Preparation of TS-1 molecular sieve catalyst and application of TS-1 molecular sieve catalyst in epoxidized chloropropene
An amphiphilic TS-1 catalyst was prepared by combining soft and hard dual template agents and low-temperature-high-temperature stepwise crystallization with organosilicon modification. This solved the problem of poor activity and stability of existing TS-1 catalysts in the hydrogen peroxide-based epichlorohydrin process, and achieved a reduction in solvent usage and cost.
Patent Information
- Application Number
- CN202411120408.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
The existing TS-1 catalyst has problems such as poor catalytic activity and stability, large solvent consumption and high energy consumption in the hydrogen peroxide method for epichlorohydrin production, which affects the economic efficiency of the process.
The morphology and porous structure of the catalyst were controlled by using soft and hard dual template agents, and the hydrolysis rate of silicon/titanium was controlled by low-temperature-high-temperature stepwise crystallization. Combined with organosilicon modification, an amphiphilic TS-1 catalyst was prepared.
The catalyst's skeletal titanium content and pore abundance were increased, enabling heterogeneous epoxidation of chloropropylene, reducing solvent usage, lowering costs, and enhancing catalytic activity and stability.
Smart Images

Figure CN119016100A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a TS-1 molecular sieve catalyst, and in particular to a method for preparing an amphiphilic TS-1 catalyst. The amphiphilic TS-1 catalyst is prepared through the steps of hydrothermal crystallization, forming calcination and modification. Background Art
[0002] Epoxy resins are widely used in aerospace, new energy, electrical and electronic, rail transit, engineering and construction and other industrial fields. The development of emerging applications such as 5G, wind power, and water-based coatings has driven the rapid growth of epoxy resin demand. It is estimated that the average annual compound growth rate of epoxy resins will be about 6% from 2021 to 2025. It is estimated that my country's epoxy resin production capacity will reach 4.9 million tons in 2025. Based on the unit consumption of epichlorohydrin (ECH) of 0.54t / t epoxy resin, the total demand for ECH is as high as 2.5 million tons.
[0003] The hydrogen peroxide method of epichlorohydrin has the advantages of being green, environmentally friendly, high atom economy, mild reaction conditions and a wide range of raw material sources, but the process has high requirements for catalysts. The TS-1 catalyst currently under development has a large number of silanol groups on the surface and has good hydrophilicity. Allyl chloride cannot efficiently enter the active site and needs to be epoxidized under homogeneous conditions. At the same time, the catalyst has a short single-pass life and poor stability, which affects the economic efficiency of the hydrogen peroxide method of epichlorohydrin. The main problems of hydrogen peroxide method ECH using titanium silicon molecular sieve as catalyst are: 1. The amount of solvent used in the process is large, the recovery energy consumption is high, and the economic efficiency of the process is reduced; 2. The catalyst activity and stability are poor, and the reaction temperature is high (40-60℃).
[0004] Therefore, there is an urgent need in the art to develop an improved method for preparing TS-1 molecular sieve catalysts, which can increase the content of catalytically active skeleton titanium in TS-1 catalysts. The TS-1 molecular sieve catalyst prepared by the method has high catalytic activity and good stability, and the use of the TS-1 catalyst can reduce the cost of the hydrogen peroxide method epichlorohydrin process. Summary of the invention
[0005] The first aspect of the present disclosure provides a method for preparing a TS-1 molecular sieve catalyst, the method comprising the following steps:
[0006] (1) mixing a first template, an alkali source, a silicon source and water to obtain a first mixed solution, wherein the first template comprises at least one tetraalkylammonium hydroxide or tetraalkylammonium halide, the alkali source comprises ammonia or alkylamine, and the molar ratio of the first template, the alkali source, the silicon source and the water is 1:0-1:1-8:20-40;
[0007] (2) adding a second template to the first mixed solution to obtain a second mixed solution, wherein the second template comprises at least one of polyethylene glycol monoalkyl ether, polyethylene glycol dialkyl ether, polyethylene glycol alkyl phenyl ether, polypropylene glycol monoalkyl ether, polypropylene glycol dialkyl ether or polypropylene glycol alkyl phenyl ether, wherein the amount of the second template is 5-20%, based on the weight of the silicon source;
[0008] (3) dissolving a titanium source in a polar aprotic solvent to obtain a third mixed solution, wherein the molar ratio of the titanium source to the silicon source is 0.02-0.06:1, and the weight ratio of the titanium source to the polar aprotic solvent is 1:1-10;
[0009] (4) mixing the second mixed solution and the third mixed solution and performing low-temperature and high-temperature fractional crystallization;
[0010] (5) Drying, molding, and calcining the reaction solution after crystallization to obtain a TS-1 molecular sieve catalyst.
[0011] In one embodiment of the present invention, the silicon source includes at least one alkyl orthosilicate or alkyl metasilicate.
[0012] In one embodiment of the present invention, the titanium source comprises at least one of titanium tetrachloride, metatitanic acid, orthotitanic acid or tetraalkyl titanate.
[0013] In one embodiment of the present invention, the polar aprotic solvent comprises DMF, DMSO, 1,4-dioxane, THF or a combination thereof, preferably THF.
[0014] In one embodiment of the present invention, the low-temperature and high-temperature stepwise crystallization includes crystallization at 60-100° C., preferably 70-90° C., for 12-48 hours, and crystallization at 120-180° C., preferably 140-160° C., for 12-48 hours.
