecular sieve catalyst comprises a molecular sieve having an MFI topological structure and a binder. It is understandable that there is still unremoved organic template in the lower cyclone material and the atomizer agglomerate material obtained in the spray forming process.
[0033] Directly recycling the unqualified molecular sieve catalyst obtained by spray molding can reduce the energy consumption of molding and calcining. At the same time, the unqualified molecular sieve catalyst can increase the viscosity and solid content of the spray molding slurry, which is beneficial to spray molding.
[0034] According to a preferred embodiment of the present invention, based on the total weight of the unqualified molecular sieve catalyst, the molecular sieve content is 50-95wt%, and the binder content is 5-50wt%.
[0035] In order to obtain appropriate viscosity and improve uniformity, in a further preferred embodiment, in step (1), the mixed slurry further includes an auxiliary agent, which is an alcohol compound and / or an epoxy compound. The auxiliary agent can be added to water together with the unqualified molecular sieve catalyst, molecular sieve, and alkaline silica sol for mixing and slurrying, or the auxiliary agent can be first dispersed in water and then the unqualified molecular sieve catalyst, molecular sieve, and alkaline silica sol are added.
[0036] In a further preferred embodiment, based on the mass of the mixed slurry, the amount of the auxiliary agent is 1-10wt%, preferably 3-8wt%.
[0037] The present invention has a wide selection range for the auxiliary agent. Preferably, the alcohol compound is selected from at least one of monohydric alcohol, dihydric alcohol, trihydric alcohol and polymer polyol.
[0038] Preferably, the auxiliary agent is selected from at least one of n-octanol, isooctyl alcohol, polyvinyl alcohol (1788 type or 1799 type), polyethylene oxide, starch, glycerol, and polyethylene glycol (weight average molecular weight of 2000-10000). Preferably, the auxiliary agent is polyethylene glycol and / or polyvinyl alcohol. The above preferred embodiment is conducive to increasing or improving the viscosity of the slurry.
[0039] According to a preferred embodiment of the present invention, the mixed slurry also includes a pore volume regulator. The conventional additives that can be used to adjust the pore structure of the molecular sieve catalyst in the art can be applied to the present invention. Preferably, the pore volume regulator is preferably at least one of polyacrylamine, activated carbon, sesbania powder, cellulose, urea and sucrose, and more preferably sesbania powder.
[0040] Preferably, based on the mass of the mixed slurry, the amount of the pore volume regulator is 0-5wt%, more preferably 2-4wt%. In the above preferred case, the catalytic performance of the microsphere catalyst is further improved.
[0041] In a further preferred embodiment, the viscosity of the mixed slurry is 50-100 mPa·s.
[0042] In the present invention, the viscosity of the molecular sieve-binder slurry is measured by a capillary method using a viscometer, specifically comprising: using a liquid (water) with a known kinematic viscosity as a standard (viscosity is p0, mPa·s), measuring the time t1 for it to flow out of the capillary viscometer, and then measuring the time t2 for the mixed slurry to flow out of the same viscometer. The viscosity of the mixed slurry is p (mPa·s) = t2 / t1×p0.
[0043] Preferably, the particle size of the particles in the mixed slurry satisfies: D100≤20μm, D90≤10μm, D70≤5μm. In the conventional spray forming process of molecular sieve catalysts, the usual control point is the solid content of the slurry, and a pulping machine is used to pulp the raw materials to disperse the components in the slurry. Therefore, the viscosity of the slurry obtained by conventional pulping is often low, and the particle size distribution of the particles in the slurry is not considered. However, the inventors of the present invention have found in their research that when the unqualified molecular sieve catalyst that has been spray-formed is mixed with the molecular sieve slurry and spray-formed using conventional pulping conditions, the sphericity of the obtained microsphere catalyst is poor, the particle size distribution cannot meet the requirements of qualified molecular sieve catalysts, and the catalytic performance is insufficient. The reason may be that the composition and particle size of the unqualified molecular sieve catalyst that has been formed are quite different from those of the molecular sieve slurry, resulting in poor mixing effect of the slurry. Therefore, it is necessary to strengthen the pulping of the raw materials and increase the viscosity of the mixed slurry.
[0044] Therefore, in the present invention, the viscosity and particle size distribution of the mixed slurry must be controlled at the same time. The present invention has no special requirements for the method of forming the viscosity and particle size distribution of the mixed slurry. The raw materials can be repeatedly beaten by a beater, a homogenizer, a colloid mill, a ball mill, etc. Preferably, the beating time is 1-5 hours to form a viscous mixed slurry with a specific particle size distribution.
[0045] In the present invention, preferably, the pH of the alkaline silica sol is 8-11, preferably 9-10.
[0046] Preferably, the SiO2 content in the alkaline silica sol is 20-50wt%, preferably 20-45wt%; the Na ion content is 10-500ppm.
[0047] Preferably, the amount of the alkaline silica sol calculated as SiO2 is 5-50wt%, preferably 25-45wt%, based on the dry weight of the molecular sieve.
