Forging process of low-pressure turbine disc for aviation

By optimizing the forging temperature, speed, and die design of the low-pressure turbine disk for aerospace applications, the problems of low processing quality and efficiency of aerospace die forgings have been solved, achieving high-quality and low-cost forging results.

CN119016675APending Publication Date: 2024-11-26SOUTHWEST PETROLEUM UNIV

Patent Information

Application Number
CN202411305409.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The processing quality and efficiency of aerospace die forgings are difficult to guarantee, resulting in serious problems such as low efficiency, high cost, and high scrap rate.

Method used

By rationally selecting forging temperature, speed, and die design, and combining experimental design and numerical simulation analysis, the forging process of low-pressure turbine disks for aerospace is optimized. This includes steps such as segmented heating, upsetting, pre-forging, and final forging. The die is designed using 5CrNiMo material, which has good toughness and high strength.

Benefits of technology

It improved the machining quality of low-pressure turbine disks, reduced scrap rate, decreased costs, and increased forging efficiency and success rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016675A_ABST
    Figure CN119016675A_ABST
Patent Text Reader

Abstract

The invention provides an aviation low-pressure turbine disc forging process which comprises the following steps: cutting a GH4169 bar into # imgabs0 # * 430 mm, removing oxide skin, keeping the charging temperature of the bar at 600 DEG C, sequentially heating to 800 DEG C, 950 DEG C and 1050 DEG C in sections, keeping the bar upsetting speed at 2-5 mm / s, the upsetting forging ratio at 2.5-3, the upsetting frequency at 2, the pressing speed at 5-8 mm / s, the under-pressure amount at 5-10 mm and the maximum pressure less than or equal to 200 MN, and carrying out heat treatment on the bar to obtain the aviation low-pressure turbine disc. And water cooling is adopted after forging, and the heat treatment temperature of the forge piece is 960-1000 DEG C. High machining quality of the low-pressure turbine disc for aviation can be guaranteed, the rejection rate is reduced, the cost is reduced, the forging efficiency and the success rate are improved, and great production practice significance is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a forging process for a low-pressure turbine disc for aviation, belonging to the technical field of metal forging. Technical Background

[0002] The main load-bearing parts of aircraft and aero-engine structures are all die forgings, such as the aircraft body load-bearing frame, main beam, landing gear, engine turbine disc, turbine shaft, blades, etc. Their manufacturing level has a significant impact on the highest performance level, reliability, life and technical and economic benefits that the aircraft can achieve. Aviation forgings are the most technically demanding, most stringent quality requirements and most expensive forgings in the forging industry. At present, the processing quality and efficiency of aviation die forgings are difficult to guarantee, resulting in serious problems of low efficiency, high cost and high scrap rate.

[0003] In response to the above problems, this paper proposes a forging process for low-pressure turbine disks for aviation by reasonably selecting parameters such as forging temperature, forging speed and die design, combining experimental design and numerical simulation analysis methods. It can ensure high processing quality of low-pressure turbine disks, reduce scrap rate, reduce costs, and improve forging efficiency and success rate. Summary of the invention

[0004] In order to overcome the defects and limitations of the above-mentioned related technologies, the purpose of the present invention is to provide a forging process for low-pressure turbine discs for aviation. The method and process involved in the present invention can reduce costs and improve forging efficiency and quality.

[0005] To this end, the present invention provides a forging process for a low-pressure turbine disk for aviation, comprising the following steps:

[0006] Step 1, Cutting: Cut the GH4169 bar into And remove the oxide scale;

[0007] Step 2, heating: low temperature furnace (600℃), heating in stages (heating to 800℃, 950℃,

[0008] 1050℃);

[0009] Step 3, upsetting: the upsetting speed is maintained at 2-5 mm / s, the upsetting forging ratio is 2.5-3, and the upsetting times are 2;

[0010] Step 4, pre-forging\final forging: pressing speed 5-8mm / s, underpressure 5-10mm, maximum pressure ≤200MN;

[0011] Step 5: Cooling, heat treatment, surface treatment: water cooling, heat treatment temperature 960-1000℃;

[0012] Step 6: Inspect and remove the parts.

[0013] In step 1 described above, the rod material is GH4169 with good processing performance, and the diameter range of the rod material is The length ranges from 425mm to 435mm and the oxide scale is removed mechanically or chemically.