[0015] In one embodiment of the present invention, the molding step comprises mixing the dried TS-1 crystallized powder with a sol and an organic binder and then extruding the mixture into a mold.
[0016] In one embodiment of the present invention, the method further comprises (6) modifying the TS-1 molecular sieve catalyst with organosilicon in the presence of a modifying solvent, wherein the weight ratio of the organosilicon to the TS-1 molecular sieve catalyst is 0.02:1-2:1.
[0017] In one embodiment of the present invention, the modified solvent comprises at least one of the following solvents: methanol, ethanol, isopropanol, tetrahydrofuran, toluene and DMF, preferably tetrahydrofuran.
[0018] In one embodiment of the present invention, the organosilicon includes polyethylene glycol bistriethoxysilane or polyethylene glycol triethoxysilane.
[0019] In one embodiment of the present invention, the modification is carried out by a hydrothermal method, the modification temperature is 60-150° C., and the modification time is 1-24 hours.
[0020] A second aspect of the present disclosure provides a TS-1 molecular sieve catalyst prepared by the method described in the present disclosure.
[0021] A third aspect of the present disclosure provides a method for preparing epichlorohydrin by epoxidizing allyl chloride, the method comprising reacting allyl chloride, hydrogen peroxide, a catalytic amount of a solvent and the TS-1 molecular sieve catalyst according to the present disclosure.
[0022] In one embodiment of the present invention, the molar ratio of hydrogen peroxide to allyl chloride is 1:1-1:4.
[0023] In one embodiment of the present invention, the amount of the solvent is 1-10% of the total mass of the hydrogen peroxide and allyl chloride.
[0024] In one embodiment of the present invention, the reaction temperature is 15-40°C.
[0025] The fourth aspect of the present disclosure provides an epichlorohydrin product prepared according to the method for preparing epichlorohydrin by epoxidizing allyl chloride described in the present disclosure.
[0026] The advantages of this application are:
[0027] In the process of preparing TS-1 molecular sieve catalyst, soft and hard dual templates are used to regulate the morphology and porous structure of the catalyst. The silicon / titanium hydrolysis rate is regulated by low-temperature-high-temperature step crystallization, the formation of anatase is inhibited, and the content of titanium in the catalyst skeleton is increased, which can effectively improve the catalyst activity. After calcination, the catalyst is modified with an organosilicon reagent to obtain an amphiphilic TS-1 catalyst. The use of this catalyst can realize the heterogeneous epoxidation of allyl chloride, effectively reduce the amount of solvent used, and reduce costs.
[0028] The TS-1 catalyst prepared by the method disclosed in the present invention has a high skeleton titanium content and abundant pores, and provides better catalyst activity in intermittent evaluations than the TS-1 catalyst prepared by the traditional process. The modified TS-1 catalyst has excellent amphiphilicity, and shows good activity and stability in the continuous evaluation of heterogeneous epoxidation of allyl chloride to prepare epichlorohydrin compared to before modification, and has broad application prospects in the "hydrogen peroxide method ECH". At the same time, according to the "heterogeneous epoxidation method of allyl chloride" provided by this patent, the circulation amount of solvent methanol can be greatly reduced, the energy consumption of solvent recovery can be reduced, and the economy of the process can be greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 are the UV characterization results of the catalysts prepared according to the comparative examples and the embodiments of the present invention;
[0030] Figure 2 TEM electron microscope characterization results of the catalysts prepared in comparative examples and in embodiments of the present invention;
[0031] Figure 3 is the contact angle test result of the catalyst prepared according to the embodiment of the present invention;
[0032] Figure 4 This is the result of continuous operation of heterogeneous epoxidation of allyl chloride using the catalyst prepared according to the embodiment of the present invention. DETAILED DESCRIPTION
[0033] "Scope" disclosed herein is defined in the form of lower limit and upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a particular range. The scope defined in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a particular parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0034] In this application, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution.
[0035] In this application, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0036] In the present application, unless otherwise specified, all steps mentioned herein may be performed sequentially or randomly, but are preferably performed sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0037] In this application, unless otherwise specified, the terms "include" and "comprising" mentioned herein may be open-ended or closed-ended. For example, the terms "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0038] In the description of this article, it should be noted that, unless otherwise specified, "above" and "below" are inclusive of the number itself, and "several" in "one or several" means two or more.
[0039] In the description herein, unless otherwise specified, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0040] Herein, unless otherwise specified, percentage (%) or part refers to percentage by weight or part by weight relative to the composition.
[0041] Herein, if there is no contrary description, the sum of the contents of the various components in the composition is 100%.
[0042] Herein, if there is no contrary description, the sum of the parts of each component in the composition may be 100 parts by weight.
[0043] In this document, unless otherwise specified, "a combination thereof" means a multi-component mixture of the elements described, for example a mixture of two, three, four and up to the maximum possible multi-component mixture.
[0044] If not specifically stated, the terms "a" or "an" used in the present specification means "at least one".
[0045] Herein, unless otherwise stated, all reactions are carried out at normal temperature and pressure.
[0046] In this document, unless otherwise specified, the terms "TS-1 catalyst" or "TS-1 molecular sieve catalyst" or "TS-1 titanium silicon molecular sieve catalyst" have the same meaning, all of which refer to molecular sieve catalysts used to catalyze the epoxidation reaction of allyl chloride, having a three-dimensional pore structure represented by ZSM-5, consisting of zigzag channels and elliptical straight channels intersecting therewith. The TS-1 catalyst forms a skeleton Si-O-Ti bond with special properties due to the uniform distribution of titanium atoms in the skeleton, which makes it have both catalytic oxidation activity and shape-selective catalytic performance.