[0048] The present invention has a wide selection range for the solid content of the mixed slurry. Preferably, the solid content of the mixed slurry is 10-60% by weight, preferably 20-60% by weight. In this preferred case, it is more conducive to the pulping and spraying forming, so that the catalyst wear index is lower.
[0049] In the present invention, the content of the unqualified molecular sieve catalyst in the mixed slurry can be selected in a wide range, as long as the viscosity and particle size distribution requirements of the mixed slurry can be met. Preferably, based on the total weight of the unqualified molecular sieve catalyst and the molecular sieve on a dry basis, the amount of the unqualified molecular sieve catalyst does not exceed 50wt%, preferably 5-20wt%.
[0050] According to a preferred embodiment of the present invention, the spray drying method is centrifugal spray drying, and the rotation speed of the atomizing wheel in the centrifugal spray drying is 15-45 Hz, for example, it can be 15 Hz, 20 Hz, 25 Hz, 30 Hz, 35 Hz, 40 Hz, 45 Hz and other typical but non-limiting rotation speeds or a range therebetween, and more preferably 20-30 Hz. By adjusting the rotation speed of the atomizing wheel in the centrifugal spray drying, a catalyst with an ideal catalyst particle size distribution and wear index can be obtained.
[0051] According to the present invention, preferably, the inlet temperature of the spray drying is 200-400° C., preferably 200-280° C.; the outlet temperature is not less than 100° C., preferably 100-130° C. In this preferred embodiment, the performance of the catalyst is better, which is more conducive to improving the conversion rate of cyclohexanone oxime and the selectivity of caprolactam.
[0052] According to a specific embodiment of the present invention, the molding and calcining in step (2) is carried out in an oxygen-containing atmosphere, and the oxygen-containing atmosphere can be provided by oxygen, air, or a mixture of oxygen and an inert gas.
[0053] Preferably, the molding and calcining process is carried out at a temperature of 400-650° C., preferably 500-600° C., and for a time of 1-20 h, preferably 6-18 h.
[0054] In a further preferred embodiment, the molding calcination method is a step-by-step temperature increase calcination, that is, the temperature is increased stepwise from room temperature to the above molding calcination temperature, the step temperature gradient is preferably 50-200°C, and the step insulation time is preferably 1-3h. The above preferred molding calcination method is beneficial to improving the roundness and smoothness of the catalyst.
[0055] According to the present invention, preferably, the step (2) comprises:
[0056] (2-1) spray-drying the mixed slurry, and then screening the microspheres obtained by the spray-drying to obtain qualified microspheres and unqualified microspheres;
[0057] The particle size of the qualified microspheres is 50-300 μm, and the particle size of the unqualified microspheres is less than 50 μm or greater than 300 μm;
[0058] (2-2) The qualified microspheres are molded and calcined, and the unqualified microspheres are returned to step (1) as unqualified molecular sieve catalysts.
[0059] In the present invention, the contact process of step (3) can be repeated. The present invention does not specifically limit the number of repetitions, which can be determined according to the effect of the contact, with the purpose of improving the performance of the catalyst. For example, the process can be repeated 1-3 times, preferably 2-3 times. In the above preferred case, it is beneficial to further reduce the wear index and improve the conversion rate and selectivity of the catalyst.
[0060] According to a specific embodiment of the present invention, in step (3), the alkaline buffer solution of the nitrogen-containing compound contains an ammonium salt and a base.
[0061] The present invention has a wide range of solvents for the alkaline buffer solution of the nitrogen-containing compound, and water is preferred.
[0062] In the present invention, the ammonium salt is preferably ammonium nitrate and / or ammonium acetate. The base is selected from at least one of aqueous ammonia, tetramethylammonium hydroxide, tetraethylammonium hydroxide and tetrapropylammonium hydroxide, preferably aqueous ammonia.
[0063] According to a preferred embodiment of the present invention, the content of the ammonium salt is 0.5-50% by weight, preferably 0.5-15% by weight; the content of the alkali is 5-30% by weight, preferably 10-28% by weight.
[0064] Preferably, the pH value of the alkaline buffer solution of the nitrogen-containing compound is 8.5-13.5, preferably 10-12, and more preferably 11-11.5.
[0065] Preferably, in step (3), the weight ratio of the product obtained in step (2) to the alkaline buffer solution of the nitrogen-containing compound, calculated on a dry basis, is 1:5-15, preferably 1:7-12.
[0066] Preferably, the contact conditions include: a temperature of 50-120°C, preferably 70-100°C; a pressure of 0.5-5 kg / cm 2 , preferably 1.5-4kg / cm 2 ; The time is 0.1-5h, preferably 1-3h.
[0067] In the present invention, the contact is preferably carried out under stirring conditions. The present invention has no particular limitation on the stirring speed, and those skilled in the art can make an appropriate selection according to actual conditions.
