Manufacturing process suitable for high-pressure casting of ceramic salt core coating
By applying a mixed liquid coating of specific powder raw materials and industrial ethanol on the salt core, and drying and sintering treatment, the problem of insufficient compressive resistance of the salt core is solved, and high-pressure casting and efficient production of complex cavity is achieved.
Patent Information
- Application Number
- CN202411022657.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-26
AI Technical Summary
The existing salt cores have insufficient compressive resistance in high-pressure casting and complex cavity casting production, which cannot meet the needs of high-performance aluminum alloy castings.
Using a process, by mixing powder raw materials such as quartz powder, alumina powder, iron oxide, quicklime, magnesium oxide, potassium oxide and sodium oxide, and uniformly proportioning with industrial ethanol, a liquid coating is formed and applied to the salt core. The surface is dried and sintered at high temperature to form a ceramic salt core coating with high compressive strength.
The compressive strength of the salt core is improved to reach more than 100MPa, which is suitable for high-pressure casting. In the cleaning of the internal cavity of the casting, the salt core can be cleaned without damage and keep the passage clean.
Smart Images

Figure CN119016679A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of salt core coating production, and in particular to a production process for high pressure casting ceramic salt core coating. Background Art
[0002] At present, due to the characteristics of ordinary salt cores, they can only be used for gravity casting and low-pressure casting of lightweight aluminum alloy products, and cannot be used for pressure casting and high-pressure casting. With the continuous upgrading and changes in the market environment, the performance requirements for aluminum alloy castings are getting higher and higher. Conventional gravity casting and low-pressure casting cannot meet the production requirements of structural functional parts, and pressure casting and high-pressure casting cannot cast complex castings with internal cavities at one time due to the characteristics of their own processes. Summary of the invention
[0003] In order to make up for the deficiencies of the prior art, the present invention provides a manufacturing process for a high-pressure casting ceramic salt core coating, through which the compressive strength of the salt core of the coating can reach above 100 MPa.
[0004] The present invention is achieved through the following technical solutions: A process for producing a high pressure casting ceramic salt core coating comprises the following steps: (1) Weigh and mix the powder raw materials. The weight ratio of the powder raw materials is: quartz powder 70-80%, aluminum oxide powder 10-15%, iron oxide 0-1.5%, quicklime 2-5%, magnesium oxide 0-1%, potassium oxide 3-8%, sodium oxide 0-5%; (2) Place the mixed powder into a heat preservation furnace and dry it at 180-220°C for 90-150 minutes; (3) Adding industrial ethanol to the dried powder, with the mass ratio of powder to industrial ethanol being 35-50:50-65, and mixing evenly to obtain a liquid coating; (4) After cleaning the surface of the salt core to be coated, immerse it in the liquid coating, take it out after 3-10 seconds, and hang it on a rack to let it stand for 5-10 minutes; (5) Send the coated salt core after standing to a drying furnace and dry it at 180-220°C; (6) The dried salt core is tested for surface coating, and the intact salt core is placed on a sintering tray for high-temperature sintering to obtain a salt core product with a complete coating.
[0005] The present invention is a manufacturing process for coating a protective film on the surface of an ordinary salt core. The compressive strength of the coated salt core can reach above 100MPa, which can meet the process requirements of high-pressure casting. The casting core is easy to clean, and the salt core in the inner cavity of the casting can be cleaned by flushing with pressurized water.
[0006] A better technical solution of the present invention is: In step (1), the weight ratio of the powder raw materials is: quartz powder 75%, aluminum oxide powder 12%, iron oxide 1%, quicklime 3%, magnesium oxide 0.5%, potassium oxide 5%, and sodium oxide 3.5%.
[0007] In step (2), the powder is placed in a heat preservation furnace and dried at 200°C for 120 minutes.
[0008] In step (3), the mass ratio of powder to industrial ethanol is 40-45:56-60, and the powder is mixed according to the above ratio to achieve the coating concentration required by the product; after the coating is mixed, the Baume concentration value of the liquid coating is detected, and the Baume concentration value at 20°C is controlled in the range of 22-26.