[0047] Herein, unless otherwise specified, the term "alkyl" refers to a straight or branched chain saturated hydrocarbon group having one or more carbon atoms, including a C1-C20 alkyl group, preferably a C1-C6 alkyl group.
[0048] As used herein, unless otherwise indicated, the term "ammonium halide" refers to ammonium salts substituted with halogen atoms, such as fluorine, chlorine, bromine, or iodine.
[0049] One aspect of the present application provides a method for preparing a TS-1 molecular sieve catalyst, the method comprising the following steps:
[0050] (1) mixing a first template, an alkali source, a silicon source and water to obtain a first mixed solution, wherein the first template comprises at least one tetraalkylammonium hydroxide or tetraalkylammonium halide, the alkali source comprises ammonia or alkylamine, and the molar ratio of the first template, the alkali source, the silicon source and the water is 1:0-1:1-8:20-40;
[0051] (2) adding a second template to the first mixed solution to obtain a second mixed solution, wherein the second template comprises at least one polyethylene glycol monoalkyl ether, polyethylene glycol dialkyl ether, polyethylene glycol alkyl phenyl ether, polypropylene glycol monoalkyl ether, polypropylene glycol dialkyl ether or polypropylene glycol alkyl phenyl ether, wherein the amount of the second template is 5-20% by weight based on the weight of the silicon source;
[0052] (3) dissolving a titanium source in a polar aprotic solvent to obtain a third mixed solution, wherein the molar ratio of the titanium source to the silicon source is 0.02-0.06:1, and the weight ratio of the titanium source to the polar aprotic solvent is 1:1-10;
[0053] (4) mixing the second mixed solution and the third mixed solution and performing low-temperature and high-temperature fractional crystallization;
[0054] (5) Drying, molding, and calcining the reaction solution after crystallization to obtain a TS-1 molecular sieve catalyst.
[0055] In the present application, the "first template" can be a soft template commonly used for preparing molecular sieve catalysts, including but not limited to tetraalkylammonium hydroxide or tetraalkylammonium halide. The tetraalkylammonium hydroxide includes tetra-C1-C20 alkylammonium hydroxide, preferably tetra-C1-C6 alkylammonium hydroxide. In one example of the present application, the tetraalkylammonium hydroxide is selected from one or more of tetraethylammonium hydroxide, tetrapropylammonium hydroxide or tetrabutylammonium hydroxide. In one example of the present application, the tetraalkylammonium halide includes tetra-C1-C20 alkylammonium halide, preferably tetra-C1-C6 alkylammonium halide. In one example of the present application, the tetraalkylammonium halide is selected from one or more of tetraethylammonium bromide, tetrapropylammonium bromide, tetrabutylammonium bromide, tetraethylammonium chloride, tetrapropylammonium chloride, and tetrabutylammonium chloride. In one example of the present application, the soft template is tetrapropylammonium bromide.
[0056] In the present application, "alkali source" can be a nitrogen-containing organic base, including but not limited to ammonia or alkylamine. When the soft template is tetraalkylammonium hydroxide, no alkali source may be provided. In one example of the present application, the alkylamine includes C1-C20 alkylamine, preferably C1-C6 alkylamine. In one example of the present application, the alkylamine is ammonia or ethylamine.
[0057] In the present application, "silicon source" can be an organic silicon compound commonly used for preparing molecular sieve catalysts, including but not limited to alkyl orthosilicates, alkyl metasilicates or combinations thereof. The alkyl orthosilicates include C1-C20 alkyl orthosilicates. In one example of the present application, the alkyl orthosilicates are selected from one or more of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate or butyl orthosilicate. In one example of the present application, the alkyl metasilicates include C1-C20 alkyl silicates. In one example of the present application, the alkyl metasilicates are selected from one or more of methyl metasilicate, ethyl metasilicate, propyl metasilicate or butyl metasilicate. In one example of the present application, the silicon source is tetraethyl orthosilicate.
[0058] In the present application, the water may be deionized water, distilled water, ultrapure water, etc.
[0059] In step (1), in addition to the first template, alkali source, silicon source and water, the raw materials may also include auxiliary agents commonly used in the art, including but not limited to pH regulators, surfactants, protective agents or combinations thereof.
[0060] In one example of the present application, the molar ratio of the first template, alkali source, silicon source and water is controlled to be 1:0-1:1-8:10-80, preferably 1:0-1:2-4:20-50, and more preferably 1:0-1:2-4:25-40.
[0061] In the present application, "second template agent" includes but is not limited to polyethylene glycol monoalkyl ether, polyethylene glycol dialkyl ether or polyethylene glycol alkylphenyl ether, polypropylene glycol monoalkyl ether, polypropylene glycol dialkyl ether or polypropylene glycol alkylphenyl ether. In an example of the present application, the second template agent is selected from one or more of polyethylene glycol monomethyl ether, polyethylene glycol dimethyl ether, polyethylene glycol octylphenyl ether, polyethylene glycol monobutyl ether, polypropylene glycol monomethyl ether, polypropylene glycol dimethyl ether, polypropylene glycol octylphenyl ether or polypropylene glycol monobutyl ether. In an example of the present application, the second template agent includes polyethylene glycol octylphenyl ether.
