Method for reducing oxygen content in tundish through gas purging

By measuring and calculating the oxygen content in the tundra, selecting inert gas for purging, optimizing the number and diameter of purge pipes, solving the problem of oxygen content control in the tundra, realizing the production demand of clean steel, and improving product quality.

CN119016689AActive Publication Date: 2024-11-26HUNAN VALIN LIANYUAN IRON & STEEL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411116048.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The prior art has problems such as lack of quantification requirements for gas flow, neglected influence on the arrangement of purge pipelines and pipe diameters, and insufficient sealing of the tundra, resulting in difficult to effectively reduce the oxygen content in the tundra, affecting the cleanliness of the molten steel. and product quality.

Method used

By measuring the intermediate volume and initial oxygen content, calculating and setting the target oxygen content, selecting inert gas for purging, optimizing the number and diameter of purge pipes, calculating the optimal gas flow rate and pressure loss, ensuring that the target is achieved within a certain period of time Oxygen content ensures that the oxygen content in the tundra is reduced before pouring the steel.

Benefits of technology

It achieves rapid and effective reduction of oxygen content in the tundra, provides scientific guidance, meets the production needs of clean steel, and improves product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016689A_ABST
    Figure CN119016689A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of steelmaking, and particularly discloses a method for reducing the oxygen content in a tundish through gas purging, which comprises the following steps: S1, before molten steel in a steel ladle is injected into the tundish, obtaining the volume QR of the tundish, and measuring the initial oxygen content C1 of the atmosphere in the tundish; s2, setting a target value C2 of the oxygen content of the atmosphere in the tundish; s3, counting a plurality of pieces of historical data of time required for the process of lifting the tundish roaster to the time before casting, calculating an average value of the plurality of pieces of historical data, and marking the average value as operation time t; s4, purge gas is selected, and the oxygen content C0 in the purge gas is obtained; s5, calculating the purge gas flow Q required for replacing the interior of the tundish; and S6, the number n of the purging pipelines and the pipe diameter d of the purging pipelines are set. The invention provides a method for reducing the oxygen content in a tundish through gas purging, which is used for efficiently and quickly reducing the oxygen content in the tundish and meeting the production requirements of clean steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steelmaking, and in particular relates to a method for reducing oxygen content in a tundish by gas purging. Background Art

[0002] In the modern iron and steel metallurgical process, the molten steel after smelting in the converter or electric furnace is contained in the ladle. After secondary refining, it is hoisted to the continuous casting platform. Then the molten steel in the ladle is injected into the tundish, and the molten steel flows into the crystallizer through the tundish to solidify and form. Before the pouring begins, the tundish is filled with air. When the molten steel in the ladle is injected into the tundish, the molten steel inevitably comes into contact with the air in the tundish, and the molten steel is oxidized. The oxidation products exist in the molten steel in the form of harmful inclusions, which will reduce the cleanliness of the molten steel. In mild cases, the water inlet is blocked, affecting the castability of the molten steel; in severe cases, the large particles that are not removed in the finished product are included in the process of user use and cracking occurs, which endangers the product quality. At the same time, the nitrogen in the air in the tundish will also dissolve into the molten steel, causing the molten steel to increase nitrogen, causing a series of problems such as abnormal composition of the molten steel or abnormal performance. Therefore, the oxygen content in the tundish atmosphere is an important indicator for measuring clean steel production.

[0003] Regarding the control of oxygen content in the tundish atmosphere, some companies use inert gas argon to purge the tundish before pouring. This operation is relatively rough and there are few related studies. The common problems are: 1) There is a lack of quantitative requirements for the purge gas flow rate in production; 2) The influence of the purge pipeline layout and pipe diameter on the purge effect is ignored; 3) The tundish itself is not sealed enough. In view of the above three problems, in the actual production process, after the tundish is purged with gas, the oxygen content in the atmosphere of the tundish is still at a high level, which does not achieve the expected effect. Therefore, it is urgent to use scientific methods to efficiently and quickly achieve a low-oxygen atmosphere in the tundish to meet the needs of clean steel production. Summary of the invention

[0004] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a method for reducing the oxygen content in the tundish by gas purging, which is used to efficiently and quickly reduce the oxygen content in the tundish and meet the needs of clean steel production.

