Zinc complex containing nitrogen-phosphorus double bonds, preparation method and application of zinc complex in catalytic synthesis of polylactide

By developing a catalyst composition of zinc complex containing nitrogen-phosphorus double bonds and organic silicone amino-based metal compounds, the problem of insufficient catalytic activity and stability of existing zinc complexes is solved, and the efficient ring-opening polymerization of lactide is achieved and the Biosafety polymer production.

CN119060091AActive Publication Date: 2024-12-03BEIJING INST OF CLOTHING TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310624138.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

The existing zinc complex catalysts have weak catalytic activity in lactide ring-opening polymerization, poor air stability, and are difficult to achieve large-scale production and industrialization processes, and their biosafety and molecular weight distribution are not optimized enough.

Method used

Develop a zinc complex containing nitrogen-phosphorus double bonds, and perform ring-opening polymerization of lactide by coordination of phosphimine and amine or imine groups, combining silicone amino metal compounds and organic alcohols as catalyst compositions. , control reaction conditions to achieve efficient polymerization.

Benefits of technology

It has achieved efficient catalytic polymerization of lactide under mild conditions, with good catalyst stability and low toxicity, suitable for industrial production, and good biosafety and molecular weight distribution uniformity of polymers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004256389940000031
    Figure BDA0004256389940000031
  • Figure BDA0004256389940000051
    Figure BDA0004256389940000051
  • Figure BDA0004256389940000061
    Figure BDA0004256389940000061
Patent Text Reader

Abstract

The zinc complex containing the nitrogen-phosphorus double bond is used as a catalyst to catalyze lactide ring-opening polymerization, the catalytic activity is high, the polymerization time is short, and green polymerization is achieved. In the actual production process, the purposes of saving energy, shortening the production period and reducing the production cost can be achieved. The method can realize controllable polymerization, the polymerization reaction condition is mild, the operation is simple, the batch industrial production is expected to be realized, the biological safety is good, and the application in the fields of biomedicine and the like is expected to be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer polymerization, and in particular relates to the polymerization of lactide, and in particular, to a zinc complex containing nitrogen and phosphorus double bonds and a preparation method thereof, and application of the zinc complex as a catalyst in the ring-opening polymerization of lactide. Background Art

[0002] In 1920, Hermann Staudinger published the first article introducing the concept of polymerization. Over the past 100 years, with the development of the petrochemical industry, polymer materials have gradually become the cornerstone of modern life and are widely used in various fields. However, from an environmental perspective, most polymers are derivatives of petrochemical products, so there are corresponding defects in sustainability. Although only a small part of oil and natural gas is currently used to make polymer materials, since fossil fuels are a non-renewable resource, it is crucial to find renewable raw material substitutes. On the other hand, in the post-processing of waste polymers, only a part of them enters the landfill, while a considerable amount of plastic fragments enter the marine cycle, causing harmful effects on marine life and potential human life. The emergence of biodegradable polymer materials provides a more convenient way to process polymers, which can effectively avoid the problem of landfill accumulation; similarly, the source of biodegradable polymer materials is renewable, such as the commercialized polylactic acid (PLA), which comes from starch-rich plants: beets, corn and potatoes.

[0003] Among the numerous synthetic biodegradable materials, linear aliphatic polyesters have been studied the most, especially the homopolymerization and copolymerization of polylactide (PLA), polycaprolactone (PCL), polyglycolide (PGA), etc. These polymers are metabolized in the body and discharged in the form of water and carbon dioxide, so they are not only biodegradable, but also have certain biocompatibility. In addition, lactide can be obtained from crops and cash crops, and the raw materials are inexhaustible. Therefore, it is possible to achieve large-tonnage production of these polymers and even replace petroleum-based materials. These environmentally friendly polymer materials can be rapidly degraded without harming natural organisms and the environment, and aliphatic polyesters such as PLA, as one of the materials with the most potential for replacement, play a very prominent role in various fields. With the development of technology, people expect to use efficient metal catalysts to catalyze the ROP of cyclic esters with high catalytic activity and stereoselectivity.

[0004] In recent years, Williams' research group has found that a series of metal complexes containing phosphinimine structures prepared by introducing phosphorus atoms to replace carbon atoms in the Salen structure not only have high catalytic efficiency, but also maintain good stereoselectivity for racemic lactide, so metal complexes containing phosphorus-nitrogen double bonds have attracted people's attention. Further studies have shown that compared with the C=N bond in the Salen ligand structure, the electron distribution in the P=N double bond structure is significantly different due to the large difference in electronegativity between the phosphorus and nitrogen atoms, which makes P=N have higher ionic bond performance. The nitrogen atom has two lone electron pairs and has strong σ and π electron-donating abilities, which improves the Lewis acidity of the coordinated metal center, makes the metal-oxygen bond looser, and is conducive to the insertion of monomers, thereby improving the activity of ring-opening polymerization. At the same time, in terms of geometric configuration, because phosphorus in phosphinimine (P=N) is pyramidal and has two substituents, it is different from sp 2 Unlike the hybridized C=N, the imine carbon is a trigonal planar structure with only one substituent, so their bond lengths are significantly different ( vs Therefore, the P=N double bond in phosphinimine has a highly polarized characteristic, which is mainly due to the approximate sp 2 The hybridized nitrogen atoms cooperate with transition metals to form stable complexes, thus exhibiting unique catalytic properties.

[0005] Zinc is one of the elements involved in human metabolism and is a common metal in nature with low acquisition cost and low price. In recent years, there have been many studies on the ring-opening polymerization of cyclic esters catalyzed by zinc complexes, but the catalytic activity of new catalysts is relatively weak, and the stability in the air is poor, and storage and transportation are difficult. In order to meet the large-scale production of polymer materials and to prepare biodegradable materials with high biosafety, high molecular weight and narrow molecular weight distribution, it is urgent to study and develop a polyester polymerization method with simple process and industrial production, so as to prepare biodegradable polyester with high biosafety and good performance. Summary of the invention

[0006] In order to overcome the above problems, the present invention provides a zinc complex containing nitrogen and phosphorus double bonds, and uses the zinc complex and a co-initiator as a catalyst composition to catalyze the ring-opening polymerization of lactide, thereby achieving efficient polymerization of lactide under mild conditions, thereby completing the present invention.