[0062] In one example of the present application, the amount of the second template is 5-20% by weight, preferably 10-15% by weight, based on the weight of the silicon source.
[0063] In the present application, "titanium source" may be a titanium-containing compound commonly used for preparing molecular sieve catalysts, including but not limited to titanium tetrachloride, metatitanic acid, orthotitanic acid or tetraalkyl titanate. The tetraalkyl titanate includes tetra-C1-C20 alkyl titanate, preferably tetra-C1-C6 alkyl titanate. In one example of the present application, the titanium source includes one or more of titanium tetrachloride, metatitanic acid, orthotitanic acid, tetraethyl titanate, tetraisopropyl titanate or tetrabutyl titanate. In one example of the present application, the titanium source includes tetraisopropyl titanate.
[0064] In one example of the present application, the molar ratio of the titanium source to the silicon source is 0.01-0.1:1, preferably 0.02-0.06:1, and more preferably 0.04-0.05:1.
[0065] In the present application, "polar aprotic solvent" refers to a polar solvent that cannot give out protons in the reaction system, including but not limited to acetonitrile, DMF, DMI, DMSO, 1,4-dioxane, THF. In one example of the present application, the titanium source includes THF.
[0066] In one example of the present application, the amount of the polar aprotic solvent is 1-10 times, preferably 3-6 times, of the titanium source by weight.
[0067] In the present application, low temperature and high temperature step-by-step crystallization can be carried out in a hydrothermal reactor. In one example of the present application, the low temperature crystallization temperature is 60-100°C, preferably 70-90°C, the crystallization time is 5-60 hours, preferably 12-48 hours, and the low temperature crystallization temperature is 120-180°C, preferably 140-160°C, the crystallization time is 5-60 hours, preferably 12-48 hours.
[0068] In one example of the present application, the reaction solution after crystallization is dried, preferably spray-dried to obtain TS-1 crystallized powder.
[0069] In the present application, "molding" may be a conventional molding step for imparting a shape to the crystallized powder. In one example of the present invention, the molding step comprises extruding the dried TS-1 crystallized powder after mixing it with a sol and an organic binder. The sol includes, but is not limited to, titanium dioxide, zirconium oxide, aluminum oxide, silica sol, silica-alumina, silica-titania, etc. The sol preferably comprises silica sol. The amount of the sol is 50-100wt% of the TS-1 crystallized powder, preferably 60-80wt%. The organic binder includes, but is not limited to, (hydroxy) alkyl cellulose. In one example of the present invention, the organic binder comprises one or more of methyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl methyl cellulose, preferably hydroxypropyl methyl cellulose. The amount of the organic binder is 10-30wt% of the TS-1 crystallized powder, preferably 10-20wt%.
[0070] In this application, "calcination" can adopt conventional calcination temperatures in the art. In one example of this application, the calcination temperature is 400-700°C, preferably 500-600°C.
[0071] In the present application, the method further comprises modifying the TS-1 molecular sieve catalyst with organosilicon under the action of a modifying solvent. The modifying solvent includes but is not limited to methanol, ethanol, isopropanol, tetrahydrofuran, toluene and DMF. The mass ratio of the modified solvent to the TS-1 molecular sieve catalyst is 1-15:1, preferably 3-10:1. In one example of the present invention, the modifying solvent is tetrahydrofuran. The organosilicon includes but is not limited to polyethylene glycol bistriethoxysilane or polyethylene glycol triethoxysilane. The PEG molecular weight of the polyethylene glycol bistriethoxysilane includes but is not limited to about 200, 400, 1000 or 3000. The PEG molecular weight of the polyethylene glycol triethoxysilane includes but is not limited to about 200, 400, 1000 or 3000. The mass ratio of the organosilicon to the TS-1 molecular sieve catalyst is 0.01:1-5:1, preferably 0.02:1-2:1. In one example of the present invention, the silicone comprises polyethylene glycol bistriethoxysilane with a PEG molecular weight of about 1000.
[0072] In the present application, the modification can be carried out in a hydrothermal kettle by a hydrothermal method. The modification temperature is 60-150° C., preferably 120-130° C., and the modification time is 1-24 hours, preferably 6-12 hours.
[0073] The TS-1 molecular sieve catalyst prepared by the method described in this application is oil-water amphiphilic, has good catalytic activity, high epichlorohydrin selectivity, and long life. In the heterogeneous epoxidation experiment, the TS-1 molecular sieve catalyst can effectively reduce the unit consumption of solvent methanol and improve the process economy of "hydrogen peroxide method ECH".
[0074] Another aspect of the present application provides a method for preparing epichlorohydrin by epoxidizing allyl chloride, the method comprising reacting allyl chloride, hydrogen peroxide, a catalytic amount of solvent and the TS-1 molecular sieve catalyst.
[0075] In the present application, the hydrogen peroxide is hydrogen peroxide, and preferably an aqueous solution of hydrogen peroxide is used. In one example of the present application, the concentration of hydrogen peroxide is 5-90%, preferably 30-70wt%. The molar ratio of the hydrogen peroxide and allyl chloride is 1:1-1:10, preferably 1:1-1:4. The solvent includes but is not limited to alcohols, ketones, acids, esters, preferably methanol, ethanol, propanol, butanol, acetone and methyl ethyl ketone, etc., and methanol is most preferred. In the continuous heterogeneous epoxidation reaction of the TS-1 molecular sieve catalyst prepared by the method described in the present application, only a catalytic amount of solvent can be used to activate the molecular sieve. The amount of the solvent is 1-10% of the total mass of the hydrogen peroxide and allyl chloride. In one example of the present application, the reaction temperature is 10-60°C, preferably 15-40°C.