[0005] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0006] A method for reducing oxygen content in a tundish by gas purging, the method comprising the following steps:

[0007] S1: Before the molten steel in the ladle is poured into the tundish, obtain the volume Q of the tundish R , determine the initial oxygen content C1 of the atmosphere in the tundish;

[0008] S2: Setting the target value C2 of the oxygen content of the atmosphere in the tundish;

[0009] S3: Counting multiple historical data of the time required for the process from lifting the tundish baking machine to starting pouring, calculating the average value of the multiple historical data, and marking it as the operation time t;

[0010] S4: Select a purge gas and obtain the oxygen content C0 in the purge gas;

[0011] S5: Calculate the purge gas flow rate Q required to replace the tundish;

[0012] S6: Setting the number n of purge pipes and the pipe diameter d of the purge pipes;

[0013] S7: calculating the purge gas flow rate v and the purge pipeline pressure loss Δp when the oxygen content of the atmosphere in the tundish reaches the target value C2, changing the n value and the d value, and obtaining multiple sets of data on the purge gas flow rate v and the purge pipeline pressure loss Δp;

[0014] S8: According to the data of the multiple groups of purge gas flow rate v and purge pipeline pressure loss Δp calculated in step S7, the n value and d value when the purge gas flow rate v and the purge pipeline pressure loss Δp are both the lowest are selected, that is, the required number of purge pipelines and the diameter of the purge pipelines, which are marked as the optimal number of pipelines and the optimal pipeline diameter respectively;

[0015] S9: according to the analysis result of step S8, when the tundish roaster is lifted, the purge pipe is enabled to fill the tundish with purge gas, the number of the purge pipes is the optimal number of pipes, and the diameter of the purge pipes is the optimal pipe diameter;

[0016] S10: After the time for filling the tundish with the purge gas reaches the operation time t, the gas purge work is completed, and the oxygen content of the atmosphere in the tundish is detected to be no greater than the target value C2 of the oxygen content of the atmosphere in the tundish, and the molten steel is prepared to be poured into the tundish.

[0017] Furthermore, in step S3, the specific process for counting the time required for the process from lifting the tundish baker to starting pouring is: starting the timing from the time the tundish baker completes baking of the tundish and lifting the tundish baker, to the time when the ladle starts pouring molten steel into the tundish, and counting the timing results, which are marked as the time required for the process from lifting the tundish baker to starting pouring.

[0018] Furthermore, the purge gas is an inert gas.

[0019] Furthermore, the purge gas is argon.

[0020] Furthermore, in step S5, the purge gas flow rate required for replacing the tundish is calculated using the following formula:

[0021]

[0022] Where Q is the purge gas flow rate required to replace the tundish, in m 3 / min;

[0023] t is the operation time from the lifting of the tundish baking machine to the start of pouring, in minutes;

[0024] Q R is the volume of the intermediate enclosure, in m 3 ;

[0025] C1 is the initial oxygen content of the atmosphere in the tundish;

[0026] C2 is the target value of oxygen content in the atmosphere of the tundish;

[0027] C0 is the oxygen content in the purge gas.

[0028] Furthermore, the number n of the purge pipes is a positive integer not greater than 10, and is preferably 4.

[0029] Furthermore, the value range of the pipe diameter d of the purge pipe is [0.02, 0.05].

[0030] Further, in step S7, the calculation formula of the purge gas flow rate v is as follows:

[0031]

[0032] Furthermore, in step S7, the calculation formula of the purge pipeline pressure loss Δp is as follows:

[0033]

[0034] Where λ is the drag coefficient;

[0035] l is the length of the purge pipe;

[0036] ρ is the purge gas density, in kg / m 3 ;

[0037] The calculation formula of λ is as follows:

[0038]

[0039] In the calculation formula of λ, Re is the Reynolds number, and the calculation formula of Re is as follows:

[0040]

[0041] In the calculation formula of Re, γ is the gas kinetic viscosity coefficient, the unit is m 2 / s;

[0042] In the above calculation formula, d is the diameter of the purge pipe, in meters;

[0043] v is the purge gas velocity in m / s.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] 1. The present invention provides a method for reducing the oxygen content in the tundish by gas purging, which is used to efficiently and quickly reduce the oxygen content in the tundish to meet the needs of clean steel production.

[0046] 2. The present invention quantitatively gives the purge gas flow rate required to reduce the oxygen content of the atmosphere in the tundish through theoretical calculation, and at the same time clarifies the flow rate of the purge gas and the pressure loss in the pipeline under different numbers of blowing pipelines and blowing pipelines of different diameters, which can provide scientific guidance for on-site production, thereby meeting the needs of clean steel production and improving product quality.