[0068] In the present invention, the conditions for drying the product obtained by contacting the calcined product with the alkaline buffer solution of the nitrogen-containing compound are not particularly limited, and can be carried out according to any existing technical means in the art, as long as the solvent is removed. The drying method includes but is not limited to natural drying, heating drying, and forced air drying. Specifically, for example, the drying temperature can be 100-120° C., and the drying time can be 2-36 hours.
[0069] According to the present invention, preferably, before the drying in step (3), the process further comprises: filtering and washing the product obtained in step (2) after contacting the product with an alkaline buffer solution of a nitrogen-containing compound. The present invention has no particular limitation on the washing agent used in the washing process, and the washing agent may be water, for example. Specifically, the washing process may include washing until the pH of the filtrate is 9-10.5.
[0070] According to a particularly preferred embodiment of the present invention, the preparation method comprises:
[0071] S1. Mix and slurry the unqualified molecular sieve catalyst, molecular sieve, alkaline silica sol and water to obtain a mixed slurry; based on the total weight of the unqualified molecular sieve catalyst and the molecular sieve on a dry basis, the amount of the unqualified molecular sieve catalyst does not exceed 50wt%, preferably 5-20wt%;
[0072] The viscosity of the mixed slurry is 30-120 mPa·s, and the particle size of the particles in the mixed slurry satisfies: D100≤30 μm, D90≤20 μm, D70≤10 μm;
[0073] S2, spray-drying the mixed slurry, and then screening the microspheres obtained by the spray-drying to obtain qualified microspheres and unqualified microspheres;
[0074] The particle size of the qualified microspheres is 50-300 μm, and the particle size of the unqualified microspheres is less than 50 μm or greater than 300 μm;
[0075] S3, forming and calcining the qualified microspheres;
[0076] S4, contacting the product obtained in step S3 with an alkaline buffer solution of a nitrogen-containing compound, and then washing, filtering, and drying to obtain a finished catalyst;
[0077] S5, screening the finished catalyst to obtain qualified catalyst and unqualified catalyst; the particle size of the qualified catalyst is 50-300 μm, and the particle size of the unqualified catalyst is less than 50 μm or greater than 300 μm;
[0078] The unqualified microspheres and unqualified catalysts are used to provide the unqualified molecular sieve catalyst in step S1.
[0079] The second aspect of the present invention provides a microsphere catalyst containing a molecular sieve with an MFI topological structure obtained by the above preparation method.
[0080] In the present invention, the microsphere catalyst prepared by the preparation method has a lower wear index, and the lower the wear index K, the higher the wear resistance of the catalyst. Preferably, the wear index K of the microsphere catalyst is less than 3% / h, preferably 1.5-2.5% / h. Under this preferred embodiment, the strength of the catalyst is higher, which is more conducive to improving the stability of the catalyst and facilitating the long-term use of the catalyst.
[0081] In the present invention, the wear index K is measured on a wear index analyzer according to the RIPP29-90 method in "Petrochemical Analysis Methods" (Yang Cuiding et al., Science Press, 1990).
[0082] According to the present invention, preferably, the bulk density of the microsphere catalyst is 0.6-0.9 g / cm 3 , preferably 0.65-0.8 g / cm 3 In the above preferred case, the catalyst is not easily worn away and turned into small particles, which is beneficial to prolonging the service life of the catalyst.
[0083] In the present invention, the bulk density of the catalyst is determined by passing the catalyst powder through a small funnel, allowing the powder to fall freely from the funnel into a 100 mL measuring cylinder and weighing its mass. During this period, the measuring cylinder is continuously vibrated or tapped until the volume of the catalyst powder reaches the 100 mL scale line and no longer changes. The bulk density of the catalyst is obtained by the mass of the catalyst at this time.
[0084] The third aspect of the present invention provides the use of the microsphere catalyst containing the MFI topological structure molecular sieve in the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime.
[0085] The microsphere catalyst prepared by the preparation method has suitable particle size distribution and low abrasion index, has good catalytic performance in preparing caprolactam in the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime, and is particularly suitable for circulating fluidized bed reactors.
[0086] The present invention will be described in detail below through examples.
[0087] In the following examples, unless otherwise specified, pressure is gauge pressure; normal pressure refers to one atmosphere; and normal temperature refers to 25°C.
[0088] In the present invention, the viscosity of the molecular sieve-binder slurry is measured by a capillary method using a viscometer, specifically comprising: using a liquid (water) with a known kinematic viscosity as a standard (viscosity is p0, mPa·s), measuring the time t1 for it to flow out of the capillary viscometer, and then measuring the time t2 for the mixed slurry to flow out of the same viscometer. The viscosity of the mixed slurry is p (mPa·s) = t2 / t1×p0.
[0089] The particle size distribution of the microsphere molecular sieve catalyst was measured using a 3000 laser particle size analyzer from Malvern. The test method was a wet test, with water as the medium, a sample mass concentration of 0.5%-2%, and a scanning speed of 2000 times / second.
[0090] The morphology of the catalyst was photographed at a magnification using a MG10085-1A 100X reading microscope.