[0009] In step (4), the salt cores to be coated are evenly hung on a rack, and particles and dust on the surface of the salt cores are cleaned with an electric rotating soft brush and compressed air to ensure that the surface of the salt cores is free of dust and raised granular matter; the salt cores are immersed in the liquid coating for 5 seconds, then taken out, hung on a rack and left to stand for 5 minutes, and then the industrial ethanol on the salt core products is ignited and burned off. After the open flame disappears, the salt cores are transferred to the next process.
[0010] In step (5), the salt core is dried at 200° C. for 60 min.
[0011] In step (6), the dried salt core is dried to room temperature and then the coating surface is inspected; the undamaged salt core is placed in a sintering tray for high-temperature sintering, and the high-temperature sintering process is as follows: the temperature is raised from room temperature to 300°C within 60 minutes and kept warm for 30 minutes; the temperature is raised from 300°C to 450°C within 60 minutes and kept warm for 60 minutes; the temperature is raised from 450°C to 550°C within 60 minutes and kept warm for 60 minutes; the temperature is raised from 550°C to 650°C within 60 minutes and kept warm for 60 minutes; the temperature is raised from 650°C to 750°C within 60 minutes and kept warm for 120 minutes; then the temperature is lowered to room temperature with the furnace to complete the firing operation of the product coating.
[0012] A further preferred technical solution is to take out the salt core product after sintering, inspect the surface coating of the salt core, and the salt core product without cracks is a qualified product.
[0013] The size deviation of the salt core produced by the present invention complies with the provisions of JB / T11208-2011 "Technical Standards for Internal Cooling Oil Channel Salt Cores for Aluminum Pistons of Internal Combustion Engines". The standard size tolerance of the salt core less than ф80mm is ±0.4; the coating thickness of the salt core is about 0.05mm, and the diameter size increases by 0.1mm before and after coating; the size change is within the tolerance range and has no effect on the size of the salt core. The size parameters of the salt core are shown in the attached Figure 1 shown.
[0014] Salt core technical standard parameters The present invention has the following beneficial technical effects: (1) The salt core coating process proposed in the present invention can be applied to the high-pressure casting process of non-ferrous metals, and is applicable to lightweight non-ferrous metal castings by high-pressure casting, such as engine pistons by high-pressure casting. The surface of the produced salt core is smooth, and the strength and quality can be guaranteed. When used in casting, it is not easy to affect the non-ferrous metal castings; (2) The ceramic salt core produced by the salt core coating process proposed in the present invention is used in non-ferrous metal castings, which can realize the convenient cleaning of the internal cavity of the non-ferrous metal castings. The cleaning process can be realized by simply flushing with water. After flushing, the cavity is smooth and free of inclusions, keeping the channel clean and unobstructed; (3) The salt core produced by the salt core coating process proposed in the present invention can withstand a pressure shock of 100 MPa and is suitable for pressure casting and high-pressure casting. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The present invention will be further described below in conjunction with the accompanying drawings.
[0016] Figure 1 A schematic diagram of the industry standard salt core technical standard parameters; Figure 2 This is a schematic diagram of the change in outer diameter of the salt core after coating in Example 1; Figure 3 This is a schematic diagram of the change in inner diameter of the salt core after coating in Example 1; Figure 4 This is a schematic diagram of the height size change of the salt core after coating in Example 1; Figure 5 Schematic diagram of the sintering temperature curve after salt core coating.