[0047] 3. In the present invention, by setting a plurality of groups of blowing pipes, the number of each group of blowing pipes is different, and the diameter of each group of blowing pipes is also different. The purge gas flow rate and the pressure loss of the purge pipes under different numbers of blowing pipes and different diameters are obtained by calculation. After comparison and analysis of multiple groups of data, the number of purge pipes and the diameter of the purge pipes corresponding to the lowest purge gas flow rate v and the pressure loss Δp of the purge pipes are selected, which are the optimal number of pipes and the optimal diameter of the pipes. Then, the optimal number of pipes and the optimal diameter of the pipes obtained by analysis and calculation are applied to actual production. Under the optimal number of pipes and the optimal diameter of the pipes, the purge gas is filled into the tundish, thereby ensuring that the oxygen content of the atmosphere in the tundish is not greater than the set target value C2 of the oxygen content of the atmosphere in the tundish after the purge time is over, so that subsequent molten steel pouring operations can be carried out. The present invention adopts a scientific calculation method to calculate the optimal pipe data and the optimal pipe diameter, which provides a basis for the configuration of the number of pipes and the configuration of the pipe diameter in actual production.

[0048] 4. The present invention is that before the molten steel in the ladle is injected into the tundish, a purge gas is filled into the tundish, and the air in the tundish is mixed with the purge gas and then discharged, thereby reducing the oxygen content in the tundish to the target value within a certain period of time. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0050] Figure 1 The present invention provides a flow chart of a method for reducing oxygen content in a tundish by gas purging. DETAILED DESCRIPTION

[0051] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0052] like Figure 1 As shown, a method for reducing the oxygen content in a tundish by gas purging comprises the following steps:

[0053] S1: Get the intermediate inclusion product Q R , determine the initial oxygen content C1 of the atmosphere in the tundish

[0054] Before the molten steel in the ladle is poured into the tundish, the volume Q of the tundish is obtained. R , determine the initial oxygen content C1 of the atmosphere in the tundish;

[0055] S2: Setting the target value C2 of the oxygen content of the atmosphere in the tundish;

[0056] S3: Counting multiple historical data of the time required for the process from lifting the tundish baking machine to starting pouring, calculating the average value of the multiple historical data, and marking it as the operation time t;

[0057] In step S3, the specific process of counting the time required for the process from the lifting of the tundish roaster to the start of pouring is as follows: after the tundish roaster has finished baking the tundish, the timing starts when the tundish roaster is lifted, and ends when the ladle starts pouring molten steel into the tundish, and the timing result is counted and marked as the time required for the process from the lifting of the tundish roaster to the start of pouring;

[0058] S4: Select a purge gas and obtain the oxygen content C0 in the purge gas;

[0059] In step S4, the selected purge gas is an inert gas, preferably argon;

[0060] S5: Calculate the purge gas flow rate Q required to replace the tundish;

[0061] In step S5, the purge gas flow rate required for replacing the tundish is calculated using the following formula:

[0062]

[0063] Where Q is the purge gas flow rate required to replace the tundish, in m 3 / min;

[0064] t is the operation time from the lifting of the tundish baking machine to the start of pouring, in minutes;

[0065] Q R is the volume of the intermediate enclosure, in m 3 ;

[0066] C1 is the initial oxygen content of the atmosphere in the tundish;

[0067] C2 is the target value of oxygen content in the atmosphere of the tundish;

[0068] C0 is the oxygen content in the purge gas;

[0069] Among them, the initial oxygen content C1 of the atmosphere in the tundish, the target value C2 of the oxygen content of the atmosphere in the tundish, and the oxygen content C0 in the purge gas are all volume fractions;

[0070] S6: Setting the number n of purge pipes and the pipe diameter d of the purge pipes;

[0071] Wherein, in step S6, the number n of the purge pipes is a positive integer not greater than 10, that is, the number of the set purge pipes is not greater than 10, preferably 4;

[0072] The value range of the diameter d of the purge pipe is [0.02, 0.05], that is, the range of the diameter of the purge pipe is set to 0.02-0.05m;

[0073] S7: calculating the purge gas flow rate v and the purge pipeline pressure loss Δp when the oxygen content of the atmosphere in the tundish reaches the target value C2, changing the n value and the d value, and obtaining multiple sets of data on the purge gas flow rate v and the purge pipeline pressure loss Δp;

[0074] In step S7, the calculation formula of the purge gas flow rate v is as follows:

[0075]

