Combined inhibitor for flotation separation of low-alkalinity zinc-sulfur sulfide ore and application of combined inhibitor

By using a combination inhibitor of lime and o-dinitrophene in zinc-sulfur sulfide ore flotation, the problems of separation difficulties and environmental pollution in the high alkali process are solved, and sphalerite and pyrite under low alkali conditions are realized The efficient separation reduces lime usage and improves recovery.

CN119016186AActive Publication Date: 2024-11-26KUNMING UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411256081.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-26
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The existing high-alkali process leads to severe mudification, impurity entrainment, equipment corrosion, environmental pollution and rare precious metal recovery in the flotation of zinc-sulfur sulfide ore. Moreover, the lime consumption is large and the cost is high, making it difficult to effectively separate sphingoite and pyrite. .

Method used

The combination of lime and o-phenanthrene inhibitors are used, with a mass ratio of (5-20):3, which is used for flotation of zinc-sulfur sulfide ore under low alkali conditions, inhibit pyrite through complexation reaction, reduce lime usage and Improve the capture effect of sphalerite.

Benefits of technology

The selective separation between sphalerite and pyrite is achieved under low alkali conditions, reducing the lime usage by 60-80%, solving the problems caused by the high alkali process, improving the concentrate quality and recovery rate, and reducing the Environmental pollution and pharmaceutical costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016186A_ABST
    Figure CN119016186A_ABST
Patent Text Reader

Abstract

The invention discloses a combined inhibitor for flotation separation of low-alkalinity zinc-sulfur sulfide ore and application of the combined inhibitor, the combined inhibitor comprises lime (CaO) and phenanthroline (phen), the mass ratio of the lime (CaO) to the phenanthroline (phen) is (5-20): 3, the combined inhibitor is used for inhibiting pyrite, the combined inhibitor is applied to low-alkalinity flotation separation of the zinc-sulfur sulfide ore, and the combined inhibitor can be used for flotation separation of the low-alkalinity zinc-sulfur sulfide ore or flotation separation of the low-alkalinity zinc-sulfur sulfide ore or flotation separation of the low-alkalinity zinc-sulfur sulfide ore or flotation separation of the low-alkalinity zinc-sulfur sulfide ore. The process is good in separation effect and high in concentrate grade, and has important significance on efficient recycling of the zinc-sulfur sulfide ore. In addition, the phenanthroline in the combined inhibitor can reduce the use amount of lime, the harm caused by high-alkali sulfur inhibition to beneficiation is solved, meanwhile, the phenanthroline is used, copper sulfate does not need to be additionally added to serve as a sphalerite activating agent, and the beneficiation cost is reduced. The combined inhibitor is small in dosage, stable in effect and high in inhibition capacity, and has a good process application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a combined inhibitor for flotation separation of low-basicity zinc-sulfur sulfide ores and application thereof, belonging to the technical field of ore dressing. Background Art

[0002] As a non-ferrous strategic metal, zinc plays an important role in the national economic construction and is widely used in steel, metallurgy, machinery, electrical, chemical, light industry, military and medicine. Sphalerite is one of the main sources of zinc. However, pyrite often coexists with sphalerite, and flotation is usually used to separate the two.

[0003] Lime is often used as a pyrite inhibitor in zinc-sulfur separation because of its low cost and good inhibitory effect. Although the high-alkali process has good effects, it also brings a series of problems: (1) When the mineral contains a large amount of mud, the use of a large amount of lime leads to severe mudification during the flotation process, sticky flotation foam, a large amount of impurities, and poor concentrate quality, which makes the production process difficult to stabilize. (2) The use of a large amount of lime causes the slurry to agglomerate easily, resulting in blockage of the transportation pipeline, corrosion of equipment, increased maintenance costs, and unnecessary economic losses. (3) The high-alkali environment affects the recovery of associated rare and precious metals such as Au, Ag, Ge, and In. In addition, pyrite inhibited by high alkali is difficult to activate. (4) The addition of a large amount of lime causes the ore dressing wastewater to contain a large amount of calcium ions and a high pH value, causing environmental pollution and high water treatment costs. Therefore, the research on efficient pyrite inhibitors and sphalerite collectors has become one of the current hot issues.