[0017] Figure 1 In the figure, D1 is the outer diameter of the salt core, D2 is the inner diameter of the salt core, H is the total height of the salt core, and r o is the outer arc of the small end of the salt core, r i R is the inner arc of the small end of the salt core, o is the outer arc of the large end of the salt core, R i is the inner arc of the large end of the salt core, d is the diameter of the fixed hole, α is the external slope of the salt core, and β is the internal slope of the salt core; DETAILED DESCRIPTION
[0018] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] Embodiment 1: A process for manufacturing a high pressure casting ceramic salt core coating, specifically comprising the following steps: (1) Mix the raw materials in proportion and weigh the materials as required. During the weighing process, be careful not to spill the materials; Powder material ratio: quartz powder 7.5kg, alumina powder 1.2kg, iron oxide 0.1kg, quicklime 0.3kg, magnesium oxide 0.05kg, potassium oxide 0.5kg, sodium oxide 0.35kg; (2) The weighed powder material is placed in a box-type electric furnace for drying. The drying process is set to 200°C for 120 minutes to remove moisture from the raw materials and obtain 9.985 kg of powder material; (3) Liquid coating preparation: Evenly mix the dried powder material according to the following preparation requirements: 9.985 kg of powder material and 14.98 kg of industrial ethanol; After the paint is mixed, the Baume concentration value of the paint is tested, and the Baume concentration at 20°C is 24.3; After the salt core coating is prepared, in order to prevent the precipitation of powder materials, the prepared coating needs to be continuously stirred by electric stirring; (4) Cleaning the salt core: Clean the surface of the salt core to be coated: The salt cores are evenly hung on the racks, and the particles and dust on the surface of the salt cores are cleaned with an electric rotating soft brush and compressed air, and the dust particles on the surface of the salt cores are blown away; (5) Salt core coating: Evenly immerse the cleaned salt core into the coating, take it out after soaking for 5 seconds, hang it on the rack and let it stand for 5 minutes, then ignite and burn off the industrial ethanol remaining in the salt core product; after the open flame disappears, transfer the salt core to the next process for treatment; (6) Baking: slowly push the coated salt core into a 200°C through-type drying furnace for drying, with a total drying time of 60 minutes; (7) Sintering: After the salt core is dried and cooled to room temperature, check whether the coating surface is damaged. If there is no damage, put the salt core into the sintering tray for high-temperature sintering. The high-temperature sintering process curve is as follows: The temperature was raised from room temperature to 300°C in 60 minutes and kept at this temperature for 30 minutes; Increase the temperature from 300 to 450°C in 60 minutes, and keep warm for 60 minutes; Increase the temperature from 450°C to 550°C in 60 minutes and keep it for 60 minutes; The temperature was increased from 550°C to 650°C in 60 minutes and kept at this temperature for 60 minutes; The temperature was raised from 650°C to 750°C in 60 minutes and kept at this temperature for 120 minutes.
[0020] As the furnace cools down to room temperature, the firing of the product coating is completed; After sintering, take out the product, place it in a well-lit place, and visually check whether there are cracks on the surface coating of the salt core. Products without cracks are qualified products.
[0021] During the above process, 10 salt cores were randomly selected and numbered 1-10 to compare the performance changes of the salt cores before and after coating.
[0022] (1) Comparison of salt core specifications and dimensions before and after coating The above data combined with the attached Figure 2-4 It can be seen that the dimensions of the uncoated salt core and the coated salt core are within the standard tolerance range, so the coating has no effect on the terminal use of the salt core size.
[0023] (2) Comparison of compressive strength performance test of salt core before and after coating Tensile strength calculation formula: P(Mpa)=F(N) / S(mm 2 ); Uncoated ordinary salt core tensile strength: P(Mpa)=F(N) / S(mm 2 )=63 / 33.57=1.87Mpa; Coating salt core tensile strength: P(Mpa)=F(N) / S(mm 2 )=1228.7 / 33.57=36.6Mpa; After a large amount of data testing and deduction, the compressive strength of the salt core is 3 times that of the compressive strength.
[0024] It can be inferred from this that: The compressive strength of uncoated ordinary salt core = 1.87 × 3 = 5.61Mpa; The compressive strength of the coating salt core = 36.6 × 3 = 109.8Mpa; The compressive strength of the coated salt core can meet the requirements of high-pressure casting. After coating, the overall size is uniform and consistent, within the tolerance range of the product, and does not affect the product performance.