[0007] The first aspect of the present invention aims to provide a zinc complex containing a nitrogen-phosphorus double bond, in which zinc forms a di-coordination with the phosphorus imine and the amine or imine group in the ligand, and the ligand comprises a diphenylphosphine group and a substituted or unsubstituted phenylenediamine group, and the two are connected by a nitrogen-phosphorus double bond.

[0008] Preferably, the zinc complex containing nitrogen and phosphorus double bonds is a complex having a structure as shown in formula (1):

[0009]

[0010] Among them, Ph is phenyl,

[0011] R is selected from hydrogen, alkyl, halo or aromatic, preferably selected from hydrogen, C1-C5 alkyl, fluorine substituent, chlorine substituent, bromine substituent, phenyl, alkylphenyl, alkoxyphenyl, more preferably hydrogen, methyl, chlorine substituent or fluorine substituent;

[0012] R0 is selected from hydrogen, alkyl or aromatic groups, preferably selected from hydrogen, C1-C5 alkyl, phenyl, more preferably hydrogen or phenyl;

[0013] X is an anion that makes the zinc complex containing nitrogen and phosphorus double bonds electrically neutral, such as chloride ion, bromide ion, nitrate ion, acetate ion, etc., preferably chloride ion.

[0014] The second aspect of the present invention also aims to provide a method for preparing the zinc complex containing nitrogen and phosphorus double bonds, the method specifically comprising the following steps:

[0015] Step 1, adding bromine to a diphenylphosphine solution to react and obtain a reaction solution I;

[0016] Step 2, adding the phenylenediamine compound solution to the reaction solution I, stirring and reacting to obtain the reaction solution II;

[0017] Step 3, post-treating the reaction solution II to obtain a ligand containing a nitrogen-phosphorus double bond;

[0018] Step 4: adding the zinc salt solution to the ligand solution containing nitrogen and phosphorus double bonds, stirring for reaction, and post-treating the reaction solution to obtain a zinc complex containing nitrogen and phosphorus double bonds.

[0019] The third aspect of the present invention aims to provide a catalyst composition for catalyzing the ring-opening polymerization of lactide, wherein the catalyst composition comprises the zinc complex containing nitrogen and phosphorus double bonds.

[0020] The catalyst composition further comprises an organosilicon amine metal compound and an organic alcohol.

[0021] The fourth aspect of the present invention aims to provide a method for preparing polylactide, which comprises adding lactide to a solution containing the catalyst composition to carry out polymerization.

[0022] The method specifically comprises the following steps:

[0023] Step a, adding the catalyst composition into a reaction solvent, aging, and obtaining a mixed solution;

[0024] Step b, adding lactide monomer to the mixed solution, heating for reaction, and obtaining a reaction solution;

[0025] Step c, post-treating the reaction solution to obtain polylactide.

[0026] The preparation method of the zinc complex containing nitrogen and phosphorus double bonds and polylactide provided by the present invention has the following beneficial effects:

[0027] (1) The zinc complex containing nitrogen and phosphorus double bonds in the present invention has low toxicity, a simple preparation method, is easy to synthesize, and can effectively control the high conversion rate of the reactants by controlling the reaction conditions. The obtained complex has uniform activity and good stability in air or humid environment, which is convenient for storage, transportation and subsequent catalytic application.

[0028] (2) The zinc complex containing nitrogen and phosphorus double bonds in the present invention is used as a catalyst in a small amount, which can achieve large-scale polymerization and meet the needs of industrial production. In addition, the polymerization process is simple and easy to operate, easy to control, and has low requirements for equipment, which can effectively reduce production costs.

[0029] (3) The polyester preparation method of the present invention uses a zinc complex containing nitrogen and phosphorus double bonds as a catalyst, has high activity, can catalyze the ring-opening polymerization of lactide in batches, has low toxicity, good biosafety, and will not affect the subsequent application of polyester in the biomedical field. DETAILED DESCRIPTION

[0030] The present invention is described in detail below through specific implementation modes, and the characteristics and advantages of the present invention will become clearer and more specific with these descriptions.

[0031] The first aspect of the present invention is to provide a zinc complex containing a nitrogen-phosphorus double bond, in which zinc forms a di-coordination with a phosphorus imine group and an amine group or an imine group in a ligand, and the ligand comprises a diphenylphosphine group and a substituted or unsubstituted phenylenediamine group, and the two are connected by a nitrogen-phosphorus double bond.

[0032] Preferably, the zinc complex containing nitrogen and phosphorus double bonds is a complex having a structure as shown in formula (1):

[0033]

[0034] Among them, Ph is phenyl,

[0035] R is selected from hydrogen, alkyl, halo or aromatic, preferably selected from hydrogen, C1-C5 alkyl, fluorine substituent, chlorine substituent, bromine substituent, phenyl, alkylphenyl, alkoxyphenyl, more preferably hydrogen, methyl, chlorine substituent or fluorine substituent;

[0036] R0 is selected from hydrogen, alkyl or aromatic groups, preferably selected from hydrogen, C1-C5 alkyl, phenyl, more preferably hydrogen or phenyl;

[0037] X is an anion that makes the zinc complex containing nitrogen and phosphorus double bonds electrically neutral, such as chloride ion, bromide ion, nitrate ion, acetate ion, etc., preferably chloride ion.

[0038] Preferably, the ligand is selected from L1-L5:

[0039]

[0040] Among them, -Ph is phenyl.

[0041] Preferably, the zinc complex containing nitrogen and phosphorus double bonds is selected from C1-C5:

[0042] C1: R is hydrogen (H), R0 is hydrogen (H), and X is chloride ion;

[0043] C2: R is methyl (Me), R0 is hydrogen (H), and X is chloride ion;

[0044] C3: R is a chlorine substituent (-Cl), R0 is hydrogen (H), and X is a chloride ion;

[0045] C4: R is a fluorine substituent (-F), R0 is hydrogen (H), and X is a chloride ion; C5: R is a hydrogen substituent (-H), R0 is a phenyl group (Ph), and X is a chloride ion.

[0046]

[0047] The present invention also provides a method for preparing the zinc complex containing nitrogen and phosphorus double bonds, which specifically comprises the following steps:

[0048] Step 1, adding bromine to a diphenylphosphine solution to react and obtain a reaction solution I;

[0049] The solvent is selected from one or more of alcohol, ether and ketone solvents, preferably tetrahydrofuran and / or dichloromethane, more preferably dichloromethane.