[0091] The wear index K of the catalyst was measured on a wear index analyzer according to the RIPP29-90 method in "Petrochemical Analysis Methods" (Yang Cuiding et al., Science Press, 1990);
[0092] Method for determining bulk density of catalyst: Pass the catalyst powder through a small funnel, and allow the powder to freely fall from the funnel into a 100mL measuring cylinder and weigh its mass. During this period, continuously vibrate or tap the measuring cylinder until the volume of the catalyst powder reaches the 100mL mark and no longer changes. The bulk density of the catalyst is calculated from the mass of the catalyst at this time.
[0093] In the following examples, the spray forming is carried out in a spray forming device, which is produced by Wuxi Tianyang Spray Drying Equipment Co., Ltd. and has a model number of LT-300.
[0094] Preparation Example
[0095] (1) Preparation of molecular sieve slurry
[0096] 482 kg of 95 wt% ethanol and 302 kg of 22.5 wt% tetrapropylammonium hydroxide aqueous solution were added to 2M 3 In a stainless steel reactor, stir, then add 332 kg of water to the reactor, continue stirring, then add 347 kg of tetraethyl orthosilicate, stir at room temperature (25°C) for 4 hours to form a colloidal mixture, wherein the molar ratio of SiO2: ethanol: tetrapropylammonium hydroxide: water is 1:10:0.20:20; first crystallize in an alcohol-hydrothermal system at 70°C for 1 day, then crystallize in an alcohol-hydrothermal system at 100°C for 2 days, the pH value of the crystallized product is 13.51, then use a 50 nm six-tube membrane for membrane filtration and use 40-60°C water for washing, the washing water amount is 6.0 M 3, the pH value of the washing water of the crystallized product reached 9.1. After washing and filtering, the obtained slurry was concentrated to 395 kg of molecular sieve slurry with a solid content of 26.8% by weight, recorded as S-1.
[0097] (2) Unqualified molecular sieve catalyst
[0098] The molecular sieve slurry was mixed with 113 kg of 40% alkaline silica sol (pH 9.5, sodium ion content 324 ppm, SiO2 content 40% by weight, and the surface area of SiO2 obtained after calcination was 225 m 2 / g) was mixed, the weight ratio of the molecular sieve dry basis and the alkaline silica sol in terms of SiO2 in the molecular sieve slurry was 70:30, stirred evenly, and slurried to obtain a molecular sieve-binder mixed slurry with a solid content of 29.7% by weight. It was sent to a spray molding device (produced by Wuxi Tianyang Spray Drying Equipment Co., Ltd., model LT-300) for spray molding, with the inlet and outlet temperatures of 360°C and 130°C respectively, and sieved with a 50-300 mesh sieve, and 50-300 μm microspheres were collected as qualified microspheres, and the rest were crushed and sieved through a 200 mesh sieve and used as unqualified molecular sieve catalysts for standby use (recorded as FQ-1). Then the qualified microspheres were sent to a 30M roller kiln heating furnace (manufactured by Hubei Huanggang Huayao Zhongrui Kiln Co., Ltd.) and calcined at 180°C, 350°C, 500, 530, 580, 580, 580, and 420°C in zones 1-8 for 2 h each to obtain molecular sieve catalyst A1 (as a reference agent). The particle size of A1 was concentrated in the range of 50-300 μm, the attrition index K was 6.4% / h, and the bulk density was 0.685 g / cm 3 .
[0099] Example 1
[0100] The molecular sieve slurry S-1 prepared in the preparation example was dried at 120°C for 24 hours, and then crushed through a 140-mesh sieve to obtain 123.5 kg of molecular sieve raw powder.
[0101] (1) 12.6 kg of unqualified molecular sieve catalyst FQ-1 was mixed with 123.5 kg of molecular sieve raw powder, 12.5 kg of polyethylene glycol (weight average molecular weight 6000), and 113 kg of alkaline silica sol (pH value 9.5, sodium ion content 324 ppm, SiO2 content 40% by weight), and the surface area of the obtained SiO2 after calcination was 225 m 2 / g) are mixed, and an appropriate amount of water is added to adjust the solid content of the mixed slurry to 50% to obtain a mixed slurry, wherein the weight ratio of the molecular sieve dry basis of the molecular sieve raw powder to the alkaline silica sol calculated as SiO2 is 70:30, and the amount of the unqualified molecular sieve catalyst calculated based on the molecular sieve content is 6.8wt% based on the total weight of the unqualified molecular sieve catalyst and the molecular sieve dry basis in the molecular sieve slurry is 6.8wt%, and the amount of polyethylene glycol is 5wt% based on the mass of the mixed slurry. The mixture is stirred evenly, and after beating for 2 hours using a JMS-50DG split colloid mill of Langfang Langtong Machinery Co., Ltd., the viscosity of the obtained mixed slurry is 66mPa·s, wherein the D100 of the particles in the mixed slurry is 18.3μm, the D90 is 9.3μm, and the D70 is 4.5μm.