[0004] In recent years, pyrite inhibitors have been widely studied, which are divided into inorganic inhibitors and organic inhibitors. Inorganic inhibitors are mainly cyanide, lime, sulfur oxides and some oxidants, but most of these inorganic inhibitors have problems such as large dosage, toxicity, and serious environmental pollution. Organic inhibitors mainly include dextrin, modified starch, humic acid, tannic acid, lignin, etc. Organic inhibitors are used in small amounts and have good effects, but they are costly and difficult to control in production.

[0005] Under the above conditions, the separation of sphalerite and pyrite mostly requires the use of copper sulfate as an activator for sphalerite, which also increases the beneficiation cost. Therefore, it is very necessary to find a green pyrite depressant with good selectivity that can achieve the separation of sphalerite and pyrite without using copper sulfate as an activator. Summary of the invention

[0006] In view of the shortcomings of the prior art, one of the purposes of the present invention is to provide a new type of combined inhibitor with small dosage, green and environmental protection, and strong adaptability to solve the above problems. The combined inhibitor is used to inhibit pyrite in the flotation separation of zinc-sulfur sulfide ores under low-alkali conditions, and has little effect on the flotation of sphalerite. Compared with "high alkali sulfur inhibition", this method reduces the amount of lime by about 60-80%, solving a series of problems of "high alkali sulfur inhibition". In addition, the inhibitor of the present invention is environmentally friendly, small in dosage, and highly applicable.

[0007] The combined depressant of the present invention is lime and o-phenanthroline, and the mass ratio of the combination of the two is (5-20):3. The combined depressant is a pyrite depressant used for the flotation separation of sphalerite and pyrite.

[0008] One of the combined inhibitors of the present invention is o-phenanthroline, and its structural formula is as follows:

[0009]

[0010] The second object of the present invention is to provide an application of the inhibitor in the flotation separation of zinc-sulfur sulfide ore under low-alkali conditions, and the specific steps are as follows:

[0011] (1) After slurrying the ore to be selected, a combined inhibitor, butyl xanthate and No. 2 oil are sequentially added to perform zinc roughing to obtain zinc roughing concentrate and roughing tailings;

[0012] (2) the roughing tailings obtained in step (1) are subjected to two scavenging processes, a collector and No. 2 oil are added before each scavenging process, and the scavenged concentrates are returned to the previous stage in sequence to form a closed loop, and the final zinc tailings are obtained after two scavenging processes;

[0013] (3) The zinc rougher concentrate obtained in step (1) is subjected to two concentrations, and a combined inhibitor is added each time. The tailings of each concentration are returned to the previous stage to form a closed loop, and the final zinc concentrate is obtained after two concentrations.

[0014] In step (1), the raw ore is slurried to a slurry concentration of 30-35%, the combined inhibitor is used in an amount of 800-2300 g / t, the butyl xanthate is used in an amount of 60-100 g / t, and the No. 2 oil is used in an amount of 10-20 g / t.

[0015] The dosage of reagents in the two scavenging operations in step (2) is as follows: in scavenging one, the dosage of butyl xanthate is 30-50 g / t, and the dosage of No. 2 oil is 8-15 g / t; in scavenging two, the dosage of butyl xanthate is 15-25 g / t, and the dosage of No. 2 oil is 5-10 g / t.

[0016] The dosage of the reagents in the two concentration operations in step (3) are as follows: in the first concentration, the dosage of the combined inhibitor is 400-1000 g / t; in the second concentration, the dosage of the combined inhibitor is 200-500 g / t.

[0017] In combination with the above technical solutions, the advantages, principles and beneficial effects of the present invention are as follows:

[0018] The present invention is aimed at the flotation separation process of zinc-sulfur sulfide ore, and a combined depressant and flotation scheme are developed, which can realize the selective recovery of sphalerite and the selective inhibition of pyrite under low alkalinity. When the combined depressant is used in the separation of zinc-sulfur sulfide ore, the index is stable. The combined depressant reduces the amount of lime by 60-80%, solves a series of problems caused by "high alkali sulfur inhibition", and realizes the effective separation of zinc-sulfur sulfide ore under low alkali conditions.