[0076] In step S7, the calculation formula of the purge pipeline pressure loss Δp is as follows:

[0077]

[0078] Among them, in the calculation formula of Δp, λ is the resistance coefficient;

[0079] l is the length of the purge pipe;

[0080] ρ is the purge gas density, in kg / m 3 ;

[0081] The calculation formula of λ is as follows:

[0082]

[0083] In the calculation formula of λ, Re is the Reynolds number, and the calculation formula of Re is as follows:

[0084]

[0085] In the calculation formula of Re, γ is the gas kinetic viscosity coefficient, the unit is m 2 / s;

[0086] In the above calculation formula, d is the diameter of the purge pipe, in meters;

[0087] v is the purge gas flow rate in m / s;

[0088] S8: According to the data of the multiple groups of purge gas flow rate v and purge pipeline pressure loss Δp calculated in step S7, the n value and d value when the purge gas flow rate v and the purge pipeline pressure loss Δp are both the lowest are selected, that is, the required number of purge pipelines and the diameter of the purge pipelines, which are marked as the optimal number of pipelines and the optimal pipeline diameter respectively;

[0089] S9: according to the analysis result of step S8, when the tundish roaster is lifted, the purge pipe is enabled to fill the tundish with purge gas, the number of the purge pipes is the optimal number of pipes, and the diameter of the purge pipes is the optimal pipe diameter;

[0090] S10: After the time for filling the tundish with the purge gas reaches the operation time t, the gas purge work is completed, and the oxygen content of the atmosphere in the tundish is detected to be no greater than the target value C2 of the oxygen content of the atmosphere in the tundish, and the molten steel is prepared to be poured into the tundish.

[0091] The following are specific examples.

[0092] Example

[0093] This embodiment provides a method for reducing the oxygen content in a tundish by gas purging, the method comprising the following steps:

[0094] S1: Before the molten steel in the ladle is poured into the tundish, obtain the volume Q of the tundish R , determine the initial oxygen content C1 of the atmosphere in the tundish;

[0095] Among them, the measured intermediate volume Q R 10m 3 ;

[0096] The initial oxygen content C1 of the atmosphere in the tundish is 21%;

[0097] S2: setting the target value C2 of the oxygen content of the atmosphere in the tundish to 1%;

[0098] S3: Count multiple historical data of the time required for the process from lifting the tundish baking machine to starting pouring, calculate the average value of the multiple historical data, and mark it as operation time t, where the operation time t is 4 minutes;

[0099] In step S3, the specific process of counting the time required for the process from the lifting of the tundish roaster to the start of pouring is as follows: after the tundish roaster has finished baking the tundish, the timing starts when the tundish roaster is lifted, and ends when the ladle starts pouring molten steel into the tundish, and the timing result is counted and marked as the time required for the process from the lifting of the tundish roaster to the start of pouring;

[0100] S4: Select a purge gas and obtain the oxygen content C0 in the purge gas. The selected purge gas is argon gas, and the oxygen content C0 in the purge gas is 0;

[0101] S5: Calculate the purge gas flow rate Q required to replace the tundish;

[0102] In step S5, the purge gas flow rate required for replacing the tundish is calculated using the following formula:

[0103]

[0104] Where Q is the purge gas flow rate required to replace the tundish, in m 3 / min;

[0105] t is the operation time from the lifting of the tundish baking machine to the start of pouring, in minutes;

[0106] Q R is the volume of the intermediate enclosure, in m 3 ;

[0107] C1 is the initial oxygen content of the atmosphere in the tundish;

[0108] C2 is the target value of oxygen content in the atmosphere of the tundish;

[0109] C0 is the oxygen content in the purge gas;

[0110] Substituting the data obtained in steps S1-S4 into this calculation formula, the required purge gas flow rate Q for the replacement tundish is 7.5m 3 / min;

[0111] S6: Setting the number n of purge pipes and the pipe diameter d of the purge pipes;

[0112] Wherein, in step S6, the number n of the purge pipes is a positive integer not greater than 10, that is, the number of the purge pipes set is not greater than 10;

[0113] The value range of the diameter d of the purge pipe is [0.02, 0.05], that is, the range of the diameter of the purge pipe is set to 0.02-0.05m;

[0114] According to the actual production conditions and the layout of the purge pipes, four purge pipes can fully cover the entire tundish cover. Further adding purge pipes will affect the on-site layout, make the construction more difficult, increase the economic cost, and have little effect on improving the actual purge gas effect.