[0102] (2) The mixed slurry was sent to a spray forming device (produced by Wuxi Tianyang Spray Drying Equipment Co., Ltd., model LT-300) for spray forming, with the inlet and outlet temperatures being 260°C and 130°C respectively, and the rotation speed of the atomizing wheel in the centrifugal spray drying being 27 Hz. The mixed slurry was sieved with a 50-300 mesh sieve to obtain 175 kg of qualified microspheres (particle size of 50-300 μm) and 11 kg of unqualified microspheres (recorded as FQ-2, the particle size of the unqualified microspheres was <50 or >300 μm, and the process was returned to step (1)). Then 175 kg of qualified microspheres were fed into a 30M roller kiln heating furnace (manufactured by Hubei Huanggang Huayao Zhongrui Kiln Co., Ltd.), and calcined at 180°C, 350°C, 500, 530, 580, 580, 580, and 420°C in zones 1-8 for 2 hours each to obtain formed microspheres, wherein the content of all-silica-1 molecular sieve with MFI topological structure was 69.8% by weight, and the content of binder silica sol was 30.2% by weight.
[0103] (3) 100 g of the above-mentioned formed microspheres and 1000 g of an alkaline buffer solution of a nitrogen-containing compound (the alkaline buffer solution of the nitrogen-containing compound is a mixture of ammonia water and an ammonium nitrate aqueous solution, with a pH value of 11.35, wherein the content of ammonia water is 26% by weight, the content of ammonium nitrate in the ammonium nitrate aqueous solution is 7.5% by weight, and the weight ratio of ammonia water to ammonium nitrate aqueous solution is 3:2) are added to a 2000 mL stainless steel reactor (KCF-2 magnetic stirring autoclave, Yantai High-tech Zone Keli Automatic Control Equipment Research Institute) and heated at 86°C and 2.7 kg / cm 2 Stirring at a constant temperature for 2 hours under pressure, then filtering, and drying at 90°C for 12 hours, repeating the treatment under the same conditions once, then filtering and washing until the pH of the filtered clear liquid is about 9, and then drying at 120°C for 24 hours to obtain a finished catalyst;
[0104] The finished catalyst is sieved with a 50-300 mesh sieve to obtain a qualified microsphere catalyst finished product FS1 with a particle size of 50-300 μm, and the unqualified microsphere catalyst finished product with a particle size less than 50 μm or greater than 300 μm is returned to step (1). The morphology of the catalyst FS1 is characterized by an electron microscope, such as Figure 1 As shown, it can be seen that the particle size of the catalyst is very uniform, and the particle size distribution is as follows Figure 2 shown.
[0105] The particle size of the catalyst FS1 was concentrated in the range of 70-150 μm by a vibrating screen. After testing, the attrition index K was 1.6% / h and the bulk density was 0.678 g / cm 3 .
[0106] Example 2
[0107] (1) 11 kg of unqualified molecular sieve catalyst FQ-1 was mixed with 395 kg of S-1 molecular sieve slurry with a solid content of 26.8% by weight, 1788 type polyvinyl alcohol, 113 kg of alkaline silica sol (pH value is 9.5, sodium ion content is 324 ppm, SiO2 content is 40% by weight, and the surface area of SiO2 obtained after calcination is 225 m 2 / g) are mixed, and appropriate amount of water is added to make the solid content of 31.2% to obtain a mixed slurry; the weight ratio of the molecular sieve dry basis in the molecular sieve slurry to the alkaline silica sol calculated as SiO2 is 70:30, and the amount of the unqualified molecular sieve catalyst calculated by the molecular sieve content is 6.0wt% based on the total weight of the unqualified molecular sieve catalyst and the molecular sieve dry basis in the molecular sieve slurry is taken as the benchmark, and the amount of polyvinyl alcohol is 3wt% based on the mass of the mixed slurry; after stirring evenly, the slurry is beaten for 2 hours using the JMS-50DG split colloid mill of Langfang Langtong Machinery Co., Ltd.; the viscosity of the mixed slurry is measured to be 71mPa·s, wherein the D100 of the particles in the mixed slurry is 18.6μm, the D90 is 9.6μm, and the D70 is 4.7μm.
[0108] (2) Send it to a spray forming device for spray forming, the inlet and outlet temperatures are 240°C and 110°C respectively, and the speed of the atomizing wheel in the centrifugal spray drying is 26Hz. Sieve with a 50-300 mesh sieve to obtain qualified microspheres and unqualified microspheres, and the unqualified microspheres are returned to step (1). Send the qualified microspheres to a 30M roller kiln heating furnace (produced by Hubei Huanggang Huayao Zhongrui Kiln Co., Ltd.), and roast them at 180°C, 350°C, 500, 530, 580, 580, 580, and 420°C in zones 1-8 for 2 hours respectively to obtain molded microspheres, wherein the content of all-silicon-1 molecular sieve with MFI topological structure is 70.1% by weight, and the content of binder silica sol is 29.9% by weight.