[0050] The diphenylphosphomethane is selected from diphenylphosphine-substituted methanes, preferably bis(diphenylphosphine)methane.

[0051] In the diphenylphosphine solution, the molar volume ratio of diphenylphosphine to the solvent is 10 mmol:(20-80) mL, preferably 10 mmol:(30-70) mL, and more preferably 10 mmol:(40-60) mL.

[0052] The reaction temperature is -94 to 0° C., preferably -94 to -75° C., more preferably -78° C. The reaction time is 2 to 30 hours, preferably 3 to 15 hours, more preferably 8 to 12 hours.

[0053] In step 1, the reaction is carried out in a protective gas under stirring conditions. The protective gas is nitrogen or argon, preferably nitrogen.

[0054] Step 2, adding the phenylenediamine compound solution to the reaction solution I, stirring and reacting to obtain the reaction solution II;

[0055] The phenylenediamine compound is:

[0056] in,

[0057] R is selected from hydrogen, alkyl, halo or aromatic, preferably selected from hydrogen, C1-C5 alkyl, fluorine substituent, chlorine substituent, bromine substituent, phenyl, alkylphenyl, alkoxyphenyl, more preferably hydrogen, methyl, chlorine substituent or fluorine substituent;

[0058] R0 is selected from hydrogen, alkyl or aryl, preferably selected from hydrogen, C1-C5 alkyl, phenyl, more preferably hydrogen or phenyl.

[0059] The molar ratio of the phenylenediamine compound to diphenylphosphine is (0.2-2.8):1, preferably (0.3-2.5):1, and more preferably (0.4-2.2):1.

[0060] Preferably, a bromine transfer agent is added to the phenylenediamine compound solution, wherein the bromine transfer agent is one or more of primary amines and tertiary amines, preferably one or more of phenylenediamine, triethylamine, tributylamine and triethylenediamine, more preferably triethylenediamine.

[0061] The molar ratio of the bromine transfer agent to diphenylphosphine is (0.2-1.8):1, preferably (0.3-1.5):1, and more preferably (0.4-1.2):1.

[0062] The reaction temperature is -94 to 0° C., preferably -94 to -75° C., more preferably -78° C. The reaction time is 2 to 30 hours, preferably 3 to 15 hours, more preferably 8 to 12 hours.

[0063] In step 2, the reaction is carried out in a protective gas with stirring. The protective gas is nitrogen or argon, preferably nitrogen.

[0064] Step 3, post-treating the reaction solution II to obtain a ligand containing a nitrogen-phosphorus double bond;

[0065] The post-treatment includes washing, drying and column chromatography.

[0066] The washing is to add a washing liquid to the reaction solution II. The washing agent is selected from an ammonium salt aqueous solution or water, preferably an ammonium chloride aqueous solution, a sodium chloride aqueous solution, a potassium chloride aqueous solution or deionized water, more preferably an ammonium chloride aqueous solution or deionized water.

[0067] The drying is preferably vacuum drying, and the ligand solid powder is obtained after drying.

[0068] The column chromatography stationary phase is selected from silica gel or alumina, preferably alumina, and more preferably basic alumina.

[0069] Step 4: adding the zinc salt solution to the ligand solution containing nitrogen and phosphorus double bonds, stirring for reaction, and post-treating the reaction solution to obtain a zinc complex containing nitrogen and phosphorus double bonds.

[0070] In the method, the zinc salt solution is slowly added to the ligand solution containing nitrogen and phosphorus double bonds, preferably dropwise.

[0071] The molar ratio of the ligand containing nitrogen and phosphorus double bonds to the zinc salt is 1:(0.3-1.6), preferably 1:(0.5-1.4), more preferably 1:(0.7-1.2), such as 1:1, wherein the molar amount of the zinc salt is based on the molar amount of zinc therein. During the reaction, the zinc salt solution is slowly added to the ligand solution containing nitrogen and phosphorus double bonds, so that the zinc salt and the ligand containing nitrogen and phosphorus double bonds react fully. In the present invention, it is preferred that the zinc salt and the ligand containing nitrogen and phosphorus double bonds react in equimolar amounts to avoid the difficulty in removing the excess ligand or zinc salt after the reaction is completed, which affects the subsequent reaction.

[0072] The reaction temperature is 15-38°C, preferably 20-30°C; the reaction time is 6-18h, preferably 10-14h.

[0073] After the reaction is completed, the reaction solution is filtered, preferably at a filtering temperature below 20° C., the obtained precipitate is washed, the washing solution is a cold solvent, and the precipitate is dried to obtain a zinc complex containing a nitrogen-phosphorus double bond.

[0074] The present invention also provides a catalyst composition for catalyzing the polymerization of lactide. The zinc-containing complex is used as a component of the catalyst composition to catalyze the polymerization of lactide, so that the polymerization conditions of lactide are milder and the activity is higher than that of the existing process.

[0075] The catalyst composition comprises the zinc complex containing nitrogen and phosphorus double bonds. Preferably, the zinc complex containing nitrogen and phosphorus double bonds is selected from C1-C5.

[0076] Preferably, the catalyst composition further comprises an organosilicon amide metal compound, wherein the organosilicon amide metal compound is selected from one or more of organosilicon amide lithium and organosilicon amide zinc, preferably one or more of organosilicon amide lithium, and more preferably lithium bistrimethylsilylamide.

[0077] Preferably, the catalyst composition further comprises an organic alcohol, which is selected from one or more of methanol, ethanol, isopropanol, n-butanol and benzyl alcohol, preferably one or more of isopropanol, n-butanol and benzyl alcohol, and more preferably benzyl alcohol.

[0078] The molar ratio of the organosilicon amine metal compound to the zinc complex containing nitrogen and phosphorus double bonds is (1-10):1, preferably (2-5):1, and more preferably 4:1.

[0079] The molar ratio of the zinc complex containing nitrogen and phosphorus double bonds to the organic alcohol is 1:(1-11), preferably 1:(1-8), and more preferably 1:(1-5).

[0080] The present invention also provides a method for preparing polylactide, which comprises adding lactide to a solution containing the catalyst composition to perform polymerization. The method specifically comprises the following steps:

[0081] Step a, adding the catalyst composition into a reaction solvent, aging, and obtaining a mixed solution;

[0082] The reaction solvent is selected from one or more of aromatic hydrocarbons, such as toluene, xylene, chlorobenzene, halogenated alkane solvents, such as dichloromethane, and ethers, such as tetrahydrofuran, preferably toluene and / or dichloromethane, more preferably toluene.