[0014] As described in step 2 above, a three-stage heating method is adopted. The charging furnace temperature is maintained at 600°C. After the bar is preheated to a center temperature exceeding 600°C, the material enters the plastic range, the furnace temperature is quickly heated to 800°C and kept warm for a period of time, and then the furnace temperature is quickly heated to 950°C and kept warm for a period of time, and finally the furnace temperature is quickly heated to the final forging temperature of 1050°C.

[0015] The inspection described in step 6 above includes die structure inspection, forging appearance, size, mechanical properties, surface flaw detection and ultrasonic inspection.

[0016] As described above, a forging process for a low-pressure turbine disc for aviation is characterized in that the mold is made of 5CrNiMo material with good toughness, high strength and high wear resistance, and the mold is optimized according to the stress concentration area, large deformation area, weak area and other areas of the forging that have a greater impact on the processing quality.

[0017] The forging process for a low-pressure turbine disk for aviation as described above is characterized in that the stress-strain curves of 5CrNiMo at different temperatures and different strain rates are obtained through hot compression experiments.

[0018] The forging process for a low-pressure turbine disc for aviation as described above is characterized in that the stress-strain curves of GH4169 at different strain rates at 1100°C are obtained through hot compression experiments.

[0019] The forging process for a low-pressure turbine disc for aviation as described above is characterized in that the parameters such as forging temperature, forging speed and die design are reasonably selected by combining experimental design and numerical simulation analysis methods.

[0020] It can be seen from the technical solution provided by the present invention that, compared with the prior art, the present invention provides a forging process for low-pressure turbine discs for aviation, which can ensure a higher processing quality of the low-pressure turbine discs, reduce the scrap rate, reduce costs, and improve forging efficiency and success rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A flow chart of a forging process for a low-pressure turbine disc for aviation provided by the present invention;

[0022] Figure 2 The three-dimensional diagram of the upper mold;

[0023] Figure 3The following is a three-dimensional diagram of the mold;

[0024] Figure 4 It is the stress-strain curve of 5CrNiMo at different strain rates at 490℃;

[0025] Figure 5 It is the stress-strain curve of 5CrNiMo at different strain rates at 570℃;

[0026] Figure 6 It is the stress-strain curve of GH4169 at different strain rates at 1100℃;

[0027] Figure 7 The forming diagram of forging-die with different underpressure;

[0028] Figure 8 The stress cloud diagram of 5CrNiMo at different strain rates at 570℃;

[0029] Fig. 9 The stress-strain data of forgings at different strain rates Specific implementation plan

[0030] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described with reference to the accompanying drawings.

[0031] As shown in the accompanying drawings, the present invention provides a forging process for a low-pressure turbine disk for aviation, comprising the following steps:

[0032] Step 1, Cutting: Cut the GH4169 bar into And remove the oxide scale;

[0033] Step 2, heating: low temperature furnace (600℃), heating in stages (heating to 800℃, 950℃,

[0034] 1050℃);

[0035] Step 3, upsetting: the upsetting speed is maintained at 2-5 mm / s, the upsetting forging ratio is 2.5-3, and the upsetting times are 2;

[0036] Step 4, pre-forging\final forging: pressing speed 5-8mm / s, underpressure 5-10mm, maximum pressure ≤200MN;

[0037] Step 5: Cooling, heat treatment, surface treatment: water cooling, heat treatment temperature 960-1000℃;

[0038] Step 6: Inspect and remove the parts.

[0039] In step 1, in specific implementation, the rod material is GH4169 with good processing performance, and the diameter range of the rod material is The length ranges from 425mm to 435mm and the oxide scale is removed mechanically or chemically.

[0040] In step 2, a three-stage heating method is used in the specific implementation. The charging temperature is maintained at 600°C. After the bar is preheated to a center temperature exceeding 600°C, the material enters the plastic range, the furnace temperature is quickly heated to 800°C and kept warm for a period of time, and then the furnace temperature is quickly heated to 950°C and kept warm for a period of time, and finally the furnace temperature is quickly heated to the final forging temperature of 1050°C.

[0041] In step 6, in specific implementation, the inspection includes die structure inspection, forging appearance, size, mechanical properties, surface flaw detection and ultrasonic inspection.