[0109] (3) 100 g of the above-mentioned formed microspheres and 1000 g of an alkaline buffer solution of a nitrogen-containing compound (the alkaline buffer solution of the nitrogen-containing compound is a mixture of ammonia water and an ammonium nitrate aqueous solution, with a pH value of 11.35, wherein the content of ammonia water is 26% by weight, the content of ammonium nitrate in the ammonium nitrate aqueous solution is 7.5% by weight, and the weight ratio of ammonia water to ammonium nitrate aqueous solution is 3:2) are added to a 2000 mL stainless steel reactor (KCF-2 magnetic stirring autoclave, Yantai High-tech Zone Keli Automatic Control Equipment Research Institute) and heated at 86°C and 2.7 kg / cm 2 Stir under pressure at a constant temperature for 2 hours, then filter and dry at 90°C for 12 hours. Repeat the treatment under the same conditions, then filter and wash until the pH of the filtered clear liquid is about 9, and then dry at 120°C for 24 hours to obtain the finished catalyst.
[0110] The finished catalyst is sieved with a 50-300 mesh sieve to obtain a qualified microsphere catalyst FS2 with a particle size of 50-300 μm, and the unqualified microsphere catalyst finished product with a particle size less than 50 μm or greater than 300 μm is returned to step (1). The particle size of the catalyst is concentrated in the range of 70-150 μm, the wear index K is 1.6% / h, and the bulk density is 0.68 g / cm 3 .
[0111] Example 3
[0112] The method in Example 2 is followed, except that polyvinyl alcohol is not included in the mixed slurry; after 2 hours of slurrying using a JMS-50DG split-type colloid mill produced by Langfang Langtong Machinery Co., Ltd., the viscosity of the mixed slurry is measured to be 47 mPa·s, wherein the D100 of the particles in the mixed slurry is 19 μm, the D90 is 9.5 μm, and the D70 is 4.8 μm.
[0113] The microsphere catalyst was formed according to the method of Example 2 and was recorded as FS3. The particle size of the catalyst was concentrated in the range of 70-150 μm, the wear index K was 2.3% / h, and the bulk density was 0.673 g / cm 3 .
[0114] Example 4
[0115] The unqualified microspheres FQ-1 prepared in Preparation Example 1 were sent to a 30M roller kiln heating furnace (produced by Hubei Huanggang Huayao Zhongrui Kiln Co., Ltd.) and calcined at 180°C, 350°C, 500, 530, 580, 580, 580, and 420°C in zones 1-8 for 2 h each. The product obtained was recorded as BFQ-1.
[0116] The microsphere catalyst was prepared according to the method in Example 1, except that BFQ-1 was used instead of FQ-1. The obtained catalyst was recorded as FS4, and the particle size of the catalyst was concentrated in the range of 70-150 μm, the attrition index K was 1.7% / h, and the bulk density was 0.680 g / cm 3 The unqualified material after calcination is easier to spray-form. The morphology of the catalyst was observed under a microscope, and it had good smoothness and slightly improved sphericity.
[0117] Example 5
[0118] The method of Example 2 was followed, except that the beating time was 0.5 h, and the viscosity of the mixed slurry was 44 mPa·s, wherein the D100, D90 and D70 of the particles in the mixed slurry were 22 μm, 12 μm and 8.6 μm.
[0119] Then, the catalyst FS5 was formed according to the method of Example 1. The particle size of the catalyst was concentrated in the range of 50-200 μm, the attrition index K was 3% / h, and the bulk density was 0.636 g / cm 3 .
[0120] Comparative Example 1
[0121] The method in Example 3 is followed, except that after 0.5 hour of slurrying using a JMS-50DG split-type colloid mill produced by Langfang Langtong Machinery Co., Ltd., the viscosity of the mixed slurry is 37 mPa·s, wherein the D100 of the particles in the mixed slurry is 32 μm, the D90 is 23 μm, and the D70 is 12 μm.
[0122] The catalyst DS1 was obtained. The particle size of the catalyst was concentrated in the range of 30-200 μm, the attrition index K was 3.5% / h, and the bulk density was 0.633 g / cm 3 .
[0123] Comparative Example 2
[0124] The method in Example 2 was followed, except that unqualified molecular sieve catalyst FQ-1, S-1 molecular sieve slurry, 1788 type polyvinyl alcohol, and alkaline silica sol were self-circulated through a slurry circulation pump (Yixing Zeus Pump Co., Ltd., UHB-Z type) for 1 hour, so that the viscosity of the mixed slurry was 23 mPa·s, wherein the D100 of the particles in the mixed slurry was 36 μm, D90 was 25 μm, and D70 was 13 μm.
[0125] The catalyst DS2 was obtained. The particle size of the catalyst was concentrated in the range of 30-250 μm, the attrition index K was 5.8% / h, and the bulk density was 0.622 g / cm 3 .