[0083] The aging is to age the zinc complex containing nitrogen and phosphorus double bonds and the organosilicon amine metal compound in a reaction solvent to effectively activate the zinc complex containing nitrogen and phosphorus double bonds. The aging temperature is 15-35° C., preferably 20-30° C.; the aging time is 0.1-2h, preferably 0.5-1h, such as 0.5h.

[0084] In the present invention, step a is carried out under anhydrous and oxygen-free conditions, preferably in a dry nitrogen environment, such as in a glove box filled with dry nitrogen.

[0085] Step b, adding lactide monomer to the mixed solution, heating for reaction, and obtaining a reaction solution;

[0086] The molar ratio of the lactide monomer to the zinc complex containing nitrogen and phosphorus double bonds is (100-5000):1, preferably (200-2500):1, and more preferably (250-2000):1.

[0087] The molar volume ratio of the lactide monomer to the solvent is (1-100) mmol: (0.4-5) mL, preferably (1.5-50) mmol: (0.6-3) mL, and more preferably (2.5-20) mmol: (0.8-2) mL.

[0088] The reaction temperature is 15-100°C, preferably 40-90°C, such as 80°C; the reaction time is 2-30min, preferably 8-16min, such as 10min.

[0089] Step c, post-treating the reaction solution to obtain polylactide.

[0090] After the reaction is completed, a cold precipitation solvent is added to precipitate the product, and the product is filtered and dried to obtain polylactide. The precipitation solvent is selected from alcohol solvents, preferably one or more of methanol, ethanol and propanol, and more preferably methanol.

[0091] The zinc complex containing nitrogen-phosphorus double bonds provided in the present invention can be used as a catalyst to catalyze the ring-opening polymerization of lactide to prepare polylactide, and has high catalytic activity. Compared with the existing process, the catalyst in the present invention has higher catalytic activity and shortens the polymerization time, thereby achieving the purpose of optimizing the synthesis process of polylactide and reducing production costs.

[0092] Example

[0093] Example 1

[0094] At -78 ° C, under nitrogen atmosphere, 0.159 g of liquid bromine was slowly added dropwise to a 50 mL dichloromethane solution of 3.84 g (about 0.01 mol) of bis(diphenylphosphine). As the reaction proceeded, the solution quickly became turbid and then turned into a clear and transparent yellow solution, and then heated to room temperature and stirred for 2 hours. Cooled to -78 ° C again, 2.16 g (about 0.02 mol) of 1,2-phenylenediamine in 20 mL of dichloromethane was slowly added dropwise, wherein 1,2-phenylenediamine is both a reactant and a bromine transfer agent. The solution immediately became turbid. After stirring at -78 ° C for 1 hour, the cold bath was removed and stirred at room temperature for 12 hours, during which a light yellow suspension was formed. The suspension was rinsed with water twice, the organic layer was dried with anhydrous MgSO4, and the solvent was removed under vacuum to obtain a light yellow solid. The light yellow solid was purified by column chromatography (volume ratio of petroleum ether and ethyl acetate was 1:1) with basic alumina as the stationary phase. The separated ligand L1 was a light yellow powder with a molar yield of 24%.

[0095] 0.5 g (about 0.001 mol) of ligand L1 was added to a 50 mL Shrek tube, and 10 mL of ethanol was added. The mixture was stirred at room temperature until L1 was completely dissolved. 0.14 g (about 0.001 mol) of zinc chloride was dissolved in 5 mL of ethanol. The zinc chloride ethanol solution was dropped into the ethanol solution of L1, and then stirred at room temperature for 12 hours. A white solid was generated. After the reaction was completed, the white solid was filtered, washed three times with ethanol, and dried naturally to obtain a zinc complex C1 containing a nitrogen-phosphorus double bond as a white solid with a molar yield of 85%.

[0096] The ligand L1 and the zinc complex C1 containing nitrogen and phosphorus double bonds were characterized by NMR. The NMR data are as follows:

[0097] Ligand L1:

[0098] 1 H NMR (400MHz, CDCl3, ppm): δ7.78-7.74(m,4H,PPh2),7.50-7.21(m,16H,PPh2),6.64-6.62(d, 1H,Ph),6.53-6.50(t,1,Ph),6.31-6.27(t,1H,Ph),6.21-6.20(d,1,Ph),3,25(d,2H,PCH2P).

[0099] 13 C NMR (100MHz, CDCl3, ppm): δ141.88,141.67,138.39,138.32,138.17,138.03,132.86,132.65,132.04,132.02,131.95,131.93,131.79, 131.66,131.64,130.90,128.76,128.69,128.57,128.48,128.41,119.85,119.75,118.15,117.82,113.92,30.62,30.27,29.83,29.51.

[0100] 31 P NMR (162MHz, CDCl3, ppm): δ5.76(d,1P),-27.77(d,1P).

[0101] Zinc complex C1 containing nitrogen-phosphorus double bond:

[0102] 1 H NMR (400MHz, CDCl3, ppm): δ7.93-7.88(m,4H,PPh2),7.52-7.45(m,2H,PPh2),7.39-7.36(m,8H,PPh2),7.21-7.17(m,6 H,PPh2),7.14-7.11(d,1H,Ph),6.64-6.63(m,2,Ph),6.26-6.24(m,2,Ph),4.23(s,2H,NH2),3.97-3.93(d,2H,PCH2P).

[0103] 13C NMR (100MHz, CDCl3, ppm): δ144.02,135.07,134.99,133.28,133.25,133.11,133.08,133.02,13 2.98,132.82,129.42,129.18,129.06,128.76,128.68,127.38,124.65,122.76,120.13,119.63.