[0042] The forging process for a low-pressure turbine disc for aviation is characterized in that the mold used is made of 5CrNiMo material with good toughness, high strength and high wear resistance, and the mold is optimized according to the stress concentration area, large deformation area, weak area and other areas of the forging that have a greater impact on the processing quality.

[0043] The forging process for a low-pressure turbine disk for aviation is characterized in that the stress-strain curves of 5CrNiMo at different temperatures and different strain rates are obtained through hot compression experiments.

[0044] The forging process for a low-pressure turbine disc for aviation is characterized in that the stress-strain curves of GH4169 at different strain rates at 1100°C are obtained through hot compression experiments.

[0045] The forging process for a low-pressure turbine disc for aviation is characterized by combining experimental design and numerical simulation analysis methods to reasonably select parameters such as forging temperature, forging speed and die design.

[0046] The specific embodiments of the present invention described herein are only used to explain the purpose of the present invention and cannot be understood as limiting the present invention in any way. Under the guidance of the present invention, technicians can conceive of any possible changes based on the present invention, which should all be considered to belong to the scope of the present invention.

[0047] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more related listed items.

Claims

1. A forging process for a low-pressure turbine disk for aviation, characterized in that: The following steps are involved: Step 1, Cutting: Cut the GH4169 bar into And remove the oxide scale; Step 2, heating: low temperature furnace (600°C), heating in stages (heating to 800°C, 950°C, 1050°C successively); Step 3, upsetting: the upsetting speed is maintained at 2-5 mm / s, the upsetting forging ratio is 2.5-3, and the upsetting times are 2; Step 4, pre-forging\final forging: pressing speed 5-8mm / s, underpressure 5-10mm, maximum pressure ≤200MN; Step 5: Cooling, heat treatment, surface treatment: water cooling, heat treatment temperature 960-1000℃; Step 6: Inspect and remove the parts.

2. The forging process of a low-pressure turbine disk for aviation according to claim 1, characterized in that: The rod material is GH4169 with good processing performance, and the diameter range of the rod material is The length ranges from 425mm to 435mm and the oxide scale is removed mechanically or chemically.

3. The forging process of a low-pressure turbine disk for aviation according to claim 1, characterized in that: A three-stage heating method is adopted, the charging furnace temperature is maintained at 600℃, after the bar is preheated to the center temperature exceeding 600℃, the material enters the plastic range, the furnace temperature is quickly heated to 800℃ and kept warm for a period of time, then the furnace temperature is quickly heated to 950℃ and kept warm for a period of time, and finally the furnace temperature is quickly heated to the final forging temperature of 1050℃.

4. The method according to claim 1, characterized in that: The mold is made of 5CrNiMo material with good toughness, high strength and high wear resistance. The mold is optimized according to the stress concentration area, large deformation area, weak area and other areas of the forging that have a greater impact on the processing quality.

5. The forging process of a low-pressure turbine disk for aviation according to claim 1, characterized in that: The stress-strain curves of 5CrNiMo at different temperatures and strain rates were obtained through hot compression experiments.

6. The forging process for a low-pressure turbine disk for aviation according to claim 1, characterized in that: The stress-strain curves of GH4169 at different strain rates at 1100℃ were obtained through hot compression experiments.

7. The forging process for a low-pressure turbine disk for aviation according to claim 1, characterized in that: Combining the methods of experimental design and numerical simulation analysis, reasonable selection of parameters such as forging temperature, forging speed and die design is made.

8. The forging process for a low-pressure turbine disk for aviation according to claim 1, characterized in that: The inspection includes die structure inspection, forging appearance, size, mechanical properties, surface flaw detection and ultrasonic inspection.

Citation Information

Patent Citations

  • Forging method for improving microscopic structure of iron-based superalloy blade

    CN107377836A

  • Hot die forging process for nickel-based wrought superalloy double-performance turbine disks

    CN108515132A

  • Forging forming method for TA15 titanium alloy forge piece with high strength and high tenacity

    CN109226622A

  • Forging method of GH4169 series high temperature alloy turbine disc for aero-engine

    CN109622865A

  • Manufacturing method of large-size variable cross-section GH4169 alloy power turbine rear axle forging

    CN114160730A

Cited By

  • GH738 alloy large-wall-thickness forge piece uniform-grain forging method

    CN119681162A