[0126] Comparative Example 3
[0127] The method in Example 1 is followed, except that the amount of FQ-1 is such that, based on the total weight of the unqualified molecular sieve catalyst and the molecular sieve dry basis in the molecular sieve slurry, the amount of the unqualified molecular sieve catalyst calculated by molecular sieve content is 40wt%; after slurrying for 2 hours using a JMS-50DG split-type colloid mill produced by Langfang Langtong Machinery Co., Ltd., the viscosity of the mixed slurry is 36mPa·s, wherein the D100 of the particles in the mixed slurry is 38μm, the D90 is 26μm, and the D70 is 14μm.
[0128] Then, the catalyst was molded according to the method of Example 1, and the obtained catalyst was recorded as FS6. The particle size of the catalyst was concentrated in the range of 80-200 μm, the wear index K was 3.7% / h, and the bulk density was 0.644 g / cm 3 .
[0129] Test Case
[0130] This test example is used to evaluate the catalytic reaction effect of the catalyst containing the MFI topological structure molecular sieve prepared in the examples and comparative examples in the gas-phase Beckmann rearrangement reaction:
[0131] The reaction performance of the microsphere molecular sieve catalyst was evaluated using a fixed fluidized bed. The structure of the fixed fluidized bed reactor is: a vertical 316L stainless steel reactor with an upper diameter of 20 cm and a lower diameter of 10 cm. The lengths of the upper and lower sections are 60 and 80 cm respectively. The distribution plate is a 2500 mesh (5 micron) metal sintered plate filter. The catalyst loading is 300 grams, and the feed is fed by gas atomization spray. The reactor is designed with multi-stage electric heating control, which can adjust the reactor heating power and reaction temperature, and multiple temperature measurement points are installed.
[0132] Catalyst pretreatment: The temperature of the vaporizer is maintained above 180°C, the temperature of the vaporizer to the preheater pipeline is kept at 200°C, the heater is 250-300°C, the temperature of the heater to the fixed fluidized bed reactor pipeline is kept at 300°C, nitrogen is introduced, and the catalyst is activated for 1 hour. Adjust the reaction pressure, maintain the reaction temperature at the required reaction temperature, start the horizontal flow pump, and let a certain concentration of cyclohexanone oxime ethanol solution enter the vaporizer and preheater at a certain flow rate and then enter the fixed fluidized bed reactor.
[0133] The process conditions are adjustable within the following ranges: reaction temperature range is 380-390°C; cyclohexanone oxime accounts for 35% by weight of the total amount of cyclohexanone oxime and ethanol, and the water content is 0.8% by weight; the molar ratio of nitrogen to cyclohexanone oxime is 2:1; the reaction pressure is 0.05 MPa; the weight space velocity of cyclohexanone oxime is 4 h -1The reaction product was cooled by ice-water mixture and then entered into a collection bottle for gas-liquid separation. After 10 hours of reaction, the product composition was analyzed.
[0134] The reaction products were quantitatively analyzed using a Shimadzu GC-2030 gas chromatograph (hydrogen flame ionization detector, HP-Innowax capillary column, column length 60 m, PEG20M as the stationary phase) with a vaporization chamber temperature of 250 °C, a detection chamber temperature of 280 °C, a split ratio of 50, and a column temperature programmed from 50 °C to 220 °C at a heating rate of 5 °C / min, held at this temperature for 10 min, then from 220 °C to 240 °C at a heating rate of 10 °C / min, held at this temperature for 10 min.
[0135] The conversion rate of cyclohexanone oxime (CHO) and the selectivity of caprolactam (CPL) were calculated using the following formula:
[0136] CHO conversion rate (wt%) = [(100-CHO percentage in the reaction product) / 100] × 100%
[0137] CPL selectivity (wt%) = [CPL percentage in the reaction product / (100-CHO percentage in the reaction product)] × 100%;
[0138] By-product selectivity (wt%) = [by-product percentage in the reaction product / (100-CHO percentage in the reaction product)] × 100%;
[0139] The percentages of CHO and CPL in the reaction products are chromatographic analysis values.
[0140] The contents of rearrangement products of caprolactam and cyclohexanone oxime after the reaction were calculated using the area normalization method, and the solvent was not involved in the integration.
[0141] Among the by-products of the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime, ethyl-ε-caprolactam (AEH) accounts for about 40% of the total amount of all by-products. This by-product is generated by the alcoholysis reaction between ethanol and the tautomer of the enol structure of caprolactam. Under the action of water, ethyl-ε-caprolactam continues to generate caprolactam through hydrolysis reaction. Therefore, the amount of caprolactam generated by the hydrolysis of ethyl-ε-caprolactam is included in the calculation of the total selectivity of caprolactam. The results are shown in Table 1.
[0142] Table 1
[0143]
[0144] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a microsphere catalyst containing a molecular sieve with an MFI topological structure, It is characterized in that The following steps are involved: (1) mixing and slurrying unqualified molecular sieve catalyst, molecular sieve, alkaline silica sol and water to obtain a mixed slurry; The viscosity of the mixed slurry is 30-120 mPa·s, and the particle size of the particles in the mixed slurry satisfies: D100≤30 μm, D90≤20 μm, D70≤10 μm; (2) spray drying the mixed slurry and forming and calcining the mixed slurry; (3) contacting the product obtained in step (2) with an alkaline buffer solution of a nitrogen-containing compound, and then drying; Wherein, the molecular sieve in the unqualified molecular sieve catalyst and the molecular sieve are both molecular sieves with MFI topological structure, and the particle size of the unqualified molecular sieve catalyst is less than 50 μm or greater than 300 μm.