[0115] The diameter d of the purge pipe is set because if the diameter is too small, the pressure loss will be large and the flow rate will be very high. According to the Bernoulli equation, the pressure is low where the velocity is high, which will cause the air near the pipe to be sucked into the tundish, increasing the oxygen atmosphere in the tundish; if the diameter is too large, the gas flow rate will be very small, and it will be difficult to achieve the purpose of purge. Therefore, the diameter range is set to 0.02-0.05m;

[0116] Select n, that is, the number of purge pipes is 2, 3, and 4 respectively; select d, that is, the diameters of the purge pipes are 0.02m, 0.03m, 0.04m, and 0.05m respectively;

[0117] S7: calculating the purge gas flow rate v and the purge pipeline pressure loss Δp when the oxygen content of the atmosphere in the tundish reaches the target value C2, changing the n value and the d value, and obtaining multiple sets of data on the purge gas flow rate v and the purge pipeline pressure loss Δp;

[0118] In step S7, the calculation formula of the purge gas flow rate v is as follows:

[0119]

[0120] In step S7, the calculation formula of the purge pipeline pressure loss Δp is as follows:

[0121]

[0122] Among them, in the calculation formula of Δp, λ is the resistance coefficient;

[0123] l is the length of the purge pipe. According to the site layout, the length of the purge pipe l is 4m;

[0124] ρ is the purge gas density, that is, the density of argon, which is 1.784 kg / m 3 , unit is kg / m 3 ;

[0125] The calculation formula of λ is as follows:

[0126]

[0127] In the calculation formula of λ, Re is the Reynolds number, and the calculation formula of Re is as follows:

[0128]

[0129] In the calculation formula of Re, γ is the gas kinetic viscosity coefficient, the unit is m 2 / s;

[0130] In the above calculation formula, d is the diameter of the purge pipe, in meters;

[0131] v is the purge gas flow rate, in m / s;

[0132] According to the actual production conditions and the layout of the purge pipeline, n is selected, that is, the number of purge pipelines is 2, 3, and 4 respectively; d is selected, that is, the diameters of the purge pipelines are 0.02m, 0.03m, 0.04m, and 0.05m respectively;

[0133] Substitute the values ​​of n and d into the above calculation formula to obtain multiple sets of data on the purge gas flow rate v and the purge pipeline pressure loss Δp. The detailed data are shown in Table 1. The purge gas flow rate Q required to replace the tundish is 7.5m 3 / min, gas flow rate and pressure loss under different numbers of blowing pipes and blowing pipes with different pipe diameters.

[0134] Table 1

[0135]

[0136] S8: According to the data of multiple groups of purge gas flow rate v and purge pipeline pressure loss Δp in Table 1, select the n value and d value when the purge gas flow rate v and the purge pipeline pressure loss Δp are both the lowest, that is, the required number of purge pipelines and the diameter of the purge pipelines, which are marked as the optimal number of pipelines and the optimal pipeline diameter respectively;

[0137] According to the data in Table 1, when the number of blowing pipes is 4 and the pipe diameter is 0.05m, the gas flow rate is 15.9m / s and the pipe pressure loss is 393MPa. That is, under this condition, the gas flow rate and pipe pressure loss are both the lowest, that is, the optimal number of pipes is 4 and the optimal pipe diameter is 0.05m.

[0138] S9: according to the analysis result of step S8, when the tundish roaster is lifted, the purge pipe is enabled to fill the tundish with purge gas, the number of the purge pipes is the optimal number of pipes, and the diameter of the purge pipes is the optimal pipe diameter;

[0139] S10: After the purge gas is filled into the tundish for 4 minutes, the gas purge work is completed, and the oxygen content of the atmosphere in the tundish is detected to be 0.98%, which is less than the target value C2 of the oxygen content in the atmosphere in the tundish, i.e. 1%, and the molten steel can be poured into the tundish.

[0140] The present invention provides a method for reducing the oxygen content in a tundish by gas purging, which is used for efficiently and quickly reducing the oxygen content in the tundish and meeting the needs of clean steel production. Through theoretical calculation, the purge gas flow rate required for reducing the oxygen content of the atmosphere in the tundish is quantitatively given, and at the same time, the flow rate of the purge gas and the pressure loss in the pipeline under different numbers of blowing pipelines and blowing pipelines with different pipe diameters are clarified, which can provide scientific guidance for on-site production, thereby meeting the needs of clean steel production and improving product quality.