[0019] The combined inhibitor of the present invention includes lime and o-phenanthroline, and mainly utilizes the coordination of lime and o-phenanthroline to efficiently and selectively inhibit pyrite. O-phenanthroline is a bidentate heterocyclic compound ligand with two nitrogen-containing functional groups, which has a strong chelating effect with metal ions. 2+ Forming a stable [Fe(phen) 3 ] 2+ Under weak alkaline conditions, o-phenanthroline reacts with the surface of pyrite to form [Fe(phen) 3 ] 2+ It is adsorbed on the surface of pyrite, hindering the interaction between butyl xanthate and the surface of pyrite to achieve the purpose of inhibiting pyrite. However, the complexing ability of o-phenanthroline with zinc is much weaker than that with iron, which also makes o-phenanthroline adsorbed less on the surface of sphalerite, and the adsorption of a small amount of o-phenanthroline also enhances the adsorption of butyl xanthate on the surface of sphalerite, thereby strengthening the capture effect of butyl xanthate on sphalerite and reducing the use of copper sulfate.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The inhibitor for flotation separation of zinc-sulfur sulfide ores under low alkali conditions provided by the present invention can achieve green and efficient separation of sphalerite and pyrite at a pH between 7.5 and 10, thereby solving a series of problems such as environmental pollution and foam stickiness caused by the traditional "high alkali sulfur inhibition".

[0022] (2) The inhibitor used in the present invention can chelate with the dissolved metal ions, effectively reducing the cost of treating mineral processing wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to the described contents.

[0025] Embodiment 1: The inhibitor used in the present invention is a combined inhibitor, which is a combination of lime and 1,2-phenanthroline, and the mass ratio of the combination of the two is 5:3.

[0026] Application of the combined inhibitor in flotation separation of low-alkalinity zinc-sulfur sulfide ores: The Zn grade in the lead tailings of a lead-zinc sulfide mine in Yunnan is 1.37%, and the S grade is 1.98%, and Zn is mainly sphalerite, and S is mainly pyrite. The tailings are used as the minerals to be selected, and a one-rough, two-sweep, and two-fine flotation process is used for separation. The process is as follows: Figure 1 shown.

[0027] (1) Roughing operation: add water to the above-mentioned mineral to be selected to adjust the pulp mass concentration to 30%, add 800g / t of combined inhibitor (including 500g / t of lime and 300g / t of o-phenanthroline) for 3 minutes, then measure the pulp pH to be 7.5, then add 60g / t of butyl xanthate for 3 minutes, finally add 10g / t of No. 2 oil for 2 minutes, and flotation for 4 minutes to obtain zinc roughing concentrate and roughing tailings;

[0028] (2) Scavenging operation: add 30g / t butyl xanthate to the roughing tailings for 3 minutes, and finally add 8g / t No. 2 oil for 2 minutes. After flotation for 3.5 minutes, the first scavenging concentrate and the first scavenging tailings are obtained; the first scavenging concentrate is returned to the roughing operation, and the first scavenging tailings are added with 15g / t butyl xanthate for 3 minutes, and then 5g / t No. 2 oil is added for 2 minutes. After flotation for 3 minutes, the second scavenging concentrate and the final zinc tailings are obtained, and the second scavenging concentrate is returned to the first scavenging operation in sequence;

[0029] (3) Concentration operation: Add 400g / t (i.e. 250g / t lime and 150g / t o-phenanthroline) of inhibitor to the rougher concentrate for 3 minutes, and flotate for 3 minutes to obtain the first concentrated concentrate and the first concentrated tailings. Return the first concentrated tailings to the rougher, add 200g / t (i.e. 125g / t lime and 75g / t o-phenanthroline) of inhibitor to the first concentrated concentrate for 3 minutes, and flotate for 2.5 minutes to obtain the second concentrated tailings and the final zinc concentrate, and then return the second concentrated tailings to the first concentrated operation in sequence.

[0030] The flotation reagent system of the above flotation separation method is shown in Table 1, and the experimental results are shown in Table 2.