[0104] 31 P NMR (162MHz, CDCl3, ppm, ppm): δ-33.31 (d, 1P), 27.64 (d, 1P). Example 2

[0105] At -78 ° C, under nitrogen atmosphere, 0.159 g of liquid bromine was slowly added dropwise to a 50 mL dichloromethane solution of 3.84 g of bis(diphenylphosphine). As the reaction proceeded, the solution quickly became turbid and then turned into a clear and transparent yellow solution, and then it was heated to room temperature and stirred for 2 hours. It was cooled to -78 ° C again, and a dichloromethane solution of 0.56 g (about 0.005 mol) of triethylenediamine and 1.22 g (about 0.01 mol) of 2,3-diaminotoluene was slowly added dropwise, and the solution immediately became turbid. After stirring at -78 ° C for 1 hour, the cold bath was removed and stirred at room temperature for 12 hours, during which time a brown suspension was formed. The suspension was rinsed with water twice, the organic layer was dried with anhydrous MgSO4, and the solvent was removed under vacuum to obtain a light brown solid. The light brown solid was purified by column chromatography (the volume ratio of petroleum ether and ethyl acetate was 4:1), and the isolated ligand L2 was a light yellow powder with a molar yield of 17%.

[0106] 0.5 g of ligand L2 was added to a 50 mL Shrek tube, and 10 mL of ethanol solution was added, and the mixture was stirred at room temperature until L2 was completely dissolved. 0.135 g of zinc chloride was dissolved in 5 mL of ethanol solution, and the zinc chloride ethanol solution was dropped into the ethanol solution of L2, and then stirred at room temperature for 12 hours. A white solid was generated. After the reaction was completed, the white solid was filtered, washed three times with ethanol, and dried naturally to obtain a zinc complex C2 containing a nitrogen-phosphorus double bond, and the molar yield was 85%.

[0107] The ligand L2 and the zinc complex C2 containing nitrogen and phosphorus double bonds were characterized by NMR. The NMR data are as follows:

[0108] Ligand L2:

[0109] 1H NMR (400MHz, CDCl3, ppm): δ7.78-7.66(m,4H,PPh2),7.46-7.13(m,16H,PPh2,NPh),6.34-6.32 (d,1H,Ph),6.16-6.13(t,1H,Ph),6.03-6.01(d,1H,Ph),3,15(d,2H,PCH2P),2.05(s,1H,Me).

[0110] 13 C NMR (100MHz, CDCl3, ppm): δ,138.40,138.32,138.25,137.71,132.86,132.65,132.05,132.03,131.98,131.95,131.93,131.60 ,131.58,131.09,128.74,128.67,128.56,128.46,128.39,121.27,119.70,117.43,117.33,116.94,30.65,30.33,17.99,17.94

[0111] 31 P NMR (162MHz, CDCl3, ppm): δ5.78(d,1P),-27.72(d,1P).

[0112] Zinc complex C2 containing nitrogen-phosphorus double bond:

[0113] 1 H NMR (400MHz, CDCl3, ppm): δ7.91-7.88(m,4H,PPh2),7.51-7.15(m,16H,PPh2,NPh),6.54-6. 53(m,1H,Ph),6.12-6.10(t,1H,Ph),4.31(s,2H,NH2),3,98(d,2H,PCH2P),2.31(s,1H,Me).

[0114] 13 C NMR (100MHz, CDCl3, ppm): δ143.96,135.46,135.38,135.33,135.29,133.16,133.10,133.02,132.82,12 9.33,129.13,129.01,128.70,128.67,128.63,128.49,126.45,123.69,122.81,121.34,117.88,117.77.

[0115] 31P NMR (162MHz, CDCl3, ppm): δ-33.31(d,1P),27.66(d,1P).

[0116] Example 3

[0117] The preparation was carried out according to the method in Example 2, except that 1.42 g (about 0.01 mol) of 3-chloro-1,2-phenylenediamine was added instead of 2,3-diaminotoluene to obtain 1.31 g of ligand L3, which was a light yellow solid with a molar yield of 25%. A zinc chloride ethanol solution containing 0.129 g of zinc chloride was added to coordinate with 0.5 g of L3 to obtain 0.52 g of zinc complex C3 containing a nitrogen-phosphorus double bond, which was a white solid with a molar yield of 83%.

[0118] The ligand L3 and the zinc complex C3 containing nitrogen and phosphorus double bonds were characterized by NMR. The NMR data are as follows:

[0119] Ligand L3:

[0120] 1 H NMR (400MHz, CDCl3, ppm): δ7.78-7.66(m,4H,PPh2),7.46-7.13(m,16H,PPh2,NPh),6.34-6.32 (d,1H,Ph),6.16-6.13(t,1H,Ph),6.03-6.01(d,1H,Ph),3.86(s,2H,NH2),3.21(d,2H,PCH2P).

[0121] 13 C NMR (100MHz, CDCl3, ppm): δ139.22,138.70,138.13,138.06,137.98,137.91,132.82,132.61,131.95,131.86,131.84,131.42,1 31.26,131.16,130.51,128.96,128.88,128.81,128.69,128.51,128.44,118.06,117.29,117.19,116.91,30.42,30.09,29.33.

[0122] 31 P NMR (162MHz, CDCl3, ppm): δ5.96(d,1P),-27.72(d,1P).

[0123] Zinc complex C3 containing nitrogen-phosphorus double bond:

[0124] 1H NMR (400MHz, CDCl3, ppm): δ7.90-7.88(m,4H,PPh2),7.52-7.16(m,16H,PPh2,NPh), 6.54-6.52(d,1H,Ph),6.12-6.10(t,1H,Ph),4.32(s,2H,NH2),4.03(d,2H,PCH2P).

[0125] 13 C NMR (100MHz, CDCl3, ppm): δ139.22,139.70,139.13,138.06,134.78,134.71,133.82,133.61,132.97,132.84,132.76,130.42,1 30.26,130.16,129.51,127.96,127.87,127.81,126.69,126.51,126.34,119.06,118.29,116.33,115.89,32.36,32.25,29.77.

[0126] 31 P NMR (162MHz, CDCl3, ppm): δ-33.44(d,1P),-27.88(d,1P). Example 4

[0127] The preparation was carried out according to the method in Example 2, except that 0.63 g (about 0.005 mol) of 2,3-diaminofluorobenzene was added instead of 2,3-diaminotoluene to obtain 0.33 g of ligand L4, which was a light yellow solid with a molar yield of 13%. The above process was repeated to prepare L4 for use. 0.129 g of zinc chloride was coordinated with 0.5 g of L4 to obtain 0.52 g of zinc complex C4 containing nitrogen and phosphorus double bonds, which was a white solid with a molar yield of 83%.