2. The preparation method according to claim 1, in, The unqualified molecular sieve catalyst comprises a molecular sieve having an MFI topological structure and a binder; Preferably, based on the total weight of the unqualified molecular sieve catalyst, the molecular sieve content is 50-95wt%, and the binder content is 5-50wt%.
3. The preparation method according to claim 1 or 2, in, The mixed slurry also includes an auxiliary agent, which is an alcohol compound and / or an epoxy compound; Preferably, based on the mass of the mixed slurry, the amount of the auxiliary agent is 1-10wt%; Preferably, the alcohol compound is selected from at least one of monohydric alcohol, dihydric alcohol, trihydric alcohol and polymer polyol; Preferably, the auxiliary agent is selected from at least one of n-octanol, isooctyl alcohol, polyvinyl alcohol, polyethylene oxide, starch, glycerol and polyethylene glycol; more preferably polyethylene glycol and / or polyvinyl alcohol; Preferably, the mixed slurry further comprises a pore volume regulator, and the pore volume regulator is preferably at least one of polyacrylamine, activated carbon, sesbania powder, cellulose, urea and sucrose; Preferably, based on the mass of the mixed slurry, the amount of the pore volume regulator is 0-5wt%.
4. The preparation method according to any one of claims 1 to 3, in, The viscosity of the mixed slurry is 50-100 mPa·s; And / or, the particle size of the particles in the mixed slurry satisfies: D100≤20 μm, D90≤10 μm, D70≤5 μm.
5. The preparation method according to any one of claims 1 to 4, in, The pH of the alkaline silica sol is 8-11, preferably 9-10; And / or, SiO in the alkaline silica sol 2 The content is 30-50wt%.
6. The preparation method according to any one of claims 1 to 5, in, The solid content of the mixed slurry is 20-60wt%; and / or, based on the total weight of the unqualified molecular sieve catalyst and the molecular sieve on a dry basis, the amount of the unqualified molecular sieve catalyst does not exceed 50wt%, preferably 5-20wt%; And / or, based on the dry weight of the molecular sieve, SiO 2 The amount of the alkaline silica sol is 5-50wt%.
7. The preparation method according to any one of claims 1 to 6, in, The spray drying method is centrifugal spray drying, and the rotation speed of the atomizing wheel in the centrifugal spray drying is 15-45 Hz, preferably 20-35 Hz; Preferably, the inlet temperature of the spray drying is 200-400°C, preferably 200-260°C; the outlet temperature is not less than 100°C, preferably 100-130°C.
8. The preparation method according to any one of claims 1 to 7, in, The forming and calcining in step (2) is carried out in an oxygen-containing atmosphere; Preferably, the molding and calcining process is carried out at a temperature of 400-650° C., preferably 500-600° C., and for a time of 1-20 h, preferably 6-18 h.
9. The preparation method according to any one of claims 1 to 8, in, In step (3), the alkaline buffer solution of the nitrogen-containing compound contains an ammonium salt and a base, the content of the ammonium salt is 0.5-20% by weight, the content of the base is 5-30% by weight, and the pH value of the alkaline buffer solution of the nitrogen-containing compound is 8.5-13.5; Preferably, in step (3), the weight ratio of the product obtained in step (2) to the alkaline buffer solution of the nitrogen-containing compound, calculated on a dry basis, is 1:5-15; Preferably, the contact conditions include: a temperature of 50-120°C, preferably 70-100°C; a pressure of 0.5-5 kg / cm 2 , preferably 1.5-4kg / cm 2 ; The time is 0.1-5h, preferably 1-3h; Preferably, the number of contacts is 1-5 times, preferably 2-3 times.
10. A microsphere catalyst containing a molecular sieve with an MFI topological structure obtained by the preparation method according to any one of claims 1 to 9; Preferably, the wear index of the microsphere catalyst is less than 3% / h; Preferably, the bulk density of the microsphere catalyst is 0.6-0.9 g / cm 3 , preferably 0.65-0.8 g / cm 3 .
11. Use of the microsphere catalyst containing the MFI topological structure molecular sieve according to claim 10 in the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime.
Citation Information
Patent Citations
Synthesizing method of silicon molecular sieve
CN102050464A
Silicate-1 molecular sieves containing trace metal ions and preparation method for Silicate-1 molecular sieves
CN107337213A
MFI topological structure silicon molecular sieve containing trace rare earth ions and preparation method thereof
CN109775714A
MFI topological structure silicon molecular sieve as well as preparation method and application thereof
CN111847472A
Rare earth-containing MFI topology structure silicon molecular sieve as well as preparation method and application thereof
CN112142062A
Cited By
Method for preparing caprolactam
CN120025268A