[0076] Unless otherwise specified, the various raw materials of the present application can be obtained from the market; or prepared according to conventional methods in the art. Unless otherwise defined or specified, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein can be applied to the methods disclosed herein. Other aspects of the present disclosure are obvious to those skilled in the art due to the disclosure herein.
[0077] Example
[0078] The present disclosure will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present disclosure and are not intended to limit the scope of the present disclosure. The experimental methods for which specific conditions are not specified in the following examples are usually measured in accordance with national standards. If there is no corresponding national standard, then it is carried out in accordance with general international standards, conventional conditions, or according to the conditions recommended by the manufacturer. Unless otherwise stated, all parts are parts by weight, all percentages are percentages by weight, and the polymer molecular weight is the number average molecular weight.
[0079] Raw material sources and preparation
[0080] Tetraethyl orthosilicate was purchased from Sinopharm Reagent;
[0081] Tetrapropylammonium bromide was purchased from Macklin's reagent;
[0082] Ammonia water, concentration 25-28%, purchased from Sinopharm Reagent;
[0083] Tetraisopropyl titanate was purchased from MacLean's reagent;
[0084] Tetrahydrofuran was purchased from Sinopharm Reagent;
[0085] Hydroxypropyl methylcellulose, purchased from MacLean's reagent;
[0086] Polyethylene glycol octylphenyl ether was purchased from MacLean's reagent;
[0087] Polyethylene glycol bistriethoxysilane, product brand PS2-L-2K, was purchased from Pengshuo Biotechnology.
[0088] Example 1
[0089] The TS-1 catalyst was prepared according to the following conventional preparation method:
[0090] (1) At room temperature, 420 g (~2 mol) of tetraethyl orthosilicate was weighed and placed in a 2 L three-necked flask equipped with a stirrer and a condenser, and 270 g (~1 mol) of tetrapropylammonium bromide, 70 g (~1 mol) of 25 wt% ammonia water and 500 g of water were added respectively under stirring to obtain a first mixed solution;
[0091] (2) At room temperature, weigh 26 g (~0.09 mol) of tetraisopropyl titanate and place it in a 500 mL three-necked flask equipped with a stirrer and a condenser, add 130 g of tetrahydrofuran, stir and mix until evenly mixed, then transfer to a 2 L three-necked flask and mix thoroughly with the first mixed solution;
[0092] (3) The mixed solution was transferred to a hydrothermal reactor, and crystallized at 80°C for 12 hours, then the temperature was raised to 140°C and crystallized for another 48 hours; after the crystallization was completed, the mixture was cooled to room temperature and spray-dried to obtain 170 g of TS-1 crystallized powder;
[0093] (4) Take 150 g of the above TS-1 crystallized powder, place it in a kneader, add 112 g of silica sol and 23 g of hydroxypropyl methylcellulose, knead for 10 minutes to obtain a kneaded material, place the kneaded material in a twin-screw extruder to extrude strips, dry at 50°C for 24 hours, crush, pass through a 10-20 mesh sieve, and calcine in a muffle furnace at 500°C for 8 hours to obtain a TS-1 catalyst, which is numbered YN-1.
[0094] Example 2
[0095] The TS-1 catalyst was prepared according to the following method, wherein no hard template was added and no modification was performed:
[0096] (1) At room temperature, 420 g (~2 mol) of tetraethyl orthosilicate was weighed and placed in a 2 L three-necked flask equipped with a stirrer and a condenser, and 270 g (~1 mol) of tetrapropylammonium bromide, 70 g (~1 mol) of 25 wt% ammonia water and 500 g of water were added respectively under stirring to obtain a first mixed solution;
[0097] (2) At room temperature, weigh 26 g (~0.09 mol) of tetraisopropyl titanate and place it in a 500 mL three-necked flask equipped with a stirrer and a condenser, add 130 g of tetrahydrofuran, stir and mix until evenly mixed, then transfer to a 2 L three-necked flask and mix thoroughly with the first mixed solution;
[0098] (3) The mixed solution was transferred to a hydrothermal reactor, and after crystallization at 80°C for 12 hours, the temperature was raised to 140°C and crystallization was continued for 48 hours; after the crystallization was completed, it was cooled to room temperature and spray-dried to obtain 170 g of TS-1 crystallized powder;
[0099] (4) Take 150 g of the above TS-1 crystallized powder, place it in a kneader, add 112 g of silica sol and 23 g of hydroxypropyl methylcellulose, knead for 10 minutes to obtain a kneaded material, place the kneaded material in a twin-screw extruder to extrude strips, dry at 50°C for 24 hours, crush, pass through a 10-20 mesh sieve, and calcine in a muffle furnace at 500°C for 8 hours to obtain a TS-1 catalyst, which is numbered YN-2.