[0128] The ligand L4 and the zinc complex C4 containing nitrogen and phosphorus double bonds were characterized by NMR. The NMR data are as follows:

[0129] Ligand L4:

[0130] 1 H NMR (400MHz, CDCl3, ppm): δ7.78-7.66(m,4H,PPh2),7.46-7.13(m,16H,PPh2,NPh),6.34-6.32 (d,1H,Ph),6.16-6.13(t,1H,Ph),6.03-6.01(d,1H,Ph),3.86(s,2H,NH2),3,21(d,2H,PCH2P).

[0131] 13 C NMR (100MHz, CDCl3): δ139.56,138.70,138.13,138.06,137.98,137.91,132.82,132.61,131.95,131.89,131.78,131.56,131 .26,131.16,130.51,128.96,128.88,128.81,128.69,128.51,128.44,118.06,117.29,117.19,116.91,30.58,30.56,29.45.

[0132] 31 P NMR (162MHz, CDCl3, ppm): δ5.72(d,1P),-27.62(d,1P).

[0133] Zinc complex C4 containing nitrogen-phosphorus double bond:

[0134] 1 H NMR (400MHz, CDCl3, ppm): δ7.93-7.88(m,4H,PPh2),7.53-7.17(m,16H,PPh2,NPh), 6.54-6.52(d,1H,Ph),6.12-6.10(t,1H,Ph),4.32(s,2H,NH2),3.99(d,2H,PCH2P).

[0135] 13 C NMR (100MHz, CDCl3, ppm): δ145.56,139.28,136.55,134.18,133.92,133.41,133.34,133.19,132.89,132. 76,129.54,129.43,129.78,128.98,128.58,127.48,124.76,122.54,120.25,119.16,30.42,30.09,29.33.

[0136] 31 P NMR (162MHz, CDCl3, ppm): δ-33.44(d,1P),27.88(d,1P). Example 5

[0137] The preparation was carried out according to the method in Example 2, except that 0.92 g (about 0.005 mol) of o-aminodiphenylamine was added instead of 2,3-diaminotoluene to obtain 0.59 g of ligand L5, which was a light yellow solid with a molar yield of 21%. 0.12 g of zinc chloride was coordinated with 0.5 g of L5 to obtain 0.53 g of zinc complex C5 containing nitrogen and phosphorus double bonds, which was a white solid with a molar yield of 85%.

[0138] The ligand L5 and the zinc complex C5 containing nitrogen and phosphorus double bonds were characterized by NMR. The NMR data are as follows:

[0139] Ligand L5:

[0140] 1 H NMR (400MHz, CDCl3, ppm): δ7.87-7.62(m,4H,PPh2),7.46-7.03(m,19H,PPh2,NPh),6.78-6.74( t,1H,Ph),6.53-6.50(t,1,Ph),6.31-6.27(t,1H,Ph),6.21-6.20(d,1,Ph),3,15(d,2H,PCH2P).

[0141] 13 C NMR (100MHz, CDCl3): δ132.81,132.60,131.95,131.93,131.86,131.84,131.79,131.76, 128.84,128.76,128.5,128.49,128.42,116.05,115.95,115.23,115.11,104.83,104.64.

[0142] 31 P NMR (162MHz, CDCl3, ppm): δ6.50(d,1P),-27.77(d,1P).

[0143] Zinc complex C5 containing nitrogen-phosphorus double bond:

[0144] 1H NMR (400MHz, CDCl3, ppm): δ7.78-7.66(m,4H,PPh2),7.46-7.13(m,19H,PPh2,NPh),6.34-6.32 (d,1H,Ph),6.16-6.13(t,1H,Ph),6.03-6.01(d,1H,Ph),4.06(s,2H,NH2),3,98(d,2H,PCH2P).

[0145] 13C NMR (100MHz, CDCl3, ppm): δ133.46,133.43,133.06,133.02,132.96,132.93,13 2.86,129.57,129.28,129.15,128.79,128.71,123.35,122.45,106.49,106.29.

[0146] 31 P NMR (162MHz, CDCl3, ppm): δ-34.44(d,1P),28.83(d,1P)

[0147] Example 6

[0148] In a nitrogen atmosphere glove box, 10 μmol of C2 and 1 ml of toluene were added into a 100 ml Shrek bottle and shaken for a while. Then, 1 M solution of lithium bistrimethylsilylamide in tetrahydrofuran (wherein the content of lithium bistrimethylsilylamide was 40 μmol) was added and the catalyst mixture was stirred at room temperature for 30 min for aging.

[0149] Under nitrogen atmosphere, 0.36 g (about 2.5 mmol) of L-lactide was added to the catalyst mixture and reacted at 20°C for 10 min. After the reaction, the reaction liquid was directly taken to detect the conversion rate of L-lactide monomer. Then, cold methanol was added to the reaction container and stirred to obtain a white solid. The solid was filtered and dried in a vacuum drying oven for 24 hours to collect the product polylactide. 1 The conversion rate of L-lactide monomer was 33% as determined by HNMR, and the number average molecular weight of polylactide was 1.17×10 4 g / mol, and the molecular weight distribution index is 1.61.

[0150] Example 7

[0151] Polylactide was prepared according to the preparation method in Example 6, except that the reaction temperature was 40°C. The number average molecular weight of the polylactide was 1.48×10 4 g / mol, the molecular weight distribution index was 1.37, and the monomer conversion rate was 90%.

[0152] Example 8

[0153] Polylactide was prepared according to the preparation method in Example 6, except that the reaction temperature was 60°C. The number average molecular weight of the polylactide was 1.30×10 4 g / mol, the molecular weight distribution index was 1.77, and the monomer conversion rate was 98%.

[0154] Example 9

[0155] Polylactide was prepared according to the preparation method in Example 6, except that the amount of L-lactide added was 0.72 g (about 5 mmol), the reaction temperature was 60°C, and the reaction time was 5 minutes. The number average molecular weight of the polylactide was 1.53×10 4 g / mol, the molecular weight distribution index was 1.91, and the monomer conversion rate was 83%.

[0156] Example 10

[0157] Polylactide was prepared according to the preparation method in Example 9, except that the reaction time was 10 minutes. The number average molecular weight of polylactide was 1.28×10 4 g / mol, the molecular weight distribution index was 1.80, and the monomer conversion rate was 97%.

[0158] Embodiment 11

[0159] Polylactide was prepared according to the preparation method in Example 9, except that the amount of L-lactide added was 1.44 g (about 10 mmol) and the reaction time was 10 minutes. The number average molecular weight of the polylactide was 1.40×10 4 g / mol, the molecular weight distribution index was 1.89, and the monomer conversion rate was 73%.