[0031] Comparative Example 1

[0032] Comparative Example 1 adopts the above flotation process, except that lime is used as the depressant in an unchanged dosage. The reagent system is shown in Table 1, and the experimental results are shown in Table 2.

[0033] Comparative Example 2

[0034] Comparative Example 2 still uses the above flotation process, the difference is that the inhibitor is all lime and the dosage is changed. The reagent system is shown in Table 1, and the experimental results are shown in Table 2.

[0035] Table 1. Dosage system of Example 1, Comparative Example 1 and Comparative Example 2, unit (g / t)

[0036]

[0037]

[0038] Table 2. Flotation test results of Example 1, Comparative Example 1 and Comparative Example 2

[0039]

[0040] From the above experimental results, it can be seen that under low alkalinity conditions, that is, compared with Example 1 and Comparative Example 1, it is difficult to inhibit pyrite without adding 1, resulting in unsatisfactory concentrate indicators. Compared with the high alkalinity of Example 1 and Comparative Example 2, which only add lime, the flotation results of the two are similar, and both can well inhibit pyrite to achieve flotation separation of zinc-sulfur sulfide ores. However, compared with Comparative Example 2, which only adds lime, Example 1, which adds 1, reduces the amount of lime by 84%. Reducing the amount of lime can also obtain better flotation indicators, which shows that the inhibitor is effective for flotation separation of zinc-sulfur sulfide ores.

[0041] Example 2

[0042] A method for flotation separation of low-alkalinity zinc-sulfur sulfide ore, wherein the inhibitors are lime and 1,2-phenanthroline, and the mass ratio of the combination of the two is 10:3.

[0043] In a lead-zinc sulfide ore in Inner Mongolia, the Pb grade is 1.89%, the Zn grade is 1.83%, and the S grade is 2.17%. After lead priority flotation, the lead tailings are obtained. The Zn grade of the lead tailings is 1.67%, and the S grade is 2.04%. The mine uses this tailings as the ore to be selected and adopts a flotation process of one roughing, two sweeping and two fine separation for separation. The process is as follows Figure 1 shown.

[0044] (1) Roughing operation: water was added to the above-mentioned minerals to make the mass concentration of the ore pulp 33%, and 1300g / t (including 1000g / t of lime and 300g / t of o-phenanthroline) of inhibitor was added for 3 minutes. At this time, the pH value of the ore pulp was measured to be 8.8. Then 80g / t of butyl xanthate was added for 3 minutes, and finally 15g / t of No. 2 oil was added for 2 minutes. After flotation for 4 minutes, zinc roughing concentrate and roughing tailings were obtained.

[0045] (2) Scavenging operation: Add 40g / t butyl xanthate to the roughing tailings for 3 minutes, and finally add 10g / t No. 2 oil for 2 minutes. After flotation for 3.5 minutes, the first scavenging concentrate and the first scavenging tailings are obtained. The first scavenging concentrate is returned to the roughing operation, and the first scavenging tailings are added with 20g / t butyl xanthate for 3 minutes, and then 8g / t No. 2 oil is added for 2 minutes. After flotation for 3 minutes, the second scavenging concentrate and the final zinc tailings are obtained, and the second scavenging concentrate is returned to the first scavenging operation in sequence.

[0046] (3) Concentration operation: Add 800g / t (i.e. 615g / t lime and 185g / t o-phenanthroline) as an inhibitor to the rougher concentrate for 3 minutes, and flotate for 3 minutes to obtain the first concentrated concentrate and the first concentrated tailings. Return the first concentrated tailings to the rougher concentrate, add 300g / t (i.e. 230g / t lime and 70g / t o-phenanthroline) as an inhibitor to the first concentrated concentrate for 3 minutes, and flotate for 2.5 minutes to obtain the second concentrated tailings and the final zinc concentrate, and then return the second concentrated tailings to the first concentrated operation in sequence.

[0047] The flotation reagent system of the above flotation separation method is shown in Table 3, and the experimental results are shown in Table 4.

[0048] Comparative Example 3

[0049] Comparative Example 3 adopts the above flotation process, except that lime is used as the depressant in an unchanged dosage. The reagent system is shown in Table 3, and the experimental results are shown in Table 4.