[0100] Example 3
[0101] The TS-1 catalyst was prepared according to the following method, wherein low-high temperature staged crystallization was not used and no modification was performed:
[0102] (1) At room temperature, 420 g (~2 mol) of tetraethyl orthosilicate was weighed and placed in a 2 L three-necked flask equipped with a stirrer and a condenser, and 270 g (~1 mol) of tetrapropylammonium bromide, 70 g (~1 mol) of 25 wt% ammonia water and 500 g of water were added respectively under stirring to obtain a first mixed solution;
[0103] (2) After mixing evenly, add 51 g of polyethylene glycol octylphenyl ether to the three-necked flask and stir until completely dissolved; at room temperature, weigh 26 g (~0.09 mol) of tetraisopropyl titanate, place it in a 500 mL three-necked flask with a stirrer and a condenser, add 130 g of tetrahydrofuran, stir and mix evenly, then transfer to a 2 L three-necked flask and mix thoroughly with the first mixed solution;
[0104] (3) The mixed solution was transferred to a hydrothermal reactor and crystallized at 140°C for 60 hours. After the crystallization was completed, the mixture was cooled to room temperature and spray-dried to obtain 170 g of TS-1 crystallized powder.
[0105] (4) Take 150 g of the above TS-1 crystallized powder, place it in a kneader, add 112 g of silica sol and 23 g of hydroxypropyl methylcellulose, knead for 10 min to obtain a kneaded material, place the kneaded material in a twin-screw extruder to extrude strips, dry at 50°C for 24 h, crush, pass through a 10-20 mesh sieve, and calcine in a muffle furnace at 500°C for 8 h to obtain a TS-1 catalyst, which is numbered YN-3.
[0106] Example 4
[0107] The TS-1 catalyst was prepared according to the following method, in which a hard template was added and low-high temperature staged crystallization was adopted without modification:
[0108] (1) At room temperature, 420 g (~2 mol) of tetraethyl orthosilicate was weighed and placed in a 2 L three-necked flask equipped with a stirrer and a condenser, and 270 g (~1 mol) of tetrapropylammonium bromide, 70 g (~1 mol) of 25 wt% ammonia water and 500 g of water were added respectively under stirring to obtain a first mixed solution;
[0109] (2) After mixing evenly, add 51 g of polyethylene glycol octylphenyl ether to the three-necked flask and stir until completely dissolved; at room temperature, weigh 26 g (~0.09 mol) of tetraisopropyl titanate, place it in a 500 mL three-necked flask with a stirrer and a condenser, add 130 g of tetrahydrofuran, stir and mix evenly, then transfer to a 2 L three-necked flask and mix thoroughly with the first mixed solution;
[0110] (3) The mixed solution was transferred to a hydrothermal reactor, and crystallized at 80°C for 12 hours, then the temperature was raised to 140°C and crystallized for another 48 hours; after the crystallization was completed, the mixture was cooled to room temperature and spray-dried to obtain 170 g of TS-1 crystallized powder;
[0111] (4) Take 150 g of the TS-1 crystallized powder, place it in a kneader, add 112 g of silica sol and 23 g of hydroxypropyl methylcellulose, knead for 10 min to obtain a kneaded material, place the kneaded material in a twin-screw extruder to extrude strips, dry at 50° C. for 24 h, crush, pass through a 10-20 mesh sieve, and calcine in a muffle furnace at 500° C. for 8 h to obtain a TS-1 catalyst, which is numbered YN-4.
[0112] Example 5
[0113] The TS-1 catalyst was prepared by the following method, wherein a hard template was added, low-high temperature segmented crystallization was adopted, and polyethylene glycol bistriethoxysilane (PEG-1000) was used for modification:
[0114] (1) At room temperature, 420 g (~2 mol) of tetraethyl orthosilicate was weighed and placed in a 2 L three-necked flask equipped with a stirrer and a condenser, and 270 g (~1 mol) of tetrapropylammonium bromide, 70 g (~1 mol) of 25 wt% ammonia water and 500 g of water were added respectively while stirring to obtain a first mixed solution;
[0115] (2) After mixing evenly, add 51 g of polyethylene glycol octylphenyl ether to the three-necked flask and stir until completely dissolved; at room temperature, weigh 26 g (~0.09 mol) of tetraisopropyl titanate, place it in a 500 mL three-necked flask with a stirrer and a condenser, add 130 g of tetrahydrofuran, stir and mix evenly, then transfer to a 2 L three-necked flask and mix thoroughly with the first mixed solution;
[0116] (3) The mixed solution was transferred to a hydrothermal reactor, and after crystallization at 80°C for 12 hours, the temperature was raised to 140°C and crystallization was continued for 48 hours; after the crystallization was completed, it was cooled to room temperature and spray-dried to obtain 170 g of TS-1 crystallized powder;
[0117] (4) 150 g of the above TS-1 crystallized powder was placed in a kneader, 112 g of silica sol and 23 g of hydroxypropyl methylcellulose were added, and the mixture was kneaded for 10 min to obtain a kneaded material, which was placed in a twin-screw extruder to extrude strips, dried at 50° C. for 24 h, crushed, passed through a 10-20 mesh sieve, and calcined in a muffle furnace at 500° C. for 8 h to obtain a TS-1 catalyst;
[0118] (5) Take 60g of the above TS-1 catalyst, place it in a hydrothermal reaction kettle, add 300g of tetrahydrofuran and 3g of polyethylene glycol bistriethoxysilane, place the hydrothermal kettle in a rotary oven, and modify it at 130°C for 6h; after the modification, cool it to room temperature, filter it, and wash the catalyst three times with tetrahydrofuran, using 150g of tetrahydrofuran each time; place the wet-based catalyst in a vacuum drying oven, dry it at -95kPa and 100°C for 12h, and obtain an amphiphilic TS-1 catalyst, numbered YN-5.