[0160] Example 12

[0161] Polylactide was prepared according to the preparation method in Example 11, except that the reaction temperature was 70°C. The number average molecular weight of the polylactide was 1.39×10 4 g / mol, the molecular weight distribution index was 1.63, and the monomer conversion rate was 79%.

[0162] Embodiment 13

[0163] Polylactide was prepared according to the preparation method in Example 11, except that the reaction temperature was 80°C. The number average molecular weight of the polylactide was 1.43×10 4 g / mol, the molecular weight distribution index was 1.65, and the monomer conversion rate was 94%.

[0164] Embodiment 14

[0165] Polylactide was prepared according to the preparation method in Example 11, except that the reaction temperature was 90°C. The number average molecular weight of the polylactide was 1.36×10 4 g / mol, the molecular weight distribution index was 1.92, and the monomer conversion rate was 95%.

[0166] Embodiment 15

[0167] Polylactide was prepared according to the preparation method in Example 13, except that the reaction solvent was 1 mL of n-hexane instead of toluene. The number average molecular weight of polylactide was 1.73×10 4 g / mol and 0.26×10 4 g / mol, with a bimodal distribution of molecular weight distribution index of 1.15 and 1.00. The monomer conversion rate was 15%.

[0168] Example 16

[0169] Polylactide was prepared according to the preparation method in Example 13, except that the reaction solvent was 1 mL of tetrahydrofuran instead of toluene. The number average molecular weight of polylactide was 1.36×10 4 g / mol, the molecular weight distribution index was 1.62, and the monomer conversion rate was 95%.

[0170] Embodiment 17

[0171] Polylactide was prepared according to the preparation method in Example 13, except that the reaction solvent was 1 mL of dichloromethane. The number average molecular weight of polylactide was 2.12×10 4 g / mol, the molecular weight distribution index was 1.89, and the monomer conversion rate was 88%.

[0172] Embodiment 18

[0173] Polylactide was prepared according to the preparation method in Example 13, except that the amount of L-lactide added was 1.80 g (about 15 mmol). The number average molecular weight of polylactide was 1.37×10 4 g / mol, the molecular weight distribution index was 1.96, and the monomer conversion rate was 89%.

[0174] Embodiment 19

[0175] Polylactide was prepared according to the preparation method in Example 13, except that the amount of L-lactide added was 2.16 g (about 20 mmol). The number average molecular weight of polylactide was 2.40×10 4 g / mol, the molecular weight distribution index was 1.84, and the monomer conversion rate was 66%.

[0176] Embodiment 20

[0177] Polylactide was prepared according to the preparation method in Example 19, except that 0.1 mL of benzyl alcohol toluene solution (concentration of 0.1 mmol / mL) was added. The number average molecular weight of polylactide was 2.23×10 4 g / mol, the molecular weight distribution index was 1.80, and the monomer conversion rate was 83%.

[0178] Embodiment 21

[0179] Polylactide was prepared according to the preparation method in Example 19, except that 0.5 mL of benzyl alcohol toluene solution (concentration of 0.1 mmol / mL) was added. The number average molecular weight of polylactide was 1.23×10 4 g / mol and 0.48×10 4 g / mol, the molecular weight distribution index was a bimodal distribution of 1.18 and 1.04. The monomer conversion rate was 88%.

[0180] Embodiment 22

[0181] Polylactide was prepared according to the preparation method in Example 13, except that catalyst C2 was replaced by catalyst C1. The number average molecular weight of polylactide was 1.61×10 4 g / mol, the molecular weight distribution index was 1.78, and the monomer conversion rate was 92%.

[0182] Embodiment 23

[0183] Polylactide was prepared according to the preparation method in Example 13, except that catalyst C2 was replaced by catalyst C3. The number average molecular weight of polylactide was 1.41×10 4 g / mol, the molecular weight distribution index was 1.47, and the monomer conversion rate was 94%.

[0184] Embodiment 24

[0185] Polylactide was prepared according to the preparation method in Example 13, except that catalyst C2 was replaced by catalyst C4. The number average molecular weight of polylactide was 2.07×10 4 g / mol, the molecular weight distribution index was 1.85, and the monomer conversion rate was 95%.

[0186] Embodiment 25

[0187] Polylactide was prepared according to the preparation method in Example 13, except that catalyst C2 was replaced by catalyst C5. The number average molecular weight of polylactide was 2.19×10 4 g / mol, the molecular weight distribution index was 1.84, and the monomer conversion rate was 95%.

[0188] Embodiment 26

[0189] Polylactide was prepared according to the preparation method in Example 19, except that catalyst C2 was replaced by catalyst C1. The number average molecular weight of polylactide was 2.13×10 4 g / mol, the molecular weight distribution index was 1.76, and the monomer conversion rate was 70%.

[0190] Embodiment 27

[0191] Polylactide was prepared according to the preparation method in Example 19, except that catalyst C2 was replaced by catalyst C3. The number average molecular weight of polylactide was 2.56×10 4 g / mol, the molecular weight distribution index was 1.82, and the monomer conversion rate was 79%.

[0192] Embodiment 28

[0193] Polylactide was prepared according to the preparation method in Example 19, except that catalyst C2 was replaced by catalyst C4. The number average molecular weight of polylactide was 2.87×10 4 g / mol, the molecular weight distribution index was 1.86, and the monomer conversion rate was 89%.

[0194] Embodiment 29

[0195] Polylactide was prepared according to the preparation method in Example 19, except that catalyst C2 was replaced by catalyst C5. The number average molecular weight of polylactide was 2.93×10 4 g / mol, the molecular weight distribution index was 1.79, and the monomer conversion rate was 45%.

[0196] Comparative Example

[0197] Comparative Example 1

[0198] Polylactide was prepared according to the preparation method in Example 13, except that the reaction solvent was 1 mL of n-hexane. The number average molecular weight of polylactide was 1.73×10 4 g / mol and 0.26×10 4 g / mol, with a bimodal distribution of molecular weight distribution index of 1.15 and 1.00. The monomer conversion rate was 15%.

[0199] Comparative Example 2

[0200] Polylactide was prepared according to the preparation method in Example 13, except that the reaction solvent was 1 mL of tetrahydrofuran. The number average molecular weight of polylactide was 1.36×10 4 g / mol, the molecular weight distribution index was 1.62, and the monomer conversion rate was 95%.