[0025] Embodiment 2: The manufacturing process of the ceramic salt core coating for high pressure casting is applicable, and the specific steps are as in Example 1, except that: (1) Powder material ratio: quartz powder 7.22kg, alumina powder 1.0kg, iron oxide 0.13kg, quicklime 0.3kg, magnesium oxide 0.8kg, potassium oxide 0.3kg, sodium oxide 0.25kg; (2) The weighed powder material was placed in a box-type electric furnace for drying. The drying process was set to 180°C for 120 min to remove moisture from the raw materials and obtain 9.993 kg of powder material; (3) Liquid coating preparation: Evenly mix the dried powder material according to the following preparation requirements: 9.993 kg of powder material and 18.558 kg of industrial ethanol; After the paint is mixed, the Baume concentration value of the paint is tested. The Baume concentration value at 20°C is 22.1; (5) Salt core coating: Evenly immerse the cleaned salt core into the coating, take it out after soaking for 8 seconds, and hang it on the rack to let it stand for 8 minutes; (6) Baking: Slowly push the coated salt core into a 180°C through-type drying furnace for drying. The overall drying time is 80 minutes.
[0026] Embodiment 3: The manufacturing process of the ceramic salt core coating for high pressure casting is applicable, and the specific steps are as in Example 1, except that: (1) Powder material ratio: quartz powder 7.95kg, alumina powder 1.15kg, iron oxide 0.08kg, quicklime 0.2kg, magnesium oxide 0.02kg, potassium oxide 0.45kg, sodium oxide 0.15kg; (2) The weighed powder material was placed in a box-type electric furnace for drying. The drying process was set to 220°C for 90 minutes to remove moisture from the raw materials and obtain 9.983 kg of powder material; (3) Liquid coating preparation: Evenly mix the dried powder material according to the following preparation requirements: 9.983 kg of powder material and 9.983 kg of industrial ethanol; After the paint is mixed, the Baume concentration value of the paint is tested, and the Baume concentration at 20°C is 25.9; (5) Salt core coating: Evenly immerse the cleaned salt core into the coating, soak for 10 seconds, take it out, and hang it on the rack to let it stand for 10 minutes; (6) Baking: Slowly push the coated salt core into a 220°C through-type drying furnace for drying. The overall drying time is 50 minutes.
[0027] Comparative Example 1: Comparative Verification of Casting Conventional Alcohol-Based Coatings for Salt Cores The specific steps of this comparative example are the same as those of Example 1, except that: (1) Take out 20 kg of conventional alcohol-based paint (commercially available) and stir it evenly. Then test the Baume concentration of the paint. The Baume concentration at 20°C is 24.5. Prepare it for use. (2) Salt core coating: Evenly immerse the cleaned salt core into the coating, soak for 5 seconds, take it out, and hang it on the rack to let it stand for 5 minutes; (3) Baking: slowly push the coated salt core into a 200°C through-type drying furnace for drying, and the overall drying time is 60 minutes; (4) Sintering: After the dried salt core is dried to room temperature, the coating surface is checked for damage. The salt core without damage is placed in a sintering tray for high-temperature sintering. The sintering process curve is consistent with that of Example 1.
[0028] Comparative Example 2: Comparative Verification of Using Conventional Water-Based Coatings for Casting Salt Cores The specific steps of this comparative example are the same as those of Example 1, except that: (1) Take out 20 kg of conventional water-based paint (commercially purchased) and stir it evenly. Then test the Baume concentration of the paint. The Baume concentration at 20°C is 22.5. Prepare it for use. (2) Salt core coating: Evenly immerse the cleaned salt core into the coating, soak for 2 seconds, take it out, and hang it on the rack to let it stand for 5 minutes; (3) Baking: slowly push the coated salt core into a 200°C through-type drying furnace for drying, and the overall drying time is 120 minutes; (4) Sintering: After the dried salt core is dried to room temperature, the coating surface is checked for damage. The salt core without damage is placed in a sintering tray for high-temperature sintering. The sintering process curve is consistent with that of Example 1.