[0119] Testing and characterization of TS-1 catalyst
[0120] The UV characterization was performed using an ultraviolet spectrophotometer MPS-2000 purchased from Shimadzu Corporation of Japan; the TEM electron microscopy characterization was performed using a transmission electron microscope Tecnai 12 purchased from PHILIPS (Philips) of the Netherlands; and the contact angle test was performed using a dynamic contact angle meter JC2000D1 purchased from Shanghai Zhongchen Digital Technology Equipment Co., Ltd.
[0121] The three catalysts YN-1, YN-4 and YN-5 were characterized by UV and TEM, and the contact angle test was performed on YN-4 and YN-5. Figure 1 As shown, the peak at 210nm is the peak of skeleton titanium with catalytic activity, the peak at 280nm is the peak of tetracoordinate titanium, which has certain catalytic activity, and the peak at 330nm is the peak of titanium dioxide with no catalytic activity. The UV characterization results show that the YN-1 catalyst prepared by the traditional method has strong absorption peaks at 280nm and 330nm, indicating that the titanium in the YN-1 catalyst exists mainly in the form of tetracoordinate and titanium dioxide, and the skeleton titanium in the YN-4 and YN-5 catalysts is significantly increased. Therefore, the catalytic activity of YN-1 is lower than that of YN-4 and YN-5. According to the UV characterization results, the use of dual templates and low-high temperature segmented crystallization effectively increases the skeleton titanium content and improves the catalyst activity.
[0122] TEM characterization results are shown in Figure 2As shown, the left picture is YN-1, the middle picture is YN-4, and the right picture is YN-5. Figure 2 As shown in the figure, YN-1 has a spherical structure with almost no pores, while YN-4 and YN-5 catalysts have a sheet structure with rich pores. TEM characterization results show that the pore structure of YN-4 / 5 is richer than that of YN-1. The rich pores can reduce the adhesion of epoxidation products on the catalyst surface, and have higher catalytic activity and stability.
[0123] The contact angle test results are as follows: Figure 3 As shown, the left figure is the test result of YN-4, and the right figure is the test result of YN-5. The contact angle test results show that the contact angle of YN-4 catalyst is 100°, which has strong hydrophobicity; after the YN-5 catalyst is modified with polyethylene glycol, the contact angle is reduced to ~70°, which has good amphiphilicity and can increase the diffusion of reactants to the catalyst. Therefore, the YN-5 catalyst has better catalytic activity and stability in heterogeneous epoxidation.
[0124] Example 6
[0125] The five catalysts prepared above were used for intermittent evaluation of epoxidation of allyl chloride, and the effects of the catalysts were judged by comparing the hydrogen peroxide conversion rate, ECH selectivity and yield data. YN-1 / 2 / 3 / 4 / 5 catalysts were taken respectively, ground and crushed, and 1 g was weighed and placed in a 500 mL four-necked bottle with a thermometer, stirring and condensing. Allyl chloride (AC) 114.8 g (1.5 mol) and methanol 6.8 g (catalytic amount) were weighed and placed in a four-necked bottle, stirred in a 20°C water bath, and after the system temperature stabilized at 20°C, 113.3 g (1 mol) of 30% hydrogen peroxide was added, and the reaction was continued by stirring for 1 hour. Every 10 minutes, instantaneous samples were taken to measure the HP content and GC quantitative measurement.
[0126] In this embodiment, the five groups of evaluation conditions remain consistent, and the specific HP conversion rate and ECH selectivity data are shown in Table 1 below.
[0127] HP conversion rate / % = (1-m 收料 *c 收料-HP / m 进料 *c 进料-HP )*100;
[0128] ECH selectivity / % = (m 收料 *c 收料-ECH / 92.5) / (m 进料 *c 进料-AC / 72.5-m 收料 *c 收料-AC / 72.5)*100;
[0129] Where m 收料 is the receiving mass, m进料 is the feed mass, c 收料-HP is the HP content in the received material, c 进料-HP is the HP content in the feed, c 进料-AC is the AC content in the feed, c 收料-AC is the AC content in the collected material, c 收料-ECH It is the ECH content in the received material.
[0130] Table 1: Allyl chloride epoxidation reaction data
[0131]
[0132] From the data in Table 1, we can see that the TS-1 catalysts numbered YN-2 and YN-4 prepared by low-high temperature step-by-step crystallization have better effects in the intermittent evaluation experiment than YN-1 prepared by the traditional method and YN-3 prepared by one-step crystallization; the catalyst YN-4 without organosilicon modification can also achieve the ideal reaction effect in the intermittent evaluation by extending the reaction time; compared with the catalyst YN-4 without organosilicon modification, the amphiphilic catalyst YN-5 modified by organosilicon has better effect on heterogeneous epoxidation. The following two catalysts YN-4 and YN-5 are used in heterogeneous continuous epoxidation reaction to evaluate the effect of YN-4 / 5 catalyst.
[0133] Example 7
[0134] Take 30g of YN-4 and YN-5 catalysts respectively and load them into fixed beds. The inner diameter of the fixed bed is 11mm. The length of the YN-4 catalyst bed is 788mm, and the length-to-diameter ratio is 71.6; the length of the YN-5 catalyst bed is 802mm, and the length-to-diameter ratio is 72.9. The bed temperature is 20°C, and the reaction is carried out under normal pressure. Allyl chloride and hydrogen peroxide-methanol are fed in two streams, allyl chloride ~19.1g / h, 30wt% hydrogen peroxide-methanol ~20g / h, where methanol accounts for 5.5% of the mass of the water-alcohol solution. Long-term experiments are carried out to evaluate the activity, selectivity and life of the two catalysts. The specific data of the heterogeneous continuous operation results of YN-4 and YN-5 are shown in Figure 4 .