[0201] Comparative Example 3

[0202] Polylactide was prepared according to the preparation method in Example 13, except that the reaction solvent was 1 mL of dichloromethane. The number average molecular weight of polylactide was 2.12×10 4 g / mol, the molecular weight distribution index was 1.89, and the monomer conversion rate was 88%.

[0203] From the comparative examples, it can be seen that the conversion rate in the polymerization system with n-hexane as solvent is the lowest, only 15%, and at the same time, there is an obvious bimodal distribution of molecular weight, which may be due to the low polarity of the solvent leading to reduced activity, and may also be due to the obvious bimodal distribution caused by the presence of two active centers. When the solvent is dichloromethane and tetrahydrofuran, the polymerization activity is slightly reduced, and the monomer conversion rate is much higher than the conversion rate when hexane is used as the solvent, which may be caused by the different solubility in different solvents.

[0204] The present invention has been described in detail above in conjunction with specific embodiments and / or exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, various equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

Claims

1. A zinc complex containing a nitrogen-phosphorus double bond, wherein zinc forms a di-coordination with a phosphorus imine group and an amine group or an imine group in a ligand, and the ligand comprises a diphenylphosphine group and a substituted or unsubstituted phenylenediamine group, and the two are connected by a nitrogen-phosphorus double bond.

2. The zinc complex containing nitrogen and phosphorus double bonds according to claim 1, characterized in that It is a complex having a structure of formula (1): Among them, Ph is phenyl, R is selected from hydrogen, alkyl, halo or aromatic, preferably selected from hydrogen, C1-C5 alkyl, fluorine substituent, chlorine substituent, bromine substituent, phenyl, alkylphenyl, alkoxyphenyl, more preferably hydrogen, methyl, chlorine substituent or fluorine substituent; R0 is selected from hydrogen, alkyl or aromatic groups, preferably selected from hydrogen, C1-C5 alkyl, phenyl, more preferably hydrogen or phenyl; X is an anion that makes the zinc complex containing nitrogen and phosphorus double bonds electrically neutral; Preferably, the zinc complex containing nitrogen and phosphorus double bonds is selected from C1-C5: C1: R is hydrogen (H), R0 is hydrogen (H), and X is chloride ion; C2: R is methyl (Me), R0 is hydrogen (H), and X is chloride ion; C3: R is a chlorine substituent (-Cl), R0 is hydrogen (H), and X is a chloride ion; C4: R is a fluorine substituent (-F), R0 is hydrogen (H), and X is a chloride ion; C5: R is a hydrogen substituent (-H), R0 is a phenyl group (Ph), and X is a chloride ion.

3. A method for preparing a zinc complex containing nitrogen and phosphorus double bonds according to claim 1 or 2, characterized in that: The method specifically comprises the following steps: Step 1, adding bromine to a diphenylphosphine solution to react and obtain a reaction solution I; Step 2, adding the phenylenediamine compound solution to the reaction solution I, stirring and reacting to obtain the reaction solution II; Step 3, post-treating the reaction solution II to obtain a ligand containing a nitrogen-phosphorus double bond; Step 4: adding the zinc salt solution to the ligand solution containing nitrogen and phosphorus double bonds, stirring for reaction, and post-treating the reaction solution to obtain a zinc complex containing nitrogen and phosphorus double bonds.

4. The method according to claim 3, characterized in that In step 2, the phenylenediamine compound is: in, R is selected from hydrogen, alkyl, halo or aromatic, preferably selected from hydrogen, C1-C5 alkyl, fluorine substituent, chlorine substituent, bromine substituent, phenyl, alkylphenyl, alkoxyphenyl, more preferably hydrogen, methyl, chlorine substituent or fluorine substituent; R0 is selected from hydrogen, alkyl or aryl, preferably selected from hydrogen, C1-C5 alkyl, phenyl, more preferably hydrogen or phenyl.

5. A catalyst composition for catalyzing the polymerization of lactide, characterized in that: The catalyst composition comprises the zinc complex containing nitrogen and phosphorus double bonds according to claim 1 or 2, The catalyst composition further comprises an organosilicon amine metal compound and an organic alcohol.

6. The catalyst composition according to claim 5, characterized in that The zinc complex containing nitrogen and phosphorus double bonds is selected from C1-C5, The organosilicon amide metal compound is selected from one or more of organosilicon amide lithium and organosilicon amide zinc, preferably one or more of organosilicon amide lithium, more preferably lithium bistrimethylsilylamide, The organic alcohol is selected from one or more of methanol, ethanol, isopropanol, n-butanol and benzyl alcohol, preferably one or more of isopropanol, n-butanol and benzyl alcohol, more preferably benzyl alcohol.

7. A method for preparing polylactide, characterized in that: The method comprises adding lactide to a solution containing the catalyst composition according to claim 5 or 6 to carry out polymerization.

8. The preparation method according to claim 7, characterized in that: The method specifically comprises the following steps: Step a, adding the catalyst composition into a reaction solvent, aging, and obtaining a mixed solution; Step b, adding lactide monomer to the mixed solution, heating for reaction, and obtaining a reaction solution; Step c, post-treating the reaction solution to obtain polylactide.

9. The preparation method according to claim 8, characterized in that: In step a, the reaction solvent is selected from one or more of aromatic hydrocarbons, such as toluene, xylene, chlorobenzene, halogenated alkane solvents, such as dichloromethane, and ethers, such as tetrahydrofuran, preferably toluene and / or dichloromethane.

10. The preparation method according to claim 8, characterized in that: In step b, The molar ratio of the lactide monomer to the zinc complex containing nitrogen and phosphorus double bonds is (100-5000):1, preferably (200-2500):1, and more preferably (250-2000):1; The molar volume ratio of the lactide monomer to the solvent is (1-100) mmol: (0.4-5) mL, preferably (1.5-50) mmol: (0.6-3) mL, and more preferably (2.5-20) mmol: (0.8-2) mL; The reaction temperature is 15-100° C., preferably 40-90° C.; the reaction time is 2-30 min, preferably 8-16 min.

Citation Information

Patent Citations

  • Zinc complex and preparation method thereof

    CN115368411A

  • Zinc catalyst for catalyzing ring-opening polymerization of cyclic esters and controlled depolymerization of polyester materials and catalytic method therefor

    WO2022041326A1