[0141] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0142] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A method for reducing oxygen content in a tundish by gas purging, characterized in that: The method comprises the following steps: S1: Before the molten steel in the ladle is poured into the tundish, obtain the volume Q of the tundish R , determine the initial oxygen content C1 of the atmosphere in the tundish; S2: Setting the target value C2 of the oxygen content of the atmosphere in the tundish; S3: Counting multiple historical data of the time required for the process from lifting the tundish baking machine to starting pouring, calculating the average value of the multiple historical data, and marking it as the operation time t; S4: Select a purge gas and obtain the oxygen content C0 in the purge gas; S5: Calculate the purge gas flow rate Q required to replace the tundish; S6: Setting the number n of purge pipes and the pipe diameter d of the purge pipes; S7: calculating the purge gas flow rate v and the purge pipeline pressure loss Δp when the oxygen content of the atmosphere in the tundish reaches the target value C2, changing the n value and the d value, and obtaining multiple sets of data on the purge gas flow rate v and the purge pipeline pressure loss Δp; S8: According to the data of the multiple groups of purge gas flow rate v and purge pipeline pressure loss Δp calculated in step S7, the n value and d value when the purge gas flow rate v and the purge pipeline pressure loss Δp are both the lowest are selected, that is, the required number of purge pipelines and the diameter of the purge pipelines, which are marked as the optimal number of pipelines and the optimal pipeline diameter respectively; S9: according to the analysis result of step S8, when the tundish roaster is lifted, the purge pipe is enabled to fill the tundish with purge gas, the number of the purge pipes is the optimal number of pipes, and the diameter of the purge pipes is the optimal pipe diameter; S10: After the time for filling the tundish with the purge gas reaches the operation time t, the gas purge work is completed, and the oxygen content of the atmosphere in the tundish is detected to be no greater than the target value C2 of the oxygen content of the atmosphere in the tundish, and the molten steel is prepared to be poured into the tundish.

2. A method for reducing oxygen content in a tundish by gas purging according to claim 1, characterized in that: In step S3, the specific process for counting the time required for the process from lifting the tundish roaster to starting pouring is: starting from the time when the tundish roaster is lifted up after the tundish roaster has finished baking the tundish, and ending when the ladle starts pouring molten steel into the tundish, counting the timing results, and marking them as the time required for the process from lifting the tundish roaster to starting pouring.

3. The method of reducing oxygen content in a tundish by gas purging according to claim 1, characterized in that: The purge gas is an inert gas.

4. The method of reducing oxygen content in a tundish by gas purging according to claim 1, characterized in that: The purge gas is argon.

5. The method of reducing oxygen content in a tundish by gas purging according to claim 1, characterized in that: In step S5, the purge gas flow rate required for replacing the tundish is calculated using the following formula: Where Q is the purge gas flow rate required to replace the tundish, in m 3 / min; t is the operation time from the lifting of the tundish baking machine to the start of pouring, in minutes; Q R is the volume of the intermediate enclosure, in m 3 ; C1 is the initial oxygen content of the atmosphere in the tundish; C2 is the target value of oxygen content in the atmosphere of the tundish; C0 is the oxygen content in the purge gas.

6. The method of reducing oxygen content in a tundish by gas purging according to claim 1, characterized in that: The number n of the purge pipes is a positive integer not greater than 10.

7. The method of reducing oxygen content in a tundish by gas purging according to claim 1, characterized in that: The value range of the diameter d of the purge pipe is [0.02, 0.05].

8. The method of reducing oxygen content in a tundish by gas purging according to claim 1, characterized in that: In step S7, the calculation formula of the purge gas flow rate v is as follows:

9. The method of reducing oxygen content in a tundish by gas purging according to claim 1, characterized in that: In step S7, the calculation formula of the purge pipeline pressure loss Δp is as follows: Where λ is the drag coefficient; l is the length of the purge pipe; ρ is the purge gas density, in kg / m 3 ; The calculation formula of λ is as follows: In the calculation formula of λ, Re is the Reynolds number, and the calculation formula of Re is as follows: In the calculation formula of Re, γ is the gas kinetic viscosity coefficient, the unit is m 2 / s; In the above calculation formula, d is the diameter of the purge pipe, in meters; v is the purge gas velocity in m / s.

Citation Information

Patent Citations

  • RH refining method for reducing total oxygen content of ultra-low carbon steel tundish

    CN109880974A

  • Method and apparatus for controlled turbulent purging of open containers

    CN1151440A

  • High-cleanliness steel manufacturing method