[0050] Comparative Example 4

[0051] Comparative Example 4 still uses the above flotation process, except that lime is used as the inhibitor and the dosage is changed. The reagent system is shown in Table 3, and the experimental results are shown in Table 4.

[0052] Table 3. Dosage system of Example 2, Comparative Example 3 and Comparative Example 4, unit (g / t)

[0053]

[0054] Table 4. Flotation test results of Example 2, Comparative Example 3 and Comparative Example 4

[0055]

[0056] From the above results, it can be seen that the addition of o-phenanthroline under low-alkali conditions is conducive to the inhibition of sulfur, ensuring the quality of the concentrate while also improving the recovery rate. The flotation results of using o-phenanthroline as a depressant for pyrite under low-alkali conditions are slightly better than those under high-alkali conditions. The addition of o-phenanthroline not only reduces the amount of lime used, but also solves a series of problems in production caused by high alkali, which is beneficial to the improvement of the economic benefits of production.

[0057] Example 3

[0058] A method for flotation separation of low-alkalinity zinc-sulfur sulfide ore, wherein the inhibitors are lime and 1,2-phenanthroline, and the mass ratio of the combination of the two is 20:3.

[0059] A copper-lead-zinc polymetallic sulfide ore in Yunnan was subjected to copper-lead mixed flotation and zinc-sulfur mixed flotation to obtain a zinc-sulfur mixed concentrate with a Zn grade of 2.85% and a S grade of 6.21%. Figure 1 The flotation process shown is used to separate zinc and sulfur. The specific steps are as follows:

[0060] (1) Roughing operation: water was added to the above-mentioned minerals to be selected to adjust the slurry mass concentration to 35%, and 2300 g / t (including 2000 g / t of lime and 300 g / t of o-phenanthroline) of inhibitor was added for 3 minutes. At this time, the pH value of the slurry was measured to be 10. Then 100 g / t of butyl xanthate was added for 3 minutes, and finally 20 g / t of No. 2 oil was added for 2 minutes. After flotation for 4 minutes, zinc roughing concentrate and roughing tailings were obtained.

[0061] (2) Scavenging operation: Add 50g / t of butyl xanthate to the roughing tailings for 3 minutes, and finally add 15g / t of No. 2 oil for 2 minutes. After flotation for 3.5 minutes, the first scavenging concentrate and the first scavenging tailings are obtained. The first scavenging concentrate is returned to the roughing operation, and the first scavenging tailings are added with 25g / t of butyl xanthate for 3 minutes, and then 10g / t of No. 2 oil is added for 2 minutes. After flotation for 3 minutes, the second scavenging concentrate and the final zinc tailings are obtained, and the second scavenging concentrate is returned to the first scavenging operation in sequence.

[0062] (3) Concentration operation: 1000g / t (i.e. 870g / t lime and 130g / t o-phenanthroline) of inhibitor was added to the rougher concentrate for 3 minutes, and flotation was performed for 3 minutes to obtain the first concentration concentrate and the first concentration tailings. The first concentration tailings were returned to the rougher, and 500g / t (i.e. 385g / t lime and 115g / t o-phenanthroline) of inhibitor was added to the first concentration concentrate for 3 minutes, and flotation was performed for 2.5 minutes to obtain the second concentration tailings and the final zinc concentrate, and then the second concentration tailings were returned to the first concentration operation in sequence.

[0063] The above flotation test reagent system is shown in Table 5, and the flotation results are shown in Table 6

[0064] Comparative Example 5

[0065] Comparative Example 5 adopts the above flotation process, except that lime is used as the depressant in an unchanged dosage. The reagent system is shown in Table 5, and the experimental results are shown in Table 6.

[0066] Comparative Example 6

[0067] Comparative Example 6 still uses the above flotation process, except that lime is used as the inhibitor and the dosage is changed. The reagent system is shown in Table 5, and the experimental results are shown in Table 6.