[0135] Depend on Figure 4 The data show that in continuous operation, the catalyst YN-4 without modification by the organosilicon reagent can provide a higher hydrogen peroxide conversion rate, which begins to decline after running for about 600 hours; after modification by the organosilicon reagent, the catalyst activity and reaction effect for the heterogeneous epoxidation reaction are further improved due to the introduction of amphiphilic polyethylene glycol groups in the catalyst. The hydrogen peroxide conversion rate of the YN-5 catalyst is greater than 99%, and it begins to decline slowly after running for about 1600 hours, and the conversion rate is maintained above 98% to 1800 hours. The ECH selectivity can be maintained above 99%, showing good catalytic activity and stability.
[0136] The above description is only a preferred embodiment of the present disclosure and is not intended to limit the scope of the substantial technical content of the present disclosure. The substantial technical content of the present disclosure is broadly defined in the scope of the claims of the application. Any technical entity or method completed by others, if it is exactly the same as that defined in the scope of the claims of the application or an equivalent variation, will be deemed to be included in the scope of the claims.
[0137] All documents mentioned in this disclosure are cited as references in this application, just as each document is cited as reference individually. In addition, it should be understood that after reading the above content of this disclosure, those skilled in the art may make various changes or modifications to this disclosure, and these equivalent forms also fall within the scope defined by the claims attached to this application.
Claims
1. A method for preparing a TS-1 molecular sieve catalyst, the method The following steps are involved: (1) mixing a first template, an alkali source, a silicon source and water to obtain a first mixed solution, wherein the first template comprises at least one tetraalkylammonium hydroxide or tetraalkylammonium halide, the alkali source comprises ammonia or alkylamine, and the molar ratio of the first template, the alkali source, the silicon source and the water is 1:0-1:1-8:20-40; (2) adding a second template to the first mixed solution to obtain a second mixed solution, wherein the second template comprises at least one of polyethylene glycol monoalkyl ether, polyethylene glycol dialkyl ether, polyethylene glycol alkyl phenyl ether, polypropylene glycol monoalkyl ether, polypropylene glycol dialkyl ether or polypropylene glycol alkyl phenyl ether, wherein the amount of the second template is 5-20%, based on the weight of the silicon source; (3) dissolving a titanium source in a polar aprotic solvent to obtain a third mixed solution, wherein the molar ratio of the titanium source to the silicon source is 0.02-0.06:1, and the weight ratio of the titanium source to the polar aprotic solvent is 1:1-10; (4) mixing the second mixed solution and the third mixed solution and performing low-temperature and high-temperature fractional crystallization; (5) Drying, molding, and calcining the reaction solution after crystallization to obtain a TS-1 molecular sieve catalyst.
2. The method according to claim 1, It is characterized in that The silicon source comprises at least one alkyl orthosilicate, alkyl metasilicate, and / or The titanium source comprises at least one of titanium tetrachloride, metatitanic acid, orthotitanic acid or tetraalkyl titanate; and / or The polar aprotic solvent includes DMF, DMSO, 1,4-dioxane, THF or a combination thereof, preferably THF.
3. The method according to claim 1 or 2, It is characterized in that The low-temperature and high-temperature stepwise crystallization includes crystallization at 60-100° C., preferably 70-90° C., for 12-48 hours, and crystallization at 120-180° C., preferably 140-160° C., for 12-48 hours.
4. The method according to claim 1 or 2, It is characterized in that The molding step comprises mixing the dried TS-1 crystallized powder with a sol and an organic binder and then extruding the mixture into a mold.
5. The method according to claim 1 or 2, It is characterized in that The method further comprises (6) modifying the TS-1 molecular sieve catalyst with organosilicon under the action of a modifying solvent, wherein the weight ratio of the organosilicon to the TS-1 molecular sieve catalyst is 0.02:1-2:
1.
6. The method according to claim 5, It is characterized in that The modified solvent comprises at least one of the following solvents: methanol, ethanol, isopropanol, tetrahydrofuran, toluene and DMF, preferably tetrahydrofuran; and / or The organosilicon comprises polyethylene glycol bistriethoxysilane or polyethylene glycol triethoxysilane; and / or The modification is carried out by a hydrothermal method, the modification temperature is 60-150° C., and the modification time is 1-24 hours.
7. The TS-1 molecular sieve catalyst prepared according to the method of any one of claims 1 to 6.
8. A method for preparing epichlorohydrin by epoxidizing allyl chloride, the method comprising reacting allyl chloride, hydrogen peroxide, a catalytic amount of a solvent and the TS-1 molecular sieve catalyst according to claim 7.
9. The method of claim 8, wherein the molar ratio of hydrogen peroxide to allyl chloride is 1:1-1:4; and / or The amount of the solvent is 1-10% of the total mass of the hydrogen peroxide and allyl chloride; and / or The reaction temperature is 15-40°C.
10. The epichlorohydrin product prepared according to the method of claim 8 or 9.
Citation Information
Cited By
TS-1 molecular sieve catalyst, preparation method and application of TS-1 molecular sieve catalyst in preparation of epoxy compound through epoxidation of hydrogen peroxide and olefin
CN121755267A