[0029] Take 10 groups of common salt cores of different strengths, 5 salt cores in each group, and prepare salt core coatings under the conditions of Examples 1-3 and Comparative Examples 1-2, respectively. The tensile strength of the coated salt cores is tested and compared. The specific results are as follows: It can be seen from the above comparison results that the salt core coating process of the present invention can effectively enhance the tensile strength and strength of the salt core, can withstand 100MPa pressure shock, and is suitable for pressure casting and high-pressure casting. It is significantly different from the alcohol-based / water-based coatings commonly used on the market. The coating coating of the present application is a special coating designed for the salt core. After a unique manufacturing process, the performance improvement effect is significant.
[0030] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A process for producing a high pressure casting ceramic salt core coating, characterized in that: The method comprises the following steps: (1) weighing and mixing powder raw materials, wherein the weight ratio of the powder raw materials is: quartz powder 70-80%, aluminum oxide powder 10-15%, iron oxide 0-1.5%, quicklime 2-5%, magnesium oxide 0-1%, potassium oxide 3-8%, and sodium oxide 0-5%; (2) Place the mixed powder into a heat preservation furnace and dry it at 180-220°C for 90-150 minutes; (3) Adding industrial ethanol to the dried powder, with the mass ratio of powder to industrial ethanol being 35-50:50-65, and mixing evenly to obtain a liquid coating; (4) After cleaning the surface of the salt core to be coated, immerse it in the liquid coating, take it out after 3-10 seconds, and hang it on a rack to let it stand for 5-10 minutes; (5) Send the coated salt core after standing to a drying furnace and dry it at 180-220°C; (6) The dried salt core is tested for surface coating, and the intact salt core is placed in a sintering tray for high-temperature sintering to obtain a salt core product with a complete coating.
2. The process for producing a high pressure casting ceramic salt core coating according to claim 1, characterized in that: In step (1), the weight ratio of the powder raw materials is: quartz powder 75%, aluminum oxide powder 12%, iron oxide 1%, quicklime 3%, magnesium oxide 0.5%, potassium oxide 5%, and sodium oxide 3.5%.
3. The process for producing a high pressure casting ceramic salt core coating according to claim 1, characterized in that: In step (2), the powder is placed in a heat preservation furnace and dried at 200°C for 120 minutes.
4. The process for producing a high pressure casting ceramic salt core coating according to claim 1, characterized in that: In step (3), the mass ratio of powder to industrial ethanol is 40-45:56-60, and the Baume degree of the liquid coating at 20°C is 22-26.
5. The process for producing a ceramic salt core coating for high pressure casting according to claim 1, characterized in that: In step (4), the salt cores to be coated are evenly hung on a rack, and particles and dust on the surface of the salt cores are cleaned using an electric rotating soft brush and compressed air; the salt cores are immersed in the liquid coating for 5 seconds, then taken out, hung on the rack and left to stand for 5 minutes, and then the industrial ethanol on the salt core products is ignited and burned. After the open flame disappears, the salt cores are transferred to the next process.
6. The process for producing a ceramic salt core coating for high pressure casting according to claim 1, characterized in that: In step (5), the salt core is dried at 200° C. for 60 min.
7. The process for producing a high pressure casting ceramic salt core coating according to claim 1, characterized in that: In step (6), the dried salt core is dried to room temperature and then the coating surface is inspected; the undamaged salt core is placed in a sintering tray for high-temperature sintering, and the high-temperature sintering process is as follows: the temperature is raised from room temperature to 300°C within 60 minutes and kept warm for 30 minutes; the temperature is raised from 300°C to 450°C within 60 minutes and kept warm for 60 minutes; the temperature is raised from 450°C to 550°C within 60 minutes and kept warm for 60 minutes; the temperature is raised from 550°C to 650°C within 60 minutes and kept warm for 60 minutes; the temperature is raised from 650°C to 750°C within 60 minutes and kept warm for 120 minutes; then the temperature is lowered to room temperature with the furnace to complete the firing operation of the product coating.
8. The process for producing a ceramic salt core coating for high pressure casting according to claim 1, characterized in that: In step (6), after sintering, the salt core product is taken out and the surface coating of the salt core is inspected. The salt core product without cracks is a qualified product.