[0068] Table 5. Dosage system of Example 3, Comparative Example 5 and Comparative Example 6, unit (g / t)

[0069]

[0070] Table 6. Flotation test results of Example 3, Comparative Example 5 and Comparative Example 6

[0071]

[0072]

[0073] From the above results, it can be seen that the addition of o-phenanthroline under low-alkali conditions is conducive to the inhibition of sulfur, ensuring the quality of the concentrate while also improving the recovery rate. The flotation results of using o-phenanthroline as a depressant for pyrite under low-alkali conditions are slightly better than those under high-alkali conditions, which also shows that the use of o-phenanthroline can not only reduce the amount of lime used, but also improve the recovery rate while ensuring the quality of the concentrate, thereby improving the efficiency of production.

[0074] The above results show that o-phenanthroline is beneficial to the flotation separation of zinc-sulfur sulfide ores, which is mainly manifested in the following aspects: (1) o-phenanthroline is used at low alkalinity, which reduces the amount of lime used; (2) o-phenanthroline does not need to add copper sulfate to activate sphalerite when separating zinc-sulfur sulfide ores, which reduces the cost of reagents; (3) The use of o-phenanthroline solves the problems of severe muddling of ore pulp and sticky foam caused by the use of a large amount of lime; the above aspects are beneficial to the separation of zinc-sulfur sulfide ores. The combined inhibitor of the present invention has stable properties, good selective inhibition effect, small dosage, safe use, strong adaptability, and broad application prospects.

[0075] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are within the scope of the technical solution of the present invention.

Claims

1. A combined depressant for flotation separation of low-basicity zinc-sulfide ore, characterized in that: The combined inhibitor is a combination of lime and 1,2-phenanthroline, and the mass ratio of the combination of the two is (5-20):

3.

2. The use of the combined depressant according to claim 1 in the flotation separation of low-basicity zinc-sulfur sulfide ores, characterized in that: The combined depressant is used to depress pyrite, and the specific flotation separation steps are as follows: (1) After slurrying the ore to be selected, a combined inhibitor, butyl xanthate and No. 2 oil are sequentially added to perform zinc roughing to obtain zinc roughing concentrate and roughing tailings; (2) the roughing tailings obtained in step (1) are subjected to two scavenging processes, a collector and No. 2 oil are added before each scavenging process, and the scavenged concentrates are returned to the previous stage in sequence to form a closed loop, and the final zinc tailings are obtained after two scavenging processes; (3) The zinc rougher concentrate obtained in step (1) is subjected to two concentrations, and a combined inhibitor is added each time. The tailings of each concentration are returned to the previous stage to form a closed loop, and the final zinc concentrate is obtained after two concentrations.

3. The use of the combined depressant according to claim 2 in the flotation separation of low-basicity zinc-sulfur sulfide ores, characterized in that: In step (1), the mineral to be selected is slurried to a slurry concentration of 30-35%, the amount of combined inhibitor is 800-2300 g / t, the amount of butyl xanthate is 60-100 g / t, and the amount of No. 2 oil is 10-20 g / t.

4. The use of the combined depressant according to claim 2 in the flotation separation of low-basicity zinc-sulfur sulfide ores, characterized in that: The dosage of reagents in the two scavenging operations in step (2) is as follows: in scavenging one, the dosage of butyl xanthate is 30-50 g / t, and the dosage of No. 2 oil is 8-15 g / t; in scavenging two, the dosage of butyl xanthate is 15-25 g / t, and the dosage of No. 2 oil is 5-10 g / t.

5. The use of the combined depressant according to claim 2 in the flotation separation of low-basicity zinc-sulfur sulfide ores, characterized in that: The dosage of the reagents in the two concentration operations in step (3) are as follows: in the first concentration, the dosage of the combined inhibitor is 400-1000 g / t; in the second concentration, the dosage of the combined inhibitor is 200-500 g / t.

Citation Information

Patent Citations

  • Flotation composite inhibitor for inhibiting pyrite under low alkalinity and using method thereof

    CN106540816A

  • Method for producing nanomagnetite

    CN109689577A

  • Inhibitor for zinc-sulfur sulfide ore flotation separation under low alkalinity and application of inhibitor

    CN118341575A

  • Method for producing nanomagnetite

    US